Method for synthesizing hydroxylamine through ketoxime-mediated conductive catalysis

Through the ketoxime-mediated electrocatalytic method, metal oxide catalysts and electrode composite materials are used to solve the problem of low yield of electrocatalytic synthesis of nitrogen-containing chemicals and environmental pollution of traditional hydroxylamine synthesis methods, achieving efficient and stable hydroxylamine formation and green chemical synthesis.

CN118992980APending Publication Date: 2024-11-22INST OF CHEM CHINESE ACAD OF SCI

Patent Information

Application Number
CN202310576983.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The current electrocatalytic synthesis of high-value nitrogen-containing chemicals has low yields, low energy utilization and limited reaction types. The traditional hydroxylamine synthesis method has complex reaction steps, harsh conditions, many by-products, and serious environmental pollution, making it difficult to achieve greenness. Sustainable carbon neutrality.

Method used

Using a ketoxime-mediated electrocatalytic method, metal oxide catalysts are prepared by metal oxide catalysts and electrode composite materials by sonication and calcination, and electrolytic reactions are carried out in combination with a flow-type electrolytic cell and a keto compound solution to produce ketones that are easy to acid-dissolve. Oxime intermediate, and finally hydroxylamine is produced.

Benefits of technology

It achieves efficient and stable production of hydroxylamine, with mild reaction conditions, few by-products and easy separation of products, providing a clean and efficient new way of green chemical synthesis, with industrial value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004240275130000011
    Figure HDA0004240275130000011
  • Figure HDA0004240275130000012
    Figure HDA0004240275130000012
  • Figure HDA0004240275130000021
    Figure HDA0004240275130000021
Patent Text Reader

Abstract

The invention discloses a method for synthesizing hydroxylamine through ketoxime dielectric conductive catalysis. According to the invention, a metal oxide catalyst is prepared, and the metal oxide catalyst and a gas diffusion layer form an electrode composite material; an electrocatalytic synthesis system composed of the electrode composite material, an electrolyte solution and an electrolytic tank device is used for electrocatalytic synthesis of hydroxylamine. The method for synthesizing hydroxylamine through dielectric conductive catalysis of ketoxime comprises the following steps: 1) adopting an electro-catalytic synthesis system, taking alkaline earth metal salt of nitric acid or nitrous acid as a raw material, and carrying out electrolytic reaction in an electrolytic tank device under the action of an electrode composite material and an electrolyte solution to obtain a system containing a cyclopentanone oxime intermediate; and 2) carrying out acidolysis on the system containing the cyclopentanone oxime intermediate by adopting an inorganic acid aqueous solution to obtain hydroxylamine. The hydroxylamine synthesis route provided by the invention has the advantages of cheap and easily available raw materials, mild reaction conditions, simple reaction, easy operation, few reaction byproducts and easy product separation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemistry and chemical engineering, in particular to the field of electrochemical synthesis technology, and relates to a method for synthesizing hydroxylamine through ketoxime-mediated electrocatalysis. Background Art

[0002] At present, adopting the concept of green chemistry and using renewable energy to drive chemical reactions is crucial to reducing the chemical industry's dependence on fossil resources, reducing carbon dioxide emissions and achieving the "dual carbon" goal. In recent years, researchers have developed a variety of chemical reaction intensification strategies based on renewable energy, such as electrocatalysis, (laser) photocatalysis, Joule heat catalysis and plasma catalysis. Among them, electrocatalytic synthesis has the advantages of simple equipment, controllable path, low cost and mild conditions, which has attracted widespread attention from academia and industry at home and abroad.

