Painting method for realizing real wood effect

Through laser engraving and resin material injection molding technology, the real wood texture and color is reproduced on non-wood substrates, and the problems of long production cycle, high cost and inconsistent quality in the existing technology are solved, and efficient and economical real wood effect production is achieved. Meet the market's demand for high-quality decorative materials.

CN118988690APending Publication Date: 2024-11-22SHANGHAI TONGLING AUTOMOTIVE TECH INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411197794.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to quickly and accurately simulate real wood textures and colors on non-wood materials, resulting in long production cycles, high costs and inconsistent quality, and lack of sustainable and cost-effective alternatives.

Method used

Laser engraving is used to form a textured surface with preset wood grain patterns, combined with resin material injection molding, specific pretreatment, primer spraying, color rubbing and transparent protective coating to achieve the visual effect of real wood on non-wood substrates .

Benefits of technology

The real wood effect production process is simplified, production efficiency is improved, costs are reduced, and the durability and aesthetics of the product are ensured, meeting the needs of high-quality real wood effect decorative materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988690A_ABST
    Figure CN118988690A_ABST
Patent Text Reader

Abstract

The invention discloses a painting method for realizing a real wood effect, which comprises the following steps: pretreating a base material to enhance the surface adhesive force of the base material; uniformly spraying a base coat with a first color on the surface of the pretreated base material to form an initial color layer; after the prime coat is dried, a dust-free cloth is used for dipping a color rubbing agent with the color different from that of the prime coat, color rubbing is carried out on the texture surface of the base material, the color rubbing agent permeates and is left in the concave position of the wood grain texture, and the texture surface with the preset wood grain pattern is formed on the mold through laser engraving; resin material injection molding, specific pretreatment, prime coat spraying, color rubbing and application of a transparent protective coating are combined, and the visual effect of real wood can be efficiently reproduced on a non-wood base material. According to the method, the traditional true wood effect manufacturing process is simplified, the production efficiency is improved, the cost is reduced, meanwhile, it is guaranteed that the product has excellent durability and attractiveness, and the requirement of the market for a high-quality true wood effect decorative material is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plate processing, and in particular relates to a painting method for achieving a real wood effect. Background Art

[0002] Traditionally, real wood effects for automotive interiors are usually achieved through veneer decoration, a process that involves using natural wood or veneer and going through multiple complex processing steps to obtain the desired texture, color, and texture. However, this traditional method has several obvious disadvantages, including long production cycles, high costs, and difficulty in achieving consistent quality standards. In addition, due to the limited availability of wood resources and the increase in environmental awareness, it has become an urgent need to find more sustainable and cost-effective alternatives.

[0003] Currently, there is a lack of an efficient process on the market that can quickly and accurately simulate the texture and color of real wood on non-wood materials. Existing methods often cannot balance cost, production speed and the quality of the final product well. Therefore, how to develop a new process that can simplify the production process, reduce production costs, and improve product consistency and durability while ensuring the real wood effect has become an urgent problem to be solved. Summary of the invention

[0004] The object of the present invention is to provide a painting method for achieving a real wood effect, which can efficiently reproduce the visual effect of real wood on a non-wood substrate to solve the problems raised in the above background technology.

[0005] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a painting method for achieving a real wood effect, comprising the following steps: S1: preparing a mold and using laser engraving to form a texture surface with a preset wood grain pattern on it; S2: injecting a resin material into the mold and curing it to form a substrate with a wood grain texture; S3: pre-treating the substrate to enhance its surface adhesion; S4: spraying a first layer of primer on the surface of the pre-treated substrate to form an initial color layer; S5: after the primer is dried, using a dust-free cloth to dip a color rubbing agent of a different color from the primer, rubbing the color on the texture surface of the substrate, so that the color rubbing agent penetrates and remains in the depression of the wood grain texture; S6: cleaning the surface of the substrate, removing excess color rubbing agent, and retaining the color that only exists in the texture depression; S7: inspecting whether the texture and color on the substrate meet the predetermined real wood effect standard; S8: if the inspection is qualified, the substrate is subjected to the last process of spraying a transparent protective coating to enhance its durability and glossiness; S9: curing after the spraying of the transparent protective coating is completed.

