Defective TiO2 nano material as well as preparation method and application thereof
By preparing defective TiO2 nanomaterials rich in oxygen vacancies, the problem of decreasing catalyst activity and low efficiency during the electrocatalytic reduction of NOx to NH3 is solved, and efficient and low-cost ammonia synthesis is achieved, suitable for miniaturization and renewable energy applications .
Patent Information
- Application Number
- CN202310573790.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art has problems of decreasing catalyst activity, low selectivity and efficiency in the process of NOx electrocatalytic reduction to NH3, especially the stability and selectivity of copper catalysts, and the lack of oxygen-rich oxide materials for use in This purpose.
Defective TiO2 nanomaterial prepared by hydrogenation method, which has abundant oxygen vacancies defect sites, is used for NOx electrocatalytic reduction and synthesis of NH3, and is prepared by acid-soluble, alkali-soluble, hydrothermal crystallization and hydrogenation reduction. The raw material is Wide range, low cost and simple operation.
It realizes efficient electrocatalytic reduction of NOx to NH3 at room temperature and pressure, improves ammonia yield and Faraday efficiency, and reduces energy consumption. This method is suitable for miniaturized and distributed nitrogen fixation applications, and is compatible with renewable energy.
Smart Images

Figure CN118993139A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of pollutant removal and ammonia synthesis catalyst, and specifically relates to defective TiO2 nanomaterials and a preparation method and application thereof. Background Art
[0002] Nitrogen oxides are a general term for NO, NO2, N2O, etc. As air pollutants of positive nitrogen (N) compounds, nitrogen oxides are the focus of governance.
[0003] NO x There are two main sources, namely nature and human activities. Although nitrogen oxides are produced in nature, they can cause serious harm due to the concentration of human activities, the high concentrations produced, and the fact that most of them are in human living areas. x Random discharge without control will cause serious harm to the natural environment and human production and life. x The hazards of carbon dioxide mainly include: (a) harm to humans; (b) acid rain, which damages plants; (c) ultraviolet radiation, hydrocarbons (C x H y ) forming photochemical smog; (d) reacting with ozone (O3) to destroy the ozone layer and produce new pollutants. Therefore, the treatment and comprehensive control of NOx has become the focus of current attention.
[0004] NO x It has brought serious environmental pollution and health impacts to people's lives, but NH3, which also contains nitrogen, is an important raw material for the production of nitrogen fertilizers, playing an important role in increasing crop yields and improving food quality. The currently widely used NH3 production process is the Haber-Bosch process, but it has problems such as high energy consumption and serious pollution. Therefore, it is necessary to develop a NO under mild conditions. x The method of electrocatalytic reduction to NH3 is of great significance for solving environmental pollution and realizing the production of green ammonia from renewable electricity. x Most of it exists in the form of NO, which is insoluble in water. It needs to be oxidized into water-soluble nitrate substances for nitrogen fixation, improving the contact ability between the N source and water to further increase the ammonia yield.
[0005] The process of nitrate reduction to NH3 is complicated, and the presence of hydrogen evolution side reaction will lead to low selectivity and current efficiency of synthesizing NH3. The development and application of electrocatalytic nitrate reduction technology focuses on the research of cathode catalyst materials. Good cathode catalyst materials must have advantages such as good stability, strong corrosion resistance, high conductivity, long life and good selectivity. Previous studies have shown that catalytic materials such as lead (Pb), nickel (Ni), tin (Sn), zinc (Zn), rhodium (Rh), ruthenium (Ru), iridium (Ir), palladium (Pd), copper (Cu), silver (Ag) and gold (Au) all have certain nitrate reduction activity. Among them, copper has attracted widespread attention from researchers due to its advantages such as good conductivity, weak hydrogen evolution ability and stable catalytic performance. However, its activity and selectivity in the electrocatalytic reduction of nitrate are inferior to those of precious metals, which limits its wide application. In addition, the stability of transition metal catalysts is also poor. For example, it has been reported that pure Cu metal electrodes are prone to spontaneous oxidative dissolution. At the same time, metal Cu electrodes may also suffer from surface poisoning due to competitive adsorption with other species. These problems will lead to a decrease in the activity of the catalyst in the electroreduction of nitrate.