[0003] Nitrogen is an important component of life in nature and the modern chemical industry. The green and sustainable synthesis of nitrogen-containing chemicals is one of the important topics of concern to scientists. In the past few decades, the synthesis of NH3 from N2 based on the Haber-Bosch method has been developed and promoted, and a series of technologies based on NH3 to synthesize nitrogen-containing chemicals such as hydroxylamine (salts), amines, nitriles and oximes have also been spawned. However, the Haber-Bosch method for synthesizing ammonia consumes a lot of energy, which is contrary to the "dual carbon" goal and the idea of ​​sustainable development. Recently, researchers have developed a series of methods based on renewable resources (such as N2 and NO x etc.) technology for electrocatalytic synthesis of nitrogen-containing chemicals, such as electrocatalytic N2 / NO x Reduction to ammonia, electrocatalytic N2 oxidation to nitric acid (salt), electrocatalytic CN coupling to urea and amines, etc. However, the current electrocatalytic synthesis of high-value-added nitrogen-containing chemicals still faces challenges such as low yield, severe hydrogen evolution and low energy utilization. In addition, the reaction types for the electrocatalytic synthesis of nitrogen-containing chemicals are currently very limited, and there are still many nitrogen-containing chemicals that cannot be synthesized via electrochemical routes. Exploring new pathways for the electrocatalytic synthesis of nitrogen-containing chemicals is of great significance for utilizing clean energy, decoupling the chemical industry from fossil energy, and achieving the "dual carbon" goals and sustainable development.

[0004] Hydroxylamine, also known as hydroxylamine, has a molecular formula of NH2OH and is an important chemical raw material. It has important applications in agriculture, medicine, chemical analysis and electrochemical analysis. In recent years, it has also shown potential in synthesizing functional materials, providing aviation fuel, processing nuclear fuel and separating rare earth metals. Due to the extreme instability of the monomer, hydroxylamine is often produced, transported and used in the form of proton salts (such as hydrochlorides, sulfates, nitrates and phosphates). Traditional methods for synthesizing hydroxylamine (salts) include the Rashing synthesis method based on NH3 oxidation, the hydrogen peroxide oxidation NH3 route with TS-1 molecular sieve as a catalyst, and the nitroalkane hydrolysis method. The traditional route for the synthesis of hydroxylamine (salts) has problems such as complex reaction steps, harsh reaction conditions, more by-products and serious environmental pollution. The development of new routes for the synthesis of hydroxylamine (salts) based on renewable resources and driven by clean energy, such as electrocatalytic hydroxylamine synthesis, is crucial to providing environmentally friendly carbon-neutral hydroxylamine raw materials for the chemical industry, which is a catalyst for N2 and NO x It provides new ideas for the clean and efficient utilization of nitrogen resources. Summary of the invention

[0005] The purpose of the present invention is to provide a method for synthesizing hydroxylamine by ketoxime-mediated electrocatalysis.

[0006] The first object of the present invention is to provide a method for preparing a metal oxide catalyst.

[0007] The preparation method of the metal oxide catalyst provided by the present invention comprises the following steps: (1) mixing a solution of a metal compound with a solution of an organic ligand, ultrasonically treating and aging the mixture to obtain a system containing a product;

[0008] (2) centrifuging, washing and vacuum drying the system containing the product to obtain a metal organic framework precursor;

[0009] (3) calcining the metal organic framework precursor to obtain a metal oxide catalyst composed of metal elements, carbon elements and oxygen elements.

[0010] In the above method, the metal element in the metal compound is selected from transition metals and / or rare earth metals; specifically, at least one selected from iron, cobalt, nickel, copper, zinc, lanthanum, cerium and praseodymium;

[0011] The metal compound is at least one of sulfate, nitrate, hydrochloride, acetate, acetic acid pyruvate and hydrates thereof of the metal element;

[0012] The organic ligand is a compound containing a carboxyl functional group, specifically at least one selected from phthalic acid, isophthalic acid, 2,5-dihydroxyterephthalic acid, 1,3,5-benzenetricarboxylic acid, benzene-1,2,4,5-tetracarboxylic acid and 1,3,5-tris(4-carboxyphenyl)benzene.