[0006] Preferably, after step S1, the method includes: wiping the texture surface with a fiber cloth to remove all residues; evenly applying a layer of sealant on the texture surface after cleaning, completely curing the sealant at room temperature to reinforce the texture structure, and then checking its surface flatness and texture integrity.

[0007] Preferably, after step S2, the method includes: monitoring the temperature and pressure conditions in the mold to ensure that the resin material is cured under the optimal environment to maintain the clarity and details of the wood grain texture; after the curing is completed, safely removing the substrate from the mold to check whether the wood grain texture on its surface is intact and meets the preset visual effect.

[0008] Preferably, after step S3, the method further comprises: sanding the surface of the substrate with sandpaper to remove any minor defects and create roughness to increase the adhesion of subsequent coatings; cleaning the substrate surface after sanding to eliminate dust and debris, and applying a layer of primer to evenly cover the entire substrate surface.

[0009] Preferably, after step S4, the method includes: setting the pressure and nozzle distance of the spray gun, and after the adjustment, steadily moving the spray gun along the texture direction to spray the first layer of primer, and after the first spraying, allowing the primer to dry naturally.

[0010] Preferably, after step S5, the method includes: selecting a color rubbing agent with a clear contrast to the base coating color, dipping the color rubbing agent with a dust-free cloth, and ensuring that the color rubbing agent can fully soak the cloth but not excessively; after preparing the color rubbing agent, applying it on the texture surface of the substrate along the direction of the wood grain, so that the color rubbing agent evenly penetrates into the depressions of the texture; allowing the color rubbing agent to penetrate the texture surface and fix in the depressions, and then wiping with a dust-free cloth to remove excess color rubbing agent.

[0011] Preferably, after step S6, the method includes: wiping the surface of the substrate with a soft cleaning tool to remove the color rubbing agent floating on the surface; after cleaning, performing secondary cleaning with a dry dust-free cloth to ensure that there is no residual color rubbing agent on the surface, but retaining the color of the texture depressions.

[0012] Preferably, after step S7, the method includes: observing the wood grain texture on the surface of the substrate under natural light or lighting conditions simulating natural light, evaluating its clarity and continuity, and ensuring that the grain lines are smooth and without breaks; comparing the color of the substrate with a predetermined real wood effect color sample, checking the color matching, and confirming whether the color saturation and hue are consistent; touching the surface of the substrate to feel the texture and verifying whether it has the natural texture of wood, and checking whether the surface is smooth without obvious graininess or scratchiness.

[0013] Preferably, after step S8, the method includes: preparing a transparent protective coating material while ensuring that the substrate is completely clean, dust-free and dry; spraying the transparent protective coating with a continuous and uniform sweeping motion to cover the entire surface of the substrate; and after spraying, allowing the transparent protective coating to cure naturally to form a protective film.

[0014] Preferably, after step S9, the method includes: moving the substrate on which the transparent protective coating has been sprayed into a set curing chamber to promote the curing of the coating, and monitoring the humidity level in the curing chamber. During the curing process, regularly checking the curing progress of the coating on the surface of the substrate to ensure that the surface is hardened and there are no abnormalities.

[0015] Technical effects and advantages of the present invention: Compared with the prior art, the present invention provides a method for painting a real wood effect, which has the following advantages:

[0016] The present invention forms a texture surface with a preset wood grain pattern by laser engraving on a mold, and combines resin material injection molding, specific pretreatment, primer spraying, rubbing color and transparent protective coating application to efficiently reproduce the visual effect of real wood on a non-wood substrate. This method not only simplifies the traditional real wood effect production process, but also improves production efficiency and reduces costs, while also ensuring that the product has excellent durability and aesthetics, meeting the market demand for high-quality real wood effect decorative materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The present invention is a flow chart of a painting method for achieving a real wood effect. DETAILED DESCRIPTION

[0018] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0019] The present invention provides Figure 1 A painting method for achieving a real wood effect is shown, comprising the following steps:

[0020] S1: preparing a mold and using laser engraving to form a texture surface having a preset wood grain pattern on the mold;

[0021] Further, the following sub-steps are included:

[0022] S1a) gently wiping the textured surface with a fiber cloth to remove all residues and ensure that the engraved details are clearly visible;

[0023] S1b) After cleaning in step S1a), evenly apply a layer of sealant on the texture surface to enhance the three-dimensional texture and prevent moisture penetration in subsequent processes;

[0024] S1c) allowing the sealant to fully cure at room temperature to reinforce the texture structure, and then inspecting its surface flatness and texture integrity;

[0025] S1d) If the texture surface quality is confirmed to meet the standard in step S1c), the subsequent process is continued, otherwise it returns to step S1a) and repeats the entire sub-process until it is satisfactory.