[0006] Oxygen vacancies are widely used to improve the performance of electrocatalysts. Oxygen vacancies can serve as adsorption sites and activity, adsorbing the activated reactant N2 well, and can also "anchor" NO x The oxygen in the catalyst can weaken the NO bond and regulate the interaction between the intermediate and the catalyst, achieving a higher NH3 yield and a higher Faraday efficiency. Nano-TiO2 is widely used in photocatalytic degradation and hydrogen production, solar cells, coatings, catalyst carriers, etc. due to its high chemical stability, non-toxicity, acid and alkali resistance, simple preparation process and low cost. Compared with nanopowders, one-dimensional TiO2 materials have the advantages of large contact area with the target degradation product and are widely used as catalyst carrier materials. At present, the preparation methods of one-dimensional TiO2 include sol-gel method, thermal decomposition method, template method and hydrothermal method. The raw materials are mostly titanium dioxide, P25 or tetrabutyl titanate. Among them, the hydrothermal method is the most widely used due to its simple operation, easy control of conditions and low cost. Through investigation, no oxygen vacancy-rich oxides have been used as NO x Report on electrocatalysts for the electroreduction synthesis of NH3.
[0007] Therefore, how to provide a NO x Oxides rich in oxygen vacancies for electroreduction synthesis of NH3 electrocatalysts remain to be studied. Summary of the invention
[0008] The first object of the present invention is to provide a defective TiO2 nanomaterial, wherein the defective TiO2 nanomaterial has oxygen vacancy defect sites;
[0009] The second object of the present invention is to provide a method for preparing the aforementioned defective TiO2 nanomaterial, which has a wide range of raw material sources, low cost, simple operation, and can obtain the aforementioned defective TiO2 nanomaterial;
[0010] The third object of the present invention is to provide a defective TiO2 nanomaterial prepared by the above-mentioned preparation method;
[0011] The fourth object of the present invention is to provide applications of the aforementioned defective TiO2 nanomaterials.
[0012] To achieve the first object of the present invention, the following technical solutions are adopted:
[0013] A defective TiO2 nanomaterial, comprising the following components:
[0014] TiO2, 98-99.8wt%, such as 98.2wt%, 98.4wt%, 98.6wt%, 98.8wt%, 99wt%, 99.2wt%, 99.4wt%, and 99.6wt%;
[0015] SO3, 0.2-1wt%, such as 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt% and 0.9wt%;
[0016] P2O5, 0.1-0.2wt%, such as 0.11wt%, 0.12wt%, 0.13wt%, 0.14wt%, 0.15wt%, 0.16wt%, 0.17wt%, 0.18wt% and 0.19wt%; and
[0017] The defective TiO2 nanomaterial has oxygen vacancy defect sites.
[0018] In one embodiment, the crystal form of the defective TiO2 nanomaterial is anatase.
[0019] In one embodiment, the oxygen vacancy defect site is located 0.1-2 nm below the surface of the defective TiO2 nanomaterial, such as 0.2 nm, 0.3 nm, 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1 nm, 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm, 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm and 1.9 nm.
[0020] In one embodiment, in the defective TiO2 nanomaterial, the content of the oxygen vacancy defect sites is 0.1-1wt%, such as 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt% and 0.9wt%.
[0021] In one embodiment, the defective TiO2 nanomaterial is obtained by hydrogenating TiO2 nanowires. In one embodiment, the length of the TiO2 nanowires is 250-300 nm, such as 260 nm, 270 nm, 2680 nm and 290 nm.
[0022] In one embodiment, the diameter of the TiO2 nanowires is 20-30 nm, such as 22 nm, 24 nm, 26 nm and 28 nm.
[0023] In one embodiment, the aspect ratio of the TiO2 nanowires is 12-15, such as 12.5, 13, 13.5, 14 and 14.5.
[0024] In one embodiment, the specific surface area of the TiO2 nanowires is 230-320 m 2 / g, for example 240m 2 / g, 250m 2 / g, 260m 2 / g, 270m 2 / g, 280m 2 / g, 290m 2 / g、300m 2 / g and 310m 2 / g.
[0025] In one embodiment, the pore volume of the TiO2 nanowire is 0.74-0.90 cm 3 / g, such as 0.75cm 3 / g, 0.76cm 3 / g, 0.77cm 3 / g, 0.78cm 3 / g, 0.79cm 3 / g, 0.8cm 3 / g, 0.82cm 3 / g, 0.84cm 3 / g, 0.86cm 3 / g and 0.88cm 3 / g.
[0026] In one embodiment, the pore size of the TiO2 nanowires is 12-15 nm, such as 12.5 nm, 13 nm, 13.5 nm, 14 nm and 14.5 nm.