[0013] In the above method, the concentration of the metal compound solution can be 0.01 to 0.5 mol·L -1 , specifically 0.15 mol·L -1 , 0.01~0.15mol·L -1 , 0.15~0.5mol·L -1 or 0.1~0.40mol·L -1 ;

[0014] The solution concentration of the organic ligand may be 0.001 to 0.05 mol·L -1 , specifically 0.015 mol·L -1 , 0.015~0.05mol·L -1 , 0.001~0.015mol·L -1 or 0.01~0.03mol·L -1 .

[0015] In the above method, the solvent used in the solution of the metal compound and the solution of the organic ligand is an organic solvent, and the organic solvent can be selected from at least one of methanol, ethanol and N,N-dimethylformamide, and can be specifically methanol.

[0016] In the above method, the ultrasonic treatment time may be 10 to 100 min, specifically 30 min, 10 to 30 min, 30 to 100 min or 20 to 70 min.

[0017] In the above method, the aging time may be 1 to 24 hours, specifically 12 hours, 1 to 12 hours, 12 to 24 hours or 5 to 20 hours;

[0018] The centrifugal speed may be 800-12000 rpm, specifically 5000 rpm, 800-12000 rpm, 800-12000 rpm or 800-12000 rpm, and the time may be 3-30 min, specifically 5 min;

[0019] The washing solvent is selected from at least one of water, methanol and ethanol;

[0020] The vacuum drying temperature may be 30-120°C, specifically 60°C, 30-60°C, 60-120°C or 50-100°C, and the drying time may be 1-48h, specifically 12h, 1-12h, 12-48h or 10-25h.

[0021] In the above method, the calcination atmosphere is selected from nitrogen, argon or air, the calcination temperature can be 200-1000°C, specifically 600°C, 200-600°C, 600-1000°C or 400-800°C, and the calcination time can be 1-10h, specifically 3h, 1-3h, 3-10h or 2-8h.

[0022] The second object of the present invention is to provide a metal oxide catalyst prepared by the above method.

[0023] The third object of the present invention is to provide an electrode composite material.

[0024] The electrode composite material provided by the present invention is composed of the above-mentioned metal oxide catalyst and a gas diffusion layer;

[0025] The metal oxide catalyst is coated on the gas diffusion layer;

[0026] The gas diffusion layer is carbon fiber paper, carbon fiber woven cloth, carbon black paper and polytetrafluoroethylene membrane.

[0027] In the above electrode composite material, the coating amount of the metal oxide catalyst on the gas diffusion layer can be 0.1 to 100 mg·cm -2 , specifically 1 mg cm -2 , 0.1~1mg·cm -2 , 1~100mg·cm -2 or 0.5~50mg·cm -2 .

[0028] The fourth object of the present invention is to provide a method for preparing the above-mentioned electrode composite material.

[0029] The method for preparing the electrode composite material provided by the present invention comprises the following steps: dispersing the metal oxide catalyst into an organic solvent by ultrasonic treatment to obtain a dispersion; coating the dispersion onto the gas diffusion layer to obtain the electrode composite material;

[0030] In the above method, the organic solvent is at least one of methanol, ethanol, n-propanol, isopropanol and acetone.

[0031] In the above method, the concentration of the dispersion is 0.1 to 20 mg·mL -1 .

[0032] A fifth object of the present invention is to provide an electrocatalytic synthesis system.

[0033] The electrocatalytic synthesis system provided by the present invention comprises the above-mentioned electrode composite material, electrolyte solution and electrolytic cell device.