[0026] Sub-steps S1a) to S1d) are an extension of step S1, ensuring that the laser engraved texture surface is in optimal condition before the subsequent processes. Each sub-step is based on the results of the previous step to ensure that the texture surface is both clean and properly protected to maintain the delicate appearance of the wood grain. This meticulous preparation helps to improve the beauty and durability of the final product while reducing potential problems in the production process.

[0027] S2: injecting a resin material into the mold and curing the resin material to form a substrate with a wood grain texture;

[0028] Further, the following sub-steps are included:

[0029] S2a) monitoring the temperature and pressure conditions in the mold to ensure that the resin material is cured under the optimal environment to maintain the clarity and details of the wood grain texture;

[0030] S2b) During the curing process of the resin material, regularly check the tightness of the mold to prevent any external factors from interfering with the curing process and maintain the consistency of the texture;

[0031] S2c) After curing is completed, the substrate is safely removed from the mold and the wood grain texture on its surface is checked to see if it is intact and meets the preset visual effect;

[0032] S2d) If any defects or unclear textures are found on the substrate surface in step S2c), they need to be marked and repaired, and steps S2a) to S2d) are repeated if necessary.

[0033] In this embodiment, sub-steps S2a) to S2d) focus on monitoring and post-curing during the curing process to ensure the perfect presentation of the quality and texture of the substrate. Each sub-step is based on the results of the previous step, and the qualified rate of the finished product is improved by finely managing the curing conditions and subsequent inspections. By implementing these sub-steps, product quality can be effectively controlled, the scrap rate can be reduced, and the efficiency and economy of the entire production process can be improved.

[0034] S3: pretreating the substrate to enhance its surface adhesion;

[0035] Further, the following sub-steps are included:

[0036] S3a) lightly sanding the surface of the substrate using fine sandpaper to remove any minor imperfections and create a slight roughness to enhance the adhesion of subsequent coatings;

[0037] S3b) After grinding in step S3a), thoroughly clean the surface of the substrate to remove all dust and debris to ensure a clean surface to provide optimal adsorption conditions for the coating;

[0038] S3c) Apply a layer of special primer to evenly cover the entire substrate surface. This primer is designed to strengthen the bond between the subsequent coating and the substrate;

[0039] S3d) ensuring that the primer applied in step S3c) is completely dry, and checking whether the substrate surface is smooth and has no exposed areas, so as to ensure the smooth progress of subsequent processes.

[0040] In this embodiment, sub-steps S3a) to S3d) ensure the uniformity of the primer and the preparation of the substrate surface. Each step is to optimize the painting effect and make the final real wood effect more realistic. By carefully adjusting the sanding, cleaning and application of the primer, color unevenness and quality problems can be effectively avoided, and the consistency and appearance of the product can be improved. In addition, careful inspection of the primer after drying and necessary re-coating measures ensure that every inch of the substrate surface can obtain sufficient color coverage, laying a solid foundation for subsequent processes.

[0041] S4: spraying a first color primer uniformly on the surface of the pretreated substrate to form an initial color layer;

[0042] Further, the following sub-steps are included:

[0043] S4a) Set the spray gun pressure and nozzle distance to ensure that the primer is evenly distributed and avoid any over-thickness or over-thinness;

[0044] S4b) After the adjustment in step S4a) is completed, the first layer of primer is sprayed, and the operator needs to move the spray gun steadily along the direction of the texture to enhance the fusion of color and texture;

[0045] S4c) After the first spray, allow the primer to dry naturally, monitoring the ambient temperature and humidity to ensure ideal curing conditions;

[0046] S4d) After the primer in step S4c) is completely dry, check whether there are any missed spraying or uneven spots on the surface. If necessary, perform local re-coating to ensure the integrity of the color layer.