[0027] To achieve the second purpose of the present invention, the following technical solutions are adopted:
[0028] A method for preparing the aforementioned defective TiO2 nanomaterial comprises the following steps:
[0029] (1) Dissolution of Fe from ilmenite 2+ , Fe 3+ and TiO 2+
[0030] Mix ilmenite with concentrated sulfuric acid and undergo acid dissolution reaction, and filter out the Fe 2+ , Fe 3+ and TiO 2+ a first filtrate;
[0031] (2)Fe 3+ Reduction to Fe 2+
[0032] Add iron powder to the first filtrate obtained in step (1) to cause a reduction reaction, and filter to obtain a filtrate containing Fe 2+ and TiO 2+ a second filtrate;
[0033] (3) Crystallization to remove Fe 2+
[0034] The second filtrate obtained in step (2) is cooled and crystallized, and FeSO4·7H2O crystals and TiO-containing 2+ The third filtrate;
[0035] (4)TiO 2+ Converted to H2TiO3
[0036] Slowly adding the third filtrate obtained in step (3) into deionized water for hydrolysis reaction; then aging and filtering in sequence at room temperature to obtain a first filter cake containing H2TiO3 precipitate;
[0037] (5) H2TiO3 Calcination
[0038] The first filter cake obtained in step (4) is sequentially washed, dried and calcined to obtain mixed crystal nano-TiO2 particles;
[0039] (6) Alkali dissolution + hydrothermal crystallization
[0040] Adding the mixed crystal nano-TiO2 particles obtained in step (5) into an alkaline solution for alkaline dissolution to obtain an alkaline-dissolved mixed solution; then subjecting the obtained alkaline-dissolved mixed solution to hydrothermal crystallization, and filtering to obtain a second filter cake;
[0041] (7) Second filter cake cleaning and calcination
[0042] The second filter cake obtained in step (6) is sequentially washed, dried and calcined to obtain TiO2 nanowires;
[0043] (8) Hydrogenation reduction
[0044] The TiO2 nanowires obtained in step (7) are subjected to surface hydrogenation reduction to obtain the defective TiO2 nanomaterial.
[0045] In the preparation method of the present invention, the acid dissolution in step (1) can affect the chemical composition of the obtained defective TiO2 nanomaterial; the alkali dissolution + hydrothermal crystallization process in step (6) can affect the linear morphology of the TiO2 nanowire as a precursor; the hydrogenation reduction process in step (8) affects the catalytic efficiency of the obtained defective TiO2 nanomaterial when used as a catalyst, including ammonia yield and Faraday efficiency. The preparation method of the present invention has a wide range of raw material sources, low cost, simple operation, and can obtain the above-mentioned defective TiO2 nanomaterial.
[0046] In one embodiment, in step (1), the acid dissolution reaction conditions include: a reaction temperature of 120-160°C, such as 130°C, 140°C and 150°C; and / or a reaction time of 1-12h, such as 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h and 11h, so that the acid dissolution reaction of the ilmenite is carried out smoothly and effectively, and the Fe is dissolved smoothly. 2+ , Fe 3+ and TiO 2+ .
[0047] Those skilled in the art will appreciate that in order for the acid dissolution reaction to proceed uniformly and rapidly, the acid dissolution reaction may be carried out under stirring.
[0048] In order to improve the acid dissolution rate and acid dissolution effect, in one embodiment, in step (1), the concentration of concentrated sulfuric acid is 12-18 mol / L, such as 13 mol / L, 14 mol / L, 15 mol / L, 16 mol / L and 17 mol / L.
[0049] In order to improve the acid dissolution effect, in one embodiment, in step (1), the mass ratio of ilmenite to concentrated sulfuric acid is 1:(1.176-1.568), such as 1:1.18, 1:1.2, 1:1.22, 1:1.24, 1:1.26, 1:1.28, 1:1.3, 1:1.32, 1:1.34, 1:1.36, 1:1.38, 1:1.4, 1:1.42, 1:1.44, 1:1.46, 1:1.48, 1:1.5, 1:1.52, 1:1.54 and 1:1.56.
[0050] In one embodiment, in step (2), the conditions for the reduction reaction include: a reaction temperature of 120-160°C, such as 125°C, 130°C, 135°C, 140°C, 145°C, 150°C and 155°C; and / or a reaction time of 15-30min, such as 16min, 18min, 20min, 22min, 24min, 26min and 28min, so that the reduction reaction is carried out smoothly and effectively, and the Fe in the first filtrate obtained in step (1) is reduced to 0.05% by weight. 3+ Successfully reduced to Fe 2+ .
[0051] In order to improve the reaction efficiency and reaction effect of the reduction reaction, in one embodiment, in step (2), the amount of iron powder added is according to the mass ratio of ilmenite to iron powder of 1:(0.03-0.05), such as 1:0.032, 1:0.034, 1:0.036, 1:0.038, 1:0.04, 1:0.042, 1:0.044, 1:0.046 and 1:0.048.
[0052] Those skilled in the art will appreciate that in step (2), the filtration may be a filtration method commonly used in the art, such as suction filtration.