[0034] In the above-mentioned electrocatalytic synthesis system, the electrolyte solution includes an aqueous solution of a metal salt electrolyte and a ketone compound;

[0035] The metal salt electrolyte is selected from at least one of potassium nitrate, sodium nitrate, potassium nitrite and sodium nitrite;

[0036] The ketone compound is selected from at least one of methyl ethyl ketone, diethyl ketone, cyclopentanone and cyclohexanone, preferably cyclopentanone;

[0037] The concentration of the metal salt electrolyte in the electrolyte solution may be 0.1 mol·L -1 To saturation concentration, specifically 1 mol·L -1 The concentration of the ketone compound may be 0.01 to 0.2 mol·L -1 , specifically 0.1 mol·L -1 ;

[0038] The electrolytic cell device is an H-type electrolytic cell or a flow-type electrolytic cell, preferably a flow-type electrolytic cell.

[0039] A sixth object of the present invention is to provide application of the electrode composite material and / or the electrocatalytic synthesis system in electrocatalytic synthesis of hydroxylamine.

[0040] The seventh object of the present invention is to provide a method for synthesizing hydroxylamine by ketoxime-mediated electrocatalysis.

[0041] The method for electrocatalytic synthesis of hydroxylamine provided by the present invention comprises the following steps: 1) using the above-mentioned electrocatalytic synthesis system, taking an alkaline earth metal salt of nitric acid or nitrous acid as a raw material, and performing an electrolytic reaction in the electrolytic cell device through the action of the electrode composite material and the electrolyte solution to obtain a system containing a cyclopentanone oxime intermediate;

[0042] 2) The system containing the cyclopentanone oxime intermediate is subjected to acid hydrolysis with an inorganic acid aqueous solution to obtain hydroxylamine.

[0043] In the above method, the potential of the electrolysis reaction may be -0.8 to -2.2 V vs. Ag / AgCl, and the electrolysis time may be 0.1 to 3 h;

[0044] The inorganic acid in the inorganic acid aqueous solution is selected from at least one of hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid;

[0045] The concentration of the inorganic acid aqueous solution can be 0.1 to 2 mol·L -1 ;

[0046] The molar ratio of the cyclopentanone oxime to the inorganic acid is 1:1 to 10;

[0047] The reaction time of the acid hydrolysis may be 0.5 to 24 hours.

[0048] The present invention has the following beneficial effects:

[0049] 1. The electrocatalyst provided by the present invention has the characteristics of simple preparation, controllable cost and good stability, and can efficiently and stably generate ketoxime intermediates that are easy to acid-lyze for hydroxylamine synthesis.

[0050] 2. The hydroxylamine synthesis pathway provided by the present invention has the advantages of cheap and readily available raw materials, mild reaction conditions, simple and easy reaction operation, few reaction by-products, and easy product separation; in addition, it provides a new clean and efficient green chemical synthesis pathway for hydroxylamine products that are important and widely used in industry, and has potential industrial value. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 Cu x C y O z Scanning electron microscope image @600;

[0052] Figure 2 Cu x C y O z Powder X-ray diffraction pattern of @600;

[0053] Figure 3 Cu x C y O z @600 element distribution image;

[0054] Figure 4 This is the electron ionization mass spectrum of cyclopentanone oxime (the molecular ion peak is marked);

[0055] Figure 5 Cu x C y O z Faradaic efficiency and yield plot for electrocatalytic cyclopentanone oxime synthesis at @600;

[0056] Figure 6 For different Cu x C y O z @T catalyst catalyzed cyclopentanone oxime synthesis yield diagram;

[0057] Figure 7 This is the yield diagram of hydroxylamine prepared by acidolysis of cyclopentanone oxime.

[0058] Figure 8 For the cycle Cu x C y Oz Faradaic efficiency and yield plot for the synthesis of cyclopentanone oxime catalyzed by @600. DETAILED DESCRIPTION

[0059] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0060] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0061] Example 1 Preparation and characterization of catalyst:

[0062] The Cu obtained by pyrolysis of the precursor at 600 °C x C y O z @T catalyst (T can be 400, 600, 800, 1000) as an example. First, 500mL of 0.15mol·L -1 Cu(NO3)2 methanol solution and 500mL of 0.015mol·L -1 The suspension was aged at room temperature for 12 h. The suspension was centrifuged at 5000 rpm for 5 min, and the solid powder was dried at 60 °C under vacuum for 12 h. The catalyst precursor was pyrolyzed at 400, 600, 800, and 1000 °C in air for 3 h to obtain Cu x C y O z @T Catalyst.