[0047] In this embodiment, sub-steps S4a) to S4d) ensure the uniformity of the primer and the integrity of the color layer. Each step is to optimize the spraying effect and make the final real wood effect more realistic. By carefully adjusting the spray gun parameters and monitoring the drying conditions, color unevenness and quality problems can be effectively avoided, and the consistency and appearance of the product can be improved. In addition, careful inspection of the primer after drying and necessary re-coating measures ensure that every inch of the substrate surface can obtain sufficient color coverage, laying a solid foundation for subsequent processes.

[0048] S5: After the primer is dry, use a dust-free cloth to dip a color rubbing agent of a color different from the primer, and rub the color on the texture surface of the substrate, so that the color rubbing agent penetrates and remains in the concave parts of the wood grain texture;

[0049] Further, the following sub-steps are included:

[0050] S5a) Select a color rubbing agent with a clear contrast to the base coating color, and dip a dust-free cloth into an appropriate amount of the color rubbing agent, ensuring that the color rubbing agent can fully soak the cloth but not too much;

[0051] S5b) After the rubbing agent is prepared in step S5a), the rubbing agent is gently applied on the texture surface of the substrate along the direction of the wood grain, so that the rubbing agent evenly penetrates into the concave parts of the texture to enhance the layering effect;

[0052] S5c) Allow the rubbing agent to remain on the textured surface for a while to allow it to have enough time to penetrate and fix in the recessed areas, then gently wipe with a clean dust-free cloth to remove excess rubbing agent;

[0053] S5d) After step S5c) is completed, check the color rubbing effect on the texture surface to ensure that each depression has appropriate coloring and there is no excessive color rubbing agent remaining to affect the overall appearance.

[0054] In this embodiment, sub-steps S5a) to S5d) ensure the correct application of the coloring agent and the coloring effect of the texture depressions, which enhances the realism of the wood texture. Each step is closely connected, from the selection of the coloring agent to its correct application on the texture surface, to the cleaning of the excess parts, each step is to ultimately achieve a more realistic real wood effect. Through the meticulous treatment of the coloring agent and the careful inspection of the texture surface, it is ensured that the final product visually presents a wood grain effect with a well-defined depth and distinct layers.

[0055] S6: cleaning the surface of the substrate, removing excess color rubbing agent, and retaining the color only in the texture depressions;

[0056] Further, the following sub-steps are included:

[0057] S6a) Use a soft cleaning tool, such as a special sponge or cotton cloth, to gently wipe the surface of the substrate to remove most of the rubbing agent floating on the surface;

[0058] S6b) After cleaning in step S6a), use a dry dust-free cloth to perform secondary cleaning to ensure that there is no residual color rubbing agent on the surface, but the color of the texture depressions is retained;

[0059] S6c) For hard-to-reach texture details, use a small, soft brush to carefully brush away excess color from the surface while avoiding damaging the coloring in recessed areas;

[0060] S6d) After step S6c), the substrate surface is fully inspected again to confirm that all non-texture recessed areas are free of excess color, ensuring that the texture is prominent and the surface is clean.

[0061] In this embodiment, sub-steps S6a) to S6d) focus on removing excess color rubbing agent from the substrate surface, ensuring that only the color of the texture depressions is retained to enhance the three-dimensional and realistic feel of the wood grain. Each step revolves around fine cleaning, from preliminary surface cleaning to special treatment of texture details, and finally a comprehensive inspection to ensure high-quality completion of the entire surface treatment process. Through these meticulous cleaning steps, not only the refinement of the product appearance is improved, but also the smooth progress of subsequent processes is ensured, laying a good foundation for the ultimate realization of high-quality real wood effects.

[0062] S7: Check whether the texture and color of the substrate meet the predetermined real wood effect standard;

[0063] Further, the following sub-steps are included:

[0064] S7a) Observe the wood grain texture on the surface of the substrate under natural light or lighting conditions that simulate natural light, and assess its clarity and continuity, ensuring that the grain lines are smooth and without breaks;

[0065] S7b) comparing the substrate color with a predetermined real wood effect color sample to check the color match and confirm whether the color saturation and hue are consistent;

[0066] S7c) Touch the surface of the substrate to feel the texture and verify whether it has the natural texture of wood. Also check whether the surface is smooth without obvious graininess or scratchiness.