[0053] In order to make the crystallization proceed smoothly and effectively, the Fe in the second filtrate obtained in step (2) 2+ Crystallization generates FeSO4·7H2O crystals. In one embodiment, in step (3), the crystallization conditions include: a crystallization temperature of 0-6°C, such as 1°C, 2°C, 3°C, 4°C and 5°C; and / or a crystallization time of 2-4 days, such as 2.5 days, 3 days and 3.5 days.
[0054] Those skilled in the art will appreciate that in step (3), the filtration may be a filtration method commonly used in the art, such as suction filtration.
[0055] In one embodiment, in step (4), the hydrolysis conditions include: a hydrolysis temperature of 90-120°C, such as 95°C, 100°C, 105°C, 110°C and 115°C; and / or a hydrolysis time of 3-5h, such as 3.5h, 4h and 4.5h, so that the hydrolysis is carried out smoothly and effectively, and the TiO 2+ Effectively hydrolyzed and converted into H2TiO3 precipitation.
[0056] Those skilled in the art will appreciate that in step (4), the filtration may be a filtration method commonly used in the art, such as suction filtration.
[0057] In order to obtain nano-sized TiO2, in one embodiment, in step (4), a dispersant is further added before the hydrolysis reaction, and the amount of the dispersant added is 1-10 g / L, such as 2 g / L, 3 g / L, 4 g / L, 5 g / L, 6 g / L, 7 g / L, 8 g / L and 9 g / L.
[0058] In order to improve the aging effect, in one embodiment, in step (4), the aging temperature is 20-30°C, such as 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C and 29°C; and / or the aging time is 12-24h, such as 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h and 23h.
[0059] Those skilled in the art will appreciate that, in step (4), stirring is required to uniformly mix the third filtrate and the deionized water. In one embodiment, in step (4), the stirring time is 10-30 min, such as 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min and 28 min.
[0060] Those skilled in the art will appreciate that in step (4), the filtration may be a filtration method commonly used in the art, such as suction filtration.
[0061] In order to clean and remove impurities in the first filter cake obtained in step (4), such as Fe 2+ In one embodiment, in step (5), the cleaning is performed by using deionized water and / or anhydrous ethanol; preferably, the cleaning is performed by using deionized water first, and then using anhydrous ethanol; preferably, the cleaning is performed 2-4 times respectively. In one embodiment, in step (5), the cleaning is performed by using deionized water first for 3 times, and then using anhydrous ethanol for 3 times.
[0062] In one embodiment, in step (5), the drying conditions include: a drying temperature of 80-110°C, such as 85°C, 90°C, 95°C, 100°C and 105°C; and / or a drying time of 1-12h, such as 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h and 11h, thereby improving the drying effect of the washed first filter cake.
[0063] In one embodiment, in step (5), the calcination conditions include: a calcination temperature of 400-650°C, such as 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C and 640°C; and / or a calcination time of 4-6h, such as 4.5h, 5h and 5.5h; and / or a heating rate of 3-10°C / min, such as 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min and 9°C / min, so as to effectively calcine the first filter cake after washing and drying to obtain mixed crystal nano-TiO2 particles.
[0064] The mixed crystal nano-TiO2 particles obtained in step (5) of the present invention are of anatase and rutile mixed crystal type, spherical in shape, and have a pore volume of 0.20-0.40cm 3 / g, such as 0.30cm 3 / g; specific surface area is 53-75m 2 / g, such as 55m 2 / g, 60m 2 / g, 65m 2 / g and 70m 2 / g; the pore diameter is 14-16nm, such as 15nm.
[0065] In order to effectively alkaline dissolve the mixed crystal nano-TiO2 particles obtained in step (5), thereby breaking the original Ti-O-Ti bonds and re-bonding to form a linear morphology to facilitate the subsequent acquisition of TiO2 nanowires, in one embodiment, in step (6), the dosage ratio of the mixed crystal nano-TiO2 particles to the alkaline solution is 1g:(100-150)mL, such as 1g:110mL, 1g:120mL, 1g:130mL and 1g:140mL; and / or the concentration of the alkaline solution is 8-12mol / L, such as 8.5mol / L, 9mol / L, 9.5mol / L, 10mol / L, 10.5mol / L, 11mol / L and 11.5mol / L.
[0066] In one embodiment, in step (6), the alkaline solution includes sodium hydroxide solution and / or potassium hydroxide solution.
[0067] In order to obtain a better dispersion effect and thus a better alkali dissolution effect, in one embodiment, in step (6), a dispersant is required to be added before alkali dissolution, and the mass ratio of the dispersant to the mixed crystal nano-TiO2 particles is (1-3):1, such as 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1 and 2.9:1.
[0068] In one embodiment, in step (4) and / or step (6), the dispersant includes any one or more of polyethylene glycol, CTAB and P123 in combination; preferably, the polyethylene glycol includes any one or more of PEG400, PEG800 and PEG2000 in combination.