[0063] Cu x C y O z The structure and performance of @600 catalyst were systematically studied. Figure 1 As shown, scanning electron microscopy images show that Cu x C y O z @600 catalyst presents a uniform granular structure. Figure 2 The powder X-ray diffraction pattern of Cu x C y O z The Cu element in @600 catalyst mainly exists in the form of CuO, with an oxidation state of +2. Figure 3 As shown in the element distribution image, the three elements Cu, C and O are evenly distributed in Cu x C y O z @600 catalyst surface.

[0064] Example 2 Electrocatalytic Synthesis of Cyclopentanone Oxime Intermediate

[0065] 20 mg of Cu prepared in Example 1 of the present invention was added x C y O z The @600 catalyst was dispersed in 2 mL of isopropanol and ultrasonicated for 30 min to obtain a uniform dispersion. -2 The loading amount was coated on the polytetrafluoroethylene membrane gas diffusion layer and allowed to stand at room temperature (25°C) for 1 hour to obtain a working electrode.

[0066] All electrochemical experiments in the present invention were conducted at room temperature and pressure (25°C, 1 atmosphere) using a CHI 660 workstation produced by Shanghai Chenhua Instrument Co., Ltd. The flow-type electrolytic cell used adopted a three-electrode system, including the above-mentioned working electrode, a nickel foam counter electrode and a built-in 3 mol·L -1 The Ag / AgCl reference electrode was a KCl aqueous solution (calibrated before the experiment). Fumasep FAA-3-PK-130 membrane was used as an anion exchange membrane to separate the positive and negative electrodes. The positive electrode used a 1M NaOH aqueous solution as the anode liquid, and the negative electrode used a 0.1 mol·L -1 cyclopentanone and 1 mol·L -1 The aqueous solution of NaNO3 was used as the cathode liquid. Each electrolysis used 10 mL of cathode and cathode solution, and the liquid flow rate was 10 mL min -1 .

[0067] Under constant voltage conditions of -0.8, -1.0, -1.2, -1.4, -1.6, and -1.8, the gas product cyclopentanone oxime was electrolyzed.

[0068] The structure was confirmed as follows:

[0069] The gaseous products were analyzed by gas chromatography (GC, HP 4890D), and the small organic molecules in the liquid products were analyzed by gas chromatography (GC, Agilent 6820) after extraction with ethyl acetate.

[0070] The electrocatalytic process generated cyclopentanone oxime product ( Figure 4 The electron ionization mass spectrum measured by gas chromatography-mass spectrometry (GC-MS, Agilent 5977A) is shown in Figure 4 As shown, the molecular ion peak has a charge-to-mass ratio of 99.0.

[0071] The Faradaic efficiency and yield of cyclopentanone oxime at different voltages are shown in Figure 2. Figure 5 As shown. Figure 5It can be seen that under the catalytic system described in the present invention, at -1.8 V vs. Ag / AgCl, the Faradaic efficiency of cyclopentanone oxime can reach 47.8%, and the yield can reach 34.9 mg h -1 cm -2 .

[0072] The cyclopentanone oxime intermediate was prepared by the same raw materials, methods and steps as in the above experiment, except that the Cu x C y O z @600 catalyst, respectively using the Cu prepared in Example 1 of the present invention x C y O z @400, Cu x C y O z @800, Cu x C y O z @1000 catalyst was used for the experiment. x C y O z @T catalyst catalytic performance of cyclopentanone oxime synthesis Figure 6 As shown by Figure 6 It can be seen that Cu x C y O z The @600 catalyst has the highest synthesis rate, so Cu x C y O z @600 catalyst for electrocatalytic synthesis of cyclopentanone oxime intermediates.