[0067] S7d) Verify whether the overall effect of the substrate is consistent with the expected real wood effect, including a comprehensive evaluation of grain, color and texture to ensure that the product meets high standards of visual and tactile experience.

[0068] In this embodiment, sub-steps S7a) to S7d) focus on comprehensive inspection of the texture and color on the substrate to ensure that it meets the predetermined real wood effect standards. Each step involves strict inspection of different aspects of the product, from visual texture clarity and color matching to tactile texture evaluation, to ensure that the final product meets high quality requirements in all aspects. These inspection steps are key links in the entire process. Through careful evaluation and verification, it is ensured that each product can perfectly simulate the effect of real wood and meet customers' demand for high-quality decorative materials.

[0069] S8: If the inspection is qualified, the substrate will be subjected to the final process of spraying a transparent protective coating to enhance its durability and glossiness;

[0070] Further, the following sub-steps are included:

[0071] S8a) preparing a transparent protective coating material while ensuring that the substrate is completely clean, dust-free and dry;

[0072] S8b) Adjust the spray gun to suit the viscosity of the clear coat to ensure that the coat is evenly distributed without dripping or accumulation;

[0073] S8c) Start spraying the transparent protective coating, using continuous and even sweeping motions to cover the entire substrate surface, paying attention to the edges and corners to ensure the integrity and consistency of the coating;

[0074] S8d) After spraying in step S8c), the substrate is placed under suitable temperature and humidity conditions to allow the transparent protective coating to cure naturally to form a strong protective film, thereby enhancing its durability and glossiness.

[0075] In this embodiment, sub-steps S8a) to S8d) focus on the spraying and curing process of the transparent protective coating to ensure that the coating is uniform and complete to provide the best protection. Each step is to optimize the adhesion and appearance quality of the coating, from material preparation to adjustment of the spray gun, to control of spraying techniques and curing conditions, to ensure that the final product has a smooth surface, long-lasting gloss and excellent durability. By implementing these carefully designed sub-steps, the overall quality of the product can be significantly improved, allowing it to show excellent performance and aesthetics in daily use.

[0076] S9: Curing is performed after the spraying of the transparent protective coating is completed.

[0077] Further, the following sub-steps are included:

[0078] S9a) moving the substrate sprayed with the transparent protective coating into a set curing room, ensuring that the ambient temperature is stable within the recommended range to promote coating curing;

[0079] S9b) In step S9a), the humidity level in the curing chamber is monitored and maintained in an appropriate range to prevent excessively high or low humidity from affecting the curing effect of the coating;

[0080] S9c) During the curing process, regularly check the progress of the coating curing on the substrate surface to ensure that the surface is hardened and free of any abnormalities such as bubbles or cracks;

[0081] S9d) After completing the monitoring of step S9c), once the coating reaches the standard of complete curing, the substrate is carefully moved out of the curing chamber and prepared for the final quality inspection.

[0082] In this embodiment, sub-steps S9a) to S9d) focus on the curing process of the transparent protective coating, ensuring that the curing conditions are appropriate to obtain a hard, flawless surface. Each step is designed to optimize the curing effect, from the control of ambient temperature and humidity to the close monitoring of the curing process to ensure that the coating is completely hardened and provides the best protection for the substrate. By performing these meticulous curing steps, it is possible to ensure that the final product has a long-lasting protective layer while maintaining the gloss and beauty of the surface, meeting the strict standards of high-quality decorative materials.

[0083] In summary, in this example, by using laser engraving on the mold to form a texture surface with a preset wood grain pattern, combined with resin material injection molding, specific pretreatment, primer spraying, rubbing color and transparent protective coating application, the visual effect of real wood can be efficiently reproduced on a non-wood substrate. This method not only simplifies the traditional real wood effect production process, but also improves production efficiency and reduces costs. At the same time, it also ensures that the product has excellent durability and aesthetics, meeting the market demand for high-quality real wood effect decorative materials.

