Double-process laminated glass and manufacturing method thereof

By using multi-stage rolling and high-pressure treatment of floating white glass substrates, film layers and sunscreen substrates in the manufacturing process of laminated glass, problems such as shrinkage and multi-glue are solved, and the quality and safety of the product are improved , reduces the scrap rate.

CN118991182APending Publication Date: 2024-11-22XINYI GLASS (TIANJIN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411057516.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Laminated glass is prone to problems such as shrinkage and glue during processing, resulting in high scrap rate and inability to perform routine cutting, resulting in waste of resources and product defects.

Method used

Using a dual process laminated glass manufacturing method, including floating white glass substrate, film layer and sun film substrate, the film layer is arranged between the two, and is treated by cleaning, film composite, multi-stage rolling and high pressure to ensure bonding and forming.

Benefits of technology

It effectively avoids problems such as shrinkage and multiple glue, improves the quality and safety of laminated glass, reduces the scrap rate, and improves the structural strength and sound insulation effect of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118991182A_ABST
    Figure CN118991182A_ABST
Patent Text Reader

Abstract

The double-process laminated glass provided by the invention comprises a float white glass substrate, a film layer and a sunlight film substrate, the film layer is arranged between the float white glass substrate and the sunlight film substrate, one side of the film layer is connected with the float white glass substrate, and the other side of the film layer is connected with the sunlight film substrate. The invention further provides a manufacturing method of the double-process laminated glass, the float white glass substrate and the sunlight film substrate are cleaned and then laminated, and rolling and high-pressure pressing are sequentially performed after lamination, so that the problems of inward shrinkage, excessive glue and the like of the double-process laminated glass are avoided, the quality of the double-process laminated glass is improved, the rejection rate of the laminated glass is reduced, and the production cost of the double-process laminated glass is reduced. According to the double-process laminated glass and the manufacturing method thereof provided by the invention, the problems of inward shrinkage, excessive glue and the like of the laminated glass can be avoided, the quality of the laminated glass can be improved, and the rejection rate of the laminated glass can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of double-process laminated glass, and in particular relates to double-process laminated glass and a manufacturing method thereof. Background Art

[0002] Laminated glass is a composite glass product made of two or more pieces of glass with one or more layers of organic polymer interlayer in between. After special processing, the glass and the interlayer are permanently bonded together. Laminated glass is a safety glass. As people pay more and more attention to the safety of buildings and scenic spots, PVB and SGP laminated glass are more and more widely used. However, laminated glass cannot be cut conventionally. Therefore, before processing, laminated glass at home and abroad is generally processed after the size is determined. The transportation of semi-finished glass consumes a lot of manpower and financial resources. If there are defects, the whole product is likely to be scrapped. In addition, the finished laminated glass may shrink or have too much glue.

[0003] In order to solve the above problems, Patent Document 108032595A relates to the technical field of laminated glass, especially ultra-thin laminated glass for automobiles, and specifically provides a method for producing ultra-thin laminated glass and ultra-thin laminated glass. The production method includes the following steps: preparing a first glass substrate and a second glass substrate; heating and bending the first glass substrate to obtain a first curved glass plate; chemically tempering the second glass substrate to obtain a second straight glass plate; and laminating the first curved glass plate, the second straight glass plate and at least one intermediate film to obtain an ultra-thin laminated glass. The present invention does not require the thinner second straight glass plate to be bent and formed, but cannot solve the above problems. Summary of the invention

[0004] The present invention is made to solve the above problems, and aims to provide a double-process laminated glass and a manufacturing method thereof, which can avoid the problems of shrinkage and excessive glue in laminated glass, improve the quality of laminated glass, and reduce the scrap rate of laminated glass. In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0005] The invention provides a double-process laminated glass having the following characteristics: comprising a float glass substrate, a film layer and a sunlight film substrate, wherein the film layer is arranged between the float glass substrate and the sunlight film substrate, one side of the film layer is connected to the float glass substrate, and the other side of the film layer is connected to the sunlight film substrate.