[0069] Those skilled in the art understand that CTAB, the full name is hexadecyltrimethylammonium bromide; P123, the full name is polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, its molecular formula is: PEO-PPO-PEO, and it is a triblock copolymer.
[0070] In one embodiment, in step (6), the alkaline dissolution is carried out under stirring at room temperature, and the preferred stirring time is 1-3 hours, such as 1.5 hours, 2 hours and 2.5 hours.
[0071] In one embodiment, in step (6), the hydrothermal crystallization conditions include: a hydrothermal crystallization temperature of 120-150°C, such as 125°C, 130°C, 135°C, 140°C and 145°C; and / or a hydrothermal crystallization time of 20-30h, such as 21h, 22h, 22h, 23h, 24h, 25h, 26h, 27h, 28h and 29h.
[0072] The present invention performs hydrothermal crystallization on alkali-soluble TiO2 to bend Ti-O bonds into linear shapes, thereby facilitating subsequent acquisition of TiO2 nanowires.
[0073] In one embodiment, in step (6), the hydrothermal crystallization is carried out in a polytetrafluoroethylene-lined stainless steel reactor.
[0074] In one embodiment, in step (7), the cleaning includes acid washing, and the acid washing is to add the second filter cake obtained in step (6) into an acid solution for mixing to adjust the pH of the solution, and then stir at 140-180°C (such as 150°C, 160°C and 170°C) for 0.5-3h (such as 1h, 1.5h, 2h and 2.5h), and filter to obtain the second filter cake after acid washing; preferably, the acid solution includes any one or more of hydrochloric acid, nitric acid, sulfuric acid and acetic acid; preferably, the concentration of the acid solution is 0.05-3mol / L, such as 0.06mol / L, 0.07mol / L, 0.08mol / L. l / L, 0.09mol / L, 0.1mol / L, 0.2mol / L, 0.4mol / L, 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L, 1mol / L, 1.1mol / L, 1.2mol / L, 1.4mol / L, 1.6mol / L, 1.8mol / L, 2mol / L, 2.2mol / L, 2.4mol / L, 2.6mol / L, 2.8mol / L and 2.9mol / L; preferably, the solution is adjusted to pH = 1 to facilitate the subsequent acquisition of a linear structure and to obtain TiO2 nanowires.
[0075] In order to remove the acid radical ions in the second filter cake obtained in step (6), in one embodiment, in step (7), the cleaning also includes water washing, and the water washing is to place the second filter cake after acid washing in hot water for water washing, and filter to obtain the washed second filter cake; preferably, the water temperature of the hot water is 25-50°C, such as 30°C, 35°C, 40°C and 45°C, and the water washing process is preferably accompanied by stirring, and the preferred number of water washings is 4-10 times, such as 5, 6, 7, 8, 9 times.
[0076] In order to further remove the acid radical ions in the second filter cake, in one embodiment, in step (7), the cleaning also includes ultrasonic water washing, and the ultrasonic water washing is to wash the second filter cake after water washing under ultrasonic conditions, and filter to obtain the second filter cake after ultrasonic water washing; preferably, ultrasonic water washing is performed until the solution conductivity is <600μs / cm, such as 590μs / cm, 580μs / cm, 550μs / cm, 500μs / cm, 450μs / cm, etc.
[0077] In one embodiment, in step (7), the drying conditions include: a drying temperature of 120-150°C, such as 125°C, 130°C, 135°C, 140°C and 145°C; and / or a drying time of 8-12h, such as 8.5h, 9h, 9.5h, 10h, 10.5h, 11h and 11.5h.
[0078] In one embodiment, in step (7), the calcination conditions include: a calcination temperature of 400-650°C, such as 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C, 580°C, 600°C, 620°C and 640°C; and / or a calcination time of 2-5h, such as 2.5h, 3h, 3.5h, 4h and 4.5h, so as to effectively calcine the washed and dried second filter cake to obtain TiO2 nanowires.
[0079] Those skilled in the art will appreciate that the calcination in the present invention can be carried out in a calcination device commonly used in the art, such as a muffle furnace.
[0080] In one embodiment, in step (8), the conditions for hydrogenation reduction include: the hydrogenation reduction pressure is normal pressure; and / or the hydrogenation reduction atmosphere is H2 atmosphere, preferably including (4.6-100)% H2 atmosphere; when it is not completely H2, other gases can be inert gases, such as N2, Ar, He, etc.; and / or the hydrogen flow rate is 100-1000ml / min, such as 200ml / min, 300ml / min, 400ml / min, 500ml / min, 600ml / min, etc. ml / min, 700ml / min, 800ml / min and 900ml / min; and / or the hydrogenation reduction temperature is 450-600°C, such as 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C and 590°C; and / or the hydrogenation reduction time is 2-12h, such as 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h and 11h.