[0084] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A painting method for achieving a real wood effect, characterized in that: The following steps are involved: S1: preparing a mold and using laser engraving to form a texture surface having a preset wood grain pattern on the mold; S2: injecting a resin material into the mold and curing the resin material to form a substrate with a wood grain texture; S3: pretreating the substrate to enhance its surface adhesion; S4: spraying a first color primer uniformly on the surface of the pretreated substrate to form an initial color layer; S5: After the primer is dry, use a dust-free cloth to dip a color rubbing agent of a color different from the primer, and rub the color on the texture surface of the substrate, so that the color rubbing agent penetrates and remains in the concave parts of the wood grain texture; S6: cleaning the surface of the substrate, removing excess color rubbing agent, and retaining the color only in the texture depressions; S7: Check whether the texture and color of the substrate meet the predetermined real wood effect standard; S8: If the inspection is qualified, the substrate will be subjected to the final process of spraying a transparent protective coating to enhance its durability and glossiness; S9: Curing is performed after the spraying of the transparent protective coating is completed.

2. A method for painting a real wood effect according to claim 1, characterized in that: After step S1, the following steps are included: Wipe the textured surface with a microfiber cloth to remove any residue; After cleaning, apply a layer of sealant evenly on the texture surface, completely cure the sealant at room temperature to strengthen the texture structure, and then check its surface flatness and texture integrity.

3. A painting method for achieving a real wood effect according to claim 1, characterized in that: After step S2, the following steps are included: Monitoring the temperature and pressure conditions within the mold to ensure that the resin material is cured under optimal conditions to maintain the clarity and detail of the wood grain texture; After curing is complete, the substrate is safely removed from the mold and checked to see if the wood grain texture on its surface is intact and meets the preset visual effect.

4. A method for painting a real wood effect according to claim 1, characterized in that: After step S3, the following steps are included: Use sandpaper to smooth the surface of the substrate to remove any minor imperfections and create roughness to increase adhesion of subsequent paint; After sanding, clean the substrate surface to eliminate dust and debris and apply a coat of primer evenly covering the entire substrate surface.

5. A painting method for achieving a real wood effect according to claim 1, characterized in that: After step S4, the following steps are included: Set the pressure and nozzle distance of the spray gun. After the adjustments are completed, move the spray gun smoothly along the grain direction to spray the first layer of primer. After the first spray, let the primer dry naturally.

6. A painting method for achieving a real wood effect according to claim 1, characterized in that: After step S5, the following steps are included: Choose a color rubbing agent that has a clear contrast with the base color, and dip the rubbing agent with a dust-free cloth to ensure that the rubbing agent can fully soak the fabric but not too much; After preparing the color rubbing agent, apply it on the texture surface of the substrate along the direction of the wood grain, so that the color rubbing agent can evenly penetrate into the depressions of the texture; Allow the colorant to penetrate the texture surface and fix in the recessed areas, then wipe with a dust-free cloth to remove excess colorant.

7. A painting method for achieving a real wood effect according to claim 1, characterized in that: After step S6, the following steps are included: Use a soft cleaning tool to wipe the surface of the substrate to remove the color rubbing agent floating on the surface; after cleaning, use a dry dust-free cloth for a second clean to ensure that there is no residual color rubbing agent on the surface, but retain the color of the texture depressions.

8. The method for painting to achieve a real wood effect according to claim 1, characterized in that: After step S7, the following steps are included: Observe the wood grain texture on the substrate surface under natural light or lighting conditions that simulate natural light, and evaluate its clarity and continuity to ensure that the grain lines are smooth and without breaks; Compare the substrate colour with the pre-determined real wood effect colour sample to check the colour match and confirm that the colour saturation and tone are consistent; Verify that it has the natural feel of wood by touching the surface of the substrate and feeling the grain. Also check that the surface is smooth without any noticeable graininess or scratchiness.

9. The method for painting to achieve a real wood effect according to claim 1, characterized in that: After step S8, the following steps are included: Prepare the transparent protective coating material while ensuring that the substrate is completely clean, dust-free and dry; spray the transparent protective coating using continuous and even sweeping motions to cover the entire substrate surface; after spraying, allow the transparent protective coating to cure naturally to form a protective film.

10. The method for painting to achieve a real wood effect according to claim 1, characterized in that: After step S9, the following steps are included: Move the substrate that has been sprayed with the transparent protective coating to the set curing chamber to promote the coating curing and monitor the humidity level in the curing chamber. During the curing process, regularly check the coating curing progress on the substrate surface to ensure that the surface is hardened and there are no abnormalities.

Citation Information

Cited By

  • Manufacturing method for instrument panel trim, instrument panel trim, and vehicle

    CN122788186A