[0006] In the double-process laminated glass provided by the present invention, it can also have the following characteristics: the film layer includes PVB film and SGP film, the PVB film is connected to the float glass substrate, and the SGP film is connected to the sunlight film substrate.

[0007] The double-process laminated glass provided by the present invention may also have the following characteristics: the thickness of the float glass substrate is in the range of 6 mm to 8 mm, and the thickness of the solar film substrate is in the range of 6 mm to 8 mm.

[0008] The double-process laminated glass provided by the present invention may also have the following characteristics: the thickness of the film layer is 1.52 mm, the thickness of the PVB film is 0.76 mm, and the thickness of the SGP film is 0.76 mm.

[0009] The present invention also provides a method for manufacturing double-process laminated glass, which is used to manufacture the above-mentioned double-process laminated glass and has the following characteristics, including the following steps: step S1, cleaning the float glass substrate and the solar film substrate; step S2, combining the sheets; step S3, rolling; step S4, high pressure.

[0010] In the manufacturing method of double-process laminated glass provided by the present invention, it can also have such a feature that in step S2, the temperature range in the laminating operation room is 18°C ​​to 25°C, the humidity range in the laminating operation room is 18% to 28%, and the moisture content of the film layer is in the range of 0.15% to 0.55%.

[0011] In the manufacturing method of double-process laminated glass provided by the present invention, it can also have such a feature that in step S3, the rolling process is divided into multi-stage rolling, and the temperature setting range of the first stage of rolling is 80℃~96℃, the temperature setting range of the second stage of rolling is 165℃~173℃, the temperature setting range of the third stage of rolling is 170℃~173℃, the temperature setting range of the fourth stage of rolling is 165℃~170℃, and the rolling speed range of the roller is 0.6m / min~0.8m / min.

[0012] The method for manufacturing the double-process laminated glass provided by the present invention may also have the following feature: in step S3, the rolling interval is equal to the total thickness of the double-process laminated glass minus 2 mm.

[0013] In the manufacturing method of double-process laminated glass provided by the present invention, it can also have the following characteristics: in step S4, the rolled product is placed in a high-pressure reactor, and the product is pressurized and heated in stages in the high-pressure reactor. The temperature of the first high-pressure stage is 80° C., the pressure of the first high-pressure stage is 0.8 MPa, and the constant temperature time of the first high-pressure stage is 10 min; the temperature of the second high-pressure stage is 110° C., the pressure of the second high-pressure stage is 1.1 MPa, and the constant temperature time of the first high-pressure stage is 25 min; the temperature of the third high-pressure stage is 137° C., the pressure of the first high-pressure stage is 1.2 MPa, and the constant temperature time of the third high-pressure stage is 120 min.

[0014] The method for manufacturing the double-process laminated glass provided by the present invention may also have the following characteristics: the filling time of the high-pressure reactor is 35 seconds per minute, the cooling temperature is 25° C., and the exhaust time is 23 minutes.

[0015] The technical effect of the present invention is as follows: the double-process laminated glass provided by the present invention comprises a float glass substrate, a film layer and a sunlight film substrate, the film layer is arranged between the float glass substrate and the sunlight film substrate, one side of the film layer is connected to the float glass substrate, and the other side of the film layer is connected to the sunlight film substrate. The present invention also provides a method for manufacturing double-process laminated glass, which comprises cleaning the float glass substrate and the sunlight film substrate and then combining them, and then successively subjecting them to rolling and high pressure, thereby avoiding problems such as shrinkage and excess glue in the double-process laminated glass, improving the quality of the double-process laminated glass, and reducing the scrap rate of the laminated glass.