[0081] To achieve the third object of the present invention, a defective TiO2 nanomaterial prepared by the above-mentioned preparation method is provided.
[0082] To achieve the fourth object of the present invention, there is provided an application of the aforementioned defective TiO2 nanomaterial in the electrocatalytic reduction of nitrogen oxides to synthesize ammonia, preferably in a reaction system of NO oxidation and electrocatalytic reduction of nitrates.
[0083] In the reaction system of NO oxidation and electrocatalytic reduction of nitrate, the water-insoluble NO is first oxidized to water-soluble NO2, and then the nitrate is further electrocatalytically reduced to ammonia (nitrate-to-ammonia reduction reaction, NARR). xWhile eliminating pollution, it synthesizes NH3 of high industrial value. This method can bypass the high temperature and high pressure (300-500℃, 200-300atm) Haber process. Compared with the Haber process with complex facilities and processes, harsh reaction conditions, and huge energy consumption and pollution, the electrocatalytic ammonia synthesis technology is more flexible and convenient, and is compatible with the power supply of renewable energy sources (wind energy, solar energy, tidal energy, etc.) with temporal and spatial fluctuations, realizing a new type of nitrogen fixation concept of miniaturization and distribution. In addition, this route can also connect with the denitrification process in environmental protection enterprises, avoid the production of low-value and difficult-to-use N2, establish an artificial "nitrogen cycle", and achieve sustainable development of the nitrogen-containing chemical industry.
[0084] The process of nitrate reduction to NH3 is complicated, and the presence of hydrogen evolution side reaction will lead to low selectivity and current efficiency of synthesizing NH3. The development and application of electrocatalytic reduction of nitrate technology focuses on the research of cathode catalyst materials. Good cathode catalyst materials must have advantages such as good stability, strong corrosion resistance, high conductivity, long life and good selectivity. Previous studies have shown that catalytic materials such as lead (Pb), nickel (Ni), tin (Sn), zinc (Zn), rhodium (Rh), ruthenium (Ru), iridium (Ir), palladium (Pd), copper (Cu), silver (Ag) and gold (Au) all have certain nitrate reduction activity. Among them, copper has attracted widespread attention from researchers due to its advantages such as good conductivity, weak hydrogen evolution ability and stable catalytic performance. However, its activity and selectivity in the electrocatalytic reduction of nitrate are poor compared with those of precious metals, which limits its wide application. In addition, the stability of transition metal catalysts also needs to be further improved. For example, it has been reported that pure Cu metal electrodes are prone to spontaneous oxidative dissolution. At the same time, metal Cu electrodes may also suffer from surface poisoning due to competitive adsorption with other species. These problems will lead to a decrease in the activity of the catalyst in the electroreduction of nitrate.
[0085] In the present invention, the transition metal oxide TiO2 can form oxygen vacancies (Ov) to enhance the NRR performance.
[0086] In one embodiment, the application is to use the defective TiO2 nanomaterial as a catalyst in the electrocatalytic reduction of nitrogen oxides to synthesize ammonia.
[0087] In one embodiment, the application method is as follows:
[0088] 300-800ppm (such as 400ppm, 500ppm, 600ppm and 700ppm) of NO and 3-10% (such as 4%, 5%, 6%, 7%, 8% and 9%) of O2 are continuously introduced at the same time, the electrocatalytic reduction reaction of nitrate occurs at the cathode, and the NO oxidation and electrocatalytic reduction reactions of nitrate are carried out simultaneously in the H-type electrolytic cell.
[0089] In one embodiment, the electrocatalytic reduction of nitrate is carried out using a cation exchange membrane (such as Nafion 117 membrane) or an anion exchange membrane.
[0090] In one embodiment, the electrocatalytic reduction of nitrates uses a three-electrode system, that is, the defective TiO2 nanomaterial / CP electrode, the platinum sheet electrode and the Ag / AgCl electrode are used as the working electrode, the counter electrode and the reference electrode respectively; the electrolyte uses a KOH electrolyte.
[0091] The electrocatalytic reduction reaction of nitrate occurs at the cathode (the defective TiO2 nanomaterial / CP electrode).
[0092] In one embodiment, the electrocatalytic reduction of nitrate is carried out on a CHI760E electrochemical analyzer from CH Instrument Co., Ltd., Shanghai, China.
[0093] In one embodiment, a 0.1 mol / L KOH electrolyte is first subjected to N2 purification for 30 minutes, and then an electrocatalytic reduction reaction of nitrate is carried out in a N2-saturated 0.1 mol / L KOH solution; after 2 hours of controlled potential electrolysis, the electrolyte in the cathode cell is collected for color development, and its absorbance is measured with an ultraviolet spectrophotometer to calculate its ammonia yield (NH3 generation rate) and Faraday efficiency (FE).