[0073] Example 3 Preparation of Hydroxylamine by Acid Hydrolysis of Cyclopentanone Oxime

[0074] The electrolyte product obtained in Example 2 of the present invention was mixed with sulfuric acid aqueous solutions of different concentrations and allowed to stand for 12 hours. The hydroxylamine content in the sample was determined by a colorimetric method using an ultraviolet-visible spectrophotometer (Lambda 1050+). Figure 7 As shown in the figure, with the increase of the concentration of aqueous sulfuric acid solution, the conversion rate of cyclopentanone oxime decomposition increases continuously. In the process of increasing the molar ratio of cyclopentanone oxime to sulfuric acid from 1:1 to 1:4, the selectivity of cyclopentanone oxime decomposition to hydroxylamine stabilizes at about 95%, and therefore, the concentration of the generated hydroxylamine product gradually increases. When the molar ratio of cyclopentanone oxime to sulfuric acid reaches 1:5, the selectivity of cyclopentanone oxime decomposition to hydroxylamine decreases, causing the concentration of hydroxylamine in the resulting final solution to decrease. In summary, when the molar ratio of cyclopentanone oxime to sulfuric acid is 1:4, even if 0.4 mol·L -1When the sulfuric acid aqueous solution was acid hydrolyzed, the hydroxylamine concentration in the solution was the highest, which was 96.1 mol·L -1 .

[0075] Example 4 Electrocatalyst Stability Study

[0076] According to the method in Example 2 of the present invention, at -1.8V vs.Ag / AgCl, the Cu prepared in Example 1 of the present invention x C y O z The @600 catalyst was used for 5 consecutive cycles, and the Faradaic efficiency and yield of the obtained cyclopentanone oxime did not change significantly. Figure 8 As shown, the results show that the catalyst of the present invention has good electrochemical stability and has potential industrial application prospects.

Claims

1. A method for preparing a metal oxide catalyst, comprising the following steps: (1) mixing a solution of a metal compound with a solution of an organic ligand, ultrasonically treating and aging the mixture to obtain a system containing a product; (2) centrifuging, washing and vacuum drying the system containing the product to obtain a metal organic framework precursor; (3) calcining the metal organic framework precursor to obtain a metal oxide catalyst composed of metal elements, carbon elements and oxygen elements.

2. The method according to claim 1, characterized in that The metal element in the metal compound is selected from transition metals and / or rare earth metals; specifically, at least one selected from iron, cobalt, nickel, copper, zinc, lanthanum, cerium and praseodymium; The metal compound is at least one of sulfate, nitrate, hydrochloride, acetate, acetic acid pyruvate and hydrates thereof of the metal element; The organic ligand is a compound containing a carboxyl functional group, specifically at least one selected from phthalic acid, isophthalic acid, 2,5-dihydroxyterephthalic acid, 1,3,5-benzenetricarboxylic acid, benzene-1,2,4,5-tetracarboxylic acid and 1,3,5-tris(4-carboxyphenyl)benzene; The concentration of the metal compound solution is 0.01 to 0.5 mol·L -1 ; The concentration of the organic ligand solution is 0.001 to 0.05 mol·L -1 ; The solvent used in the solution of the metal compound and the solution of the organic ligand is an organic solvent, and the organic solvent can be selected from at least one of methanol, ethanol and N,N-dimethylformamide; The ultrasonic treatment time is 10 to 100 minutes; The aging time is 1 to 24 hours; The centrifugal speed is 800-12000 rpm, and the time is 3-30 min; The washing solvent is selected from at least one of water, methanol and ethanol; The vacuum drying temperature is 30 to 120° C., and the drying time is 1 to 48 hours; The calcination atmosphere is selected from nitrogen, argon or air, the calcination temperature is 200-1000° C., and the calcination time can be 1-10 hours.