[0016] Therefore, the double-process laminated glass and the manufacturing method thereof provided by the present invention can avoid the problems of shrinkage, excess glue, etc. of the laminated glass, can improve the quality of the laminated glass, and reduce the scrap rate of the laminated glass. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] This specification includes the following drawings, which show the following contents:

[0018] Figure 1 is a schematic structural diagram of a double-process laminated glass in an embodiment of the present invention;

[0019] Figure 2 It is a flow chart of a method for manufacturing double-process laminated glass in an embodiment of the present invention.

[0020] Marked in the figure: 10-float glass substrate, 20-film layer, 21-PVB film, 22-SGP film, 30-sun film substrate. DETAILED DESCRIPTION

[0021] The specific implementation methods of the present invention are further explained in detail below by describing the embodiments with reference to the accompanying drawings, with the aim of helping those skilled in the art to have a more complete, accurate and in-depth understanding of the inventive concept and technical solution of the present invention and facilitating their implementation.

[0022] Figure 1 It is a schematic structural diagram of double-process laminated glass in an embodiment of the present invention.

[0023] like Figure 1As shown, the double-process laminated glass provided by the present invention includes a float glass substrate 10, a film layer 20 and a sunlight film substrate 30. The film layer 20 is arranged between the float glass substrate 10 and the sunlight film substrate 30. One side of the film layer 20 is connected to the float glass substrate 10, and the other side of the film layer 20 is connected to the sunlight film substrate 30. The film layer 20 can be used to bond the float glass substrate 10 and the sunlight film substrate 30. The film layer 20 includes a PVB film 21 and an SGP film 22. The PVB film 21 is connected to the float glass substrate 10, and the SGP film 22 is connected to the sunlight film substrate 30. The PVB film 21 and the SGP film 22 are bonded, thereby bonding the float glass substrate 10 and the sunlight film substrate 30. The PVB film 21 is made of polyvinyl alcohol resin, and has strong energy absorption and light-shielding properties. The SGP film 22 is composed of multiple layers of special polymers, which is more solid and impact-resistant, and can effectively enhance the structural strength of the double-process laminated glass, effectively prevent the double-process laminated glass from being fragmented and splashing when it is broken, thereby improving safety.

[0024] The thickness of the float glass substrate 10 is in the range of 6 mm to 8 mm, and the thickness of the sun film substrate 20 is in the range of 6 mm to 8 mm. In this embodiment, the thickness of the float glass substrate 10 is 7 mm, and the thickness of the sun film substrate 20 is 7 mm. The thickness of the film layer 20 is 1.52 mm, the thickness of the PVB film 21 is 0.76 mm, and the thickness of the SGP film 22 is 0.76 mm, which further enhances the structural strength of the double-process laminated glass.

[0025] Figure 2 It is a flow chart of a method for manufacturing double-process laminated glass in an embodiment of the present invention.

[0026] like Figure 2 As shown, the present invention also provides a method for manufacturing double-process laminated glass, comprising the following steps:

[0027] Step S1, cleaning the float glass substrate 10 and the solar film substrate 30, avoiding the presence of impurities and other pollutants on the float glass substrate 10 and the solar film substrate 30, ensuring the cleanliness of the float glass substrate 10 and the solar film substrate 30, which is beneficial to improving the bonding effect and product quality.

[0028] Step S2, laminating, in the laminating operation room, sequentially stack the float glass substrate 10, PVB film 21, SGP film 22 and sunlight film substrate 30, and perform high-precision lamination on the float glass substrate 10, PVB film 21, SGP film 22 and sunlight film substrate 30 to avoid deviation.

[0029] Step S3, rolling, the double-process laminated glass is rolled by two rollers, one of which is located below the float glass substrate 10, and the other is located above the solar film substrate 30, and the two rollers roll on both sides of the double-process laminated glass to complete the rolling of the double-process laminated glass.

[0030] Step S4, high pressure, placing the rolled double-process laminated glass in a high pressure reactor for high pressure.

[0031] In step S2, the temperature range of the laminating operation room is 18°C ​​to 25°C, the humidity range of the laminating operation room is 18% to 28%, and the moisture content of the film layer is 0.15% to 0.55%.