[0094] The calculations of NH3 generation rate and Faradaic efficiency (FE) are as follows:
[0095] in,
[0096] V NH3 is the ammonia yield, in μg·mg cat -1 ·h -1 ; C is the concentration of NH3 in the electrolyte, in μg·mL -1 ; V is the volume of the electrolyte, in mL; t is the electrolysis time, in h; m cat is the electrode mass in mg.
[0097]
[0098] FE is Faraday efficiency, unit is %; F is Faraday constant, its value is 96500C·mol -1 ; Q is the total charge consumption in the electrolysis process, unit is C.
[0099] The beneficial effects of the present invention are:
[0100] The defective TiO2 nanomaterial of the present invention has abundant oxygen vacancy defect sites. When it is applied to the reaction of electrocatalytic synthesis of ammonia, the oxygen vacancy defect sites can serve as overflow active sites and adsorption sites of O atoms, adsorbing and activating the reactant NO well to achieve oxidative nitrogen fixation, and can also "anchor" NO. x The O atoms in the catalyst can weaken the NO bond and regulate the interaction between the intermediate and the catalyst, thereby optimizing the reaction path to achieve a higher NH3 yield and hindering the formation of by-products, thereby improving the Faradaic efficiency.
[0101] The method for preparing defective TiO2 nanomaterials of the present invention has a wide range of raw materials, which are cheap and easy to obtain, low preparation cost, simple operation, and adopts a hydrogenation method to hydrogenate and reduce TiO2 nanowires to obtain the aforementioned defective TiO2 nanomaterials rich in oxygen vacancy defect sites, and is easy to achieve large-scale production;
[0102] When the defective TiO2 nanomaterial of the present invention is applied to the electrocatalytic synthesis of ammonia, it has a high ammonia yield and Faraday efficiency; the NH3 yield reaches 2.52mmol·g at room temperature and pressure at the optimal potential of -0.3V vs.RHE. cat -1 ·h -1 , Faraday efficiency reaches 10.2%;
[0103] When the defective TiO2 nanomaterial of the present invention is used in the electrocatalytic synthesis of ammonia, the electrocatalytic method is used without the need for thermal catalysis, and NO can be achieved through the coupling of wind power + photovoltaic power generation. x The greening of the reduction process to synthetic ammonia can significantly save energy compared to the Haber-Bosch process. It can be deployed in thermal power, steel and cement plants in a miniaturized or distributed manner to achieve flue gas NO x Resource utilization; Compared with the existing denitrification technology, the traditional selective catalytic reduction process (NH3-SCR) converts NO x The denitrification technology of reducing to N2 can realize the resource utilization of nitrogen sources, and the product NH3 can be further utilized as a hydrogen storage carrier, green fuel and fertilizer. BRIEF DESCRIPTION OF THE DRAWINGS
[0104] Figure 1 It is a process roadmap for the preparation of defective TiO2 nanomaterials of the present invention;
[0105] Figure 2 is the X-ray powder diffraction pattern of the mixed crystal nano-TiO2 particle B1 and the TiO2 nanowire C1 in Example 1;
[0106] Figure 3 is a nitrogen adsorption-desorption isotherm diagram of the TiO2 nanowire C1 in Example 1;
[0107] Figure 4 This is a 150,000-fold SEM image of the TiO nanowire C1 in Example 1;
[0108] Figure 5 This is a 300,000-fold SEM image of the TiO nanowire C1 in Example 1;
[0109] Figure 6 is an appearance diagram of the defective TiO nanomaterial A1 in Example 1;
[0110] Figure 7 is the EPR graph of the defective TiO nanomaterial A1 in Example 1;
[0111] Figure 8 It is the graph of ammonia yield variation under different electrode potentials;
[0112] Fig. 9 This is a graph showing the change in Faraday efficiency at different electrode potentials. DETAILED DESCRIPTION
[0113] The technical scheme and its effects of the present invention are further described below in conjunction with specific implementation methods / examples. The following implementation methods / examples are only used to illustrate the content of the present invention, and the invention is not limited to the following implementation methods or examples. Simple changes made to the present invention using the concept of the present invention are all within the scope of protection claimed by the present invention.
[0114] The sources of the raw materials and equipment used in the following examples and comparative examples are as follows:
[0115] Ilmenite, Panzhihua ilmenite mine in Sichuan;
[0116] Concentrated sulfuric acid, Chinese medicine, 95.0-98.0wt%;
[0117] Iron powder, Zhanfei Chemical, reduced iron powder, 200 mesh, iron content ≥95%;
[0118] Dispersant-polyethylene glycol, PEG400, Sinopharm, CAS 25322-68-3;
[0119] Alkaline solution-sodium hydroxide solution, Chinese medicine, 96wt%;
[0120] Anhydrous ethanol, Chinese medicine, 99.7wt%;
[0121] Hydrochloric acid, Chinese medicine, 36.5wt%;
[0122] Muffle furnace, model Sx2-2.5-1, manufacturer Lichen Technology;
[0123] The reactor is a 200mL polytetrafluoroethylene reactor manufactured by Shanghai Yanzheng.