3. A metal oxide catalyst prepared by the method according to claim 1 or 2.

4. An electrode composite material, characterized in that: The electrode composite material is composed of the metal oxide catalyst and the gas diffusion layer as claimed in claim 3; The metal oxide catalyst is coated on the gas diffusion layer; preferably, the coating amount of the metal oxide catalyst on the gas diffusion layer is 0.1 to 100 mg·cm -2 ; The gas diffusion layer is carbon fiber paper, carbon fiber woven cloth, carbon black paper and polytetrafluoroethylene membrane.

5. A method for preparing the electrode composite material according to claim 4, characterized in that: The method comprises the following steps: dispersing the metal oxide catalyst into an organic solvent through ultrasonic treatment to obtain a dispersion; coating the dispersion onto the gas diffusion layer to obtain the electrode composite material; Preferably, the organic solvent is at least one of methanol, ethanol, n-propanol, isopropanol and acetone; Preferably, the concentration of the dispersion is 0.1 to 20 mg·mL -1 .

6. An electrocatalytic synthesis system, characterized in that: The invention comprises the electrode composite material according to claim 4, an electrolyte solution and an electrolytic cell device.

7. The electrocatalytic synthesis system according to claim 6, characterized in that: The electrolyte solution includes an aqueous solution of a metal salt electrolyte and a ketone compound; The metal salt electrolyte is selected from at least one of potassium nitrate, sodium nitrate, potassium nitrite and sodium nitrite; The ketone compound is selected from at least one of methyl ethyl ketone, diethyl ketone, cyclopentanone and cyclohexanone; The concentration of the metal salt electrolyte in the electrolyte solution is 0.1 mol·L -1 to saturation concentration, the ketone compound concentration is 0.01-0.2 mol·L -1 ; The electrolytic cell device is an H-type electrolytic cell or a flow-type electrolytic cell.

8. Use of the electrode composite material according to claim 4 and / or the electrocatalytic synthesis system according to claim 6 or 7 in electrocatalytic synthesis of hydroxylamine.

9. A method for synthesizing hydroxylamine by ketoxime-mediated electrocatalysis, characterized in that: The method comprises the following steps: 1) using the electrocatalytic synthesis system according to claim 6 or 7, taking an alkaline earth metal salt of nitric acid or nitrous acid as a raw material, and performing an electrolytic reaction in the electrolytic cell device through the action of the electrode composite material and the electrolyte solution to obtain a system containing a cyclopentanone oxime intermediate; 2) The system containing the cyclopentanone oxime intermediate is subjected to acid hydrolysis with an inorganic acid aqueous solution to obtain hydroxylamine.

10. The method according to claim 9, characterized in that: The potential of the electrolysis reaction is -0.8 to -2.2 V vs. Ag / AgCl, and the electrolysis time is 0.1 to 3 h; The inorganic acid in the inorganic acid aqueous solution is selected from at least one of hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid; The concentration of the inorganic acid aqueous solution is 0.1 to 2 mol·L -1 ; The molar ratio of the cyclopentanone oxime to the inorganic acid is 1:1 to 10; The reaction time of the acid hydrolysis is 0.5 to 24 hours.

Citation Information

Patent Citations

  • Homogeneous-phase multi-element porous oxide material, preparation method and application thereof

    CN104445079A

  • Preparation method of polyhedral cobalt phosphide catalyst for hydrogen production through water electrolysis

    CN105107536A

  • MOFs-derived yolk-shell type copper-manganese composite bimetallic oxide and preparation method thereof

    CN111215092A

  • Method of making confined nanocatalysts within mesoporous materials and uses thereof

    CN112218716A

  • Manganese-cerium oxide material with adjustable oxygen vacancy and preparation method and application thereof

    CN112973673A

Cited By

  • Polymer type catalyst as well as preparation method and application thereof

    CN119710787A

  • Nitride synthesis method assisted by arc discharge plasma and nitride

    CN119956372A

  • Continuous cascade production method of alanine under photoelectric cooperative driving