[0032] In step S3, the rolling process is divided into multi-stage rolling, and the temperature setting range of the first stage of rolling is 80℃~96℃, the temperature setting range of the second stage of rolling is 165℃~173℃, the temperature setting range of the third stage of rolling is 170℃~173℃, the temperature setting range of the fourth stage of rolling is 165℃~170℃, and the rolling speed range of the roller is 0.6m / min~0.8m / min, so that the rolling process can have a smooth transition, effectively avoiding the problems of shrinkage, excess glue, etc. of double-process laminated glass, improving the quality of double-process laminated glass, and reducing the scrap rate of laminated glass.

[0033] In step S3, the rolling spacing is equal to the total thickness of the double-process laminated glass minus 2 mm, and the rolling spacing is the distance between two rollers, so as to ensure the reliability of the rolling process and avoid damaging the double-process laminated glass.

[0034] In step S4, the rolled product is placed in a high-pressure reactor, and the product is pressurized and heated in stages in the high-pressure reactor. The temperature of the first stage of high pressure is 80 degrees Celsius, the pressure of the first stage of high pressure is 0.8Mpa, and the constant temperature time of the first stage of high pressure is 10 minutes; the temperature of the second stage of high pressure is 110 degrees Celsius, the pressure of the second stage of high pressure is 1.1Mpa, and the constant temperature time of the first stage of high pressure is 25 minutes; the temperature of the third stage of high pressure is 137 degrees Celsius, the pressure of the first stage of high pressure is 1.2Mpa, and the constant temperature time of the third stage of high pressure is 120 minutes. The filling time of the high-pressure reactor is 35 seconds, the cooling temperature is 25 degrees, and the exhaust time is 23 minutes. After each stage, cooling and exhaust are required before proceeding to the next stage, so that the high-pressure process of the double-process laminated glass is smoother, effectively avoiding the problems of shrinkage and excessive glue in the double-process laminated glass, improving the quality of the double-process laminated glass, and reducing the scrap rate of the laminated glass. The double-process laminated glass produced by the method for producing the double-process laminated glass provided by the present invention is tested and found to have high quality, high safety, and good sound insulation and heat insulation effects.

[0035] Functions and Effects of the Embodiments

[0036] The double-process laminated glass provided by the present invention includes a float glass substrate 10, a film layer 20 and a sunlight film substrate 30. The film layer 20 is arranged between the float glass substrate 10 and the sunlight film substrate 30. One side of the film layer 20 is connected to the float glass substrate 10, and the other side of the film layer 20 is connected to the sunlight film substrate 30. The film layer 20 can be used to bond the float glass substrate 10 and the sunlight film substrate 30. The film layer 20 includes a PVB film 21 and an SGP film 22. The PVB film 21 is connected to the float glass substrate 10, and the SGP film 22 is connected to the sunlight film substrate 30. The PVB film 21 and the SGP film 22 are bonded, thereby bonding the float glass substrate 10 and the sunlight film substrate 30. The PVB film 21 is made of polyvinyl alcohol resin, which has strong energy absorption and light shielding properties. The SGP film 22 is composed of multiple layers of special polymers, which is more solid and impact-resistant, and can effectively enhance the structural strength of the double-process laminated glass, effectively prevent the fragments of the double-process laminated glass from splashing when it is broken, and improve safety. The rolled product is placed in a high-pressure reactor, and the product is pressurized and heated in stages in the high-pressure reactor. The temperature of the first stage of high pressure is 80 degrees Celsius, the pressure of the first stage of high pressure is 0.8Mpa, and the constant temperature time of the first stage of high pressure is 10 minutes; the temperature of the second stage of high pressure is 110 degrees Celsius, the pressure of the second stage of high pressure is 1.1Mpa, and the constant temperature time of the first stage of high pressure is 25 minutes; the temperature of the third stage of high pressure is 137 degrees Celsius, the pressure of the first stage of high pressure is 1.2Mpa, and the constant temperature time of the third stage of high pressure is 120 minutes. The filling time of the high-pressure reactor is 35smin, the cooling temperature is 25℃, and the exhaust time is 23min. After each stage, cooling and exhaust are required before proceeding to the next stage, which makes the high-pressure process of the double-process glass smoother, effectively avoiding the problems of shrinkage and excessive glue in the double-process laminated glass, improving the quality of the double-process laminated glass and reducing the scrap rate of laminated glass.