[0124] Test method:
[0125] X-ray powder diffraction pattern: the prepared mixed crystal nano-TiO2 particles and TiO2 nanowires were scanned by X-ray at room temperature using D8 ADVANCE of Bruker, Germany, to obtain their X-ray powder diffraction patterns;
[0126] Nitrogen adsorption-desorption isotherm diagram: ASAP2020 of Micromertics Company of the United States was used to perform nitrogen isothermal adsorption-desorption analysis on the prepared TiO2 nanowires at room temperature to obtain the nitrogen adsorption-desorption isotherm diagram of the TiO2 nanowires;
[0127] SEM image: The prepared TiO2 nanowires were scanned by SEM at room temperature using Nova NanoSEM 450 from FEI Company of Czech Republic to obtain the SEM image of TiO2 nanowires;
[0128] Appearance picture, taking a picture of the prepared defective TiO2 nanomaterial under normal temperature and pressure conditions to obtain an appearance picture of the defective TiO2 nanomaterial;
[0129] EPR graph: paramagnetic resonance spectroscopy analysis was performed on the prepared defective TiO2 nanomaterial at room temperature and normal pressure using BRUKER 100 to obtain the EPR graph of the defective TiO2 nanomaterial.
[0130] Example 1
[0131] like Figure 1 As shown, defective TiO2 nanomaterial A1 is prepared according to the following method:
[0132] (1) Dissolution of Fe from ilmenite 2+ , Fe 3+ and TiO 2+
[0133] Mix ilmenite with concentrated sulfuric acid and react with acid at 140℃ for 6h, and filter to obtain the Fe 2+ , Fe 3+ and TiO 2+ The first filtrate; wherein,
[0134] In step (1), the concentration of concentrated sulfuric acid is 13.5 mol / L;
[0135] In step (1), the mass ratio of ilmenite to concentrated sulfuric acid is 1:1.3;
[0136] (2)Fe 3+ Reduction to Fe 2+
[0137] Add iron powder to the first filtrate obtained in step (1) and carry out reduction reaction at 120°C for 20 min, and filter to obtain the Fe 2+ and TiO 2+ The second filtrate; wherein,
[0138] In step (2), the amount of iron powder added is based on a mass ratio of ilmenite to iron powder of 1:0.04;
[0139] (3) Crystallization to remove Fe 2+
[0140] The second filtrate obtained in step (2) is cooled and crystallized, and FeSO4·7H2O crystals and TiO-containing 2+ The third filtrate; wherein,
[0141] In step (3), the crystallization temperature is 3°C and the crystallization time is 3 days;
[0142] (4)TiO 2+ Converted to H2TiO3
[0143] The third filtrate obtained in step (3) is slowly added into deionized water, stirred for 20 minutes, heated to the hydrolysis temperature under stirring, and then a dispersant is added and the hydrolysis is maintained at a constant temperature; then aged and filtered in sequence at room temperature to obtain a first filter cake containing H2TiO3 precipitate; wherein,
[0144] In step (4), the hydrolysis temperature is 100° C. and the hydrolysis time is 4 h;
[0145] In step (4), the dispersant is PEG400; the amount of the dispersant added is 5 g / L;
[0146] In step (4), the aging temperature is 25° C. and the aging time is 18 h;
[0147] (5) H2TiO3 Calcination
[0148] The first filter cake obtained in step (4) is washed, dried and calcined in sequence to obtain mixed crystal nano-TiO2 particles B1; wherein
[0149] In step (5), the cleaning is firstly performed with deionized water for 3 times, and then with anhydrous ethanol for 3 times;
[0150] In step (5), the drying temperature is 95° C. and the drying time is 6 h;
[0151] In step (5), calcination is carried out in a muffle furnace at a calcination temperature of 520° C., a calcination time of 5 h, and a heating rate of 5° C. / min;
[0152] (6) Alkali dissolution + hydrothermal crystallization
[0153] The mixed crystal nano-TiO2 particles obtained in step (5) are added to an alkaline solution and dissolved in the presence of PEG400 to obtain an alkaline-soluble mixed solution; the obtained alkaline-soluble mixed solution is then hydrothermally crystallized and filtered to obtain a second filter cake; wherein:
[0154] In step (6), the ratio of the mixed crystal nano-TiO2