[0037] Therefore, the double-process laminated glass and the manufacturing method thereof provided by the present invention can avoid the problems of shrinkage, excess glue, etc. of the laminated glass, can improve the quality of the laminated glass, and reduce the scrap rate of the laminated glass.

[0038] The present invention is described above by way of example in conjunction with the accompanying drawings. Obviously, the specific implementation of the present invention is not limited to the above-mentioned methods. As long as various non-substantial improvements are made using the method concept and technical solution of the present invention; or the above concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A double-process laminated glass, characterized in that: The invention comprises a float glass substrate (10), a film layer (20) and a sunlight film substrate (30), wherein the film layer (20) is arranged between the float glass substrate (10) and the sunlight film substrate (30), one side of the film layer (20) is connected to the float glass substrate (10), and the other side of the film layer (20) is connected to the sunlight film substrate (30).

2. The double-process laminated glass according to claim 1, characterized in that: The film layer (20) comprises a PVB film (21) and an SGP film (22); the PVB film (21) is connected to the white float glass substrate (10), and the SGP film (22) is connected to the sunlight film substrate (30).

3. The double-process laminated glass according to claim 2, characterized in that: The thickness of the float glass substrate (10) is in the range of 6 mm to 8 mm, and the thickness of the sunlight film substrate (30) is in the range of 6 mm to 8 mm.

4. The double-process laminated glass according to claim 3, characterized in that: The thickness of the film layer (20) is 1.52 mm, the thickness of the PVB film (21) is 0.76 mm, and the thickness of the SGP film (22) is 0.76 mm.

5. A method for manufacturing double-process laminated glass, used for manufacturing the double-process laminated glass according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step S1, cleaning the float glass substrate and the solar film substrate; Step S2, sheet assembly; Step S3, rolling; Step S4, high pressure.

6. The method for manufacturing double-process laminated glass according to claim 5, characterized in that: In step S2, the temperature range of the laminating operation room is 18°C ​​to 25°C, the humidity range of the laminating operation room is 18% to 28%, and the moisture content of the film layer is 0.15% to 0.55%.

7. The method for manufacturing double-process laminated glass according to claim 6, characterized in that: In step S3, the rolling process is divided into multi-stage rolling, and the temperature setting range of the first stage of rolling is 80℃~96℃, the temperature setting range of the second stage of rolling is 165℃~173℃, the temperature setting range of the third stage of rolling is 170℃~173℃, the temperature setting range of the fourth stage of rolling is 165℃~170℃, and the roller rolling speed range is 0.6m / min~0.8m / min.

8. The method for manufacturing double-process laminated glass according to claim 7, characterized in that: In step S3, the rolling distance is equal to the total thickness of the double-process laminated glass minus 2 mm.

9. The method for manufacturing double-process laminated glass according to claim 8, characterized in that: In step S4, the rolled product is placed in a high-pressure reactor, and the product is pressurized and heated in stages in the high-pressure reactor. The temperature of the first high-pressure stage is 80° C., the pressure of the first high-pressure stage is 0.8 MPa, and the constant temperature time of the first high-pressure stage is 10 min; the temperature of the second high-pressure stage is 110° C., the pressure of the second high-pressure stage is 1.1 MPa, and the constant temperature time of the first high-pressure stage is 25 min; the temperature of the third high-pressure stage is 137° C., the pressure of the first high-pressure stage is 1.2 MPa, and the constant temperature time of the third high-pressure stage is 120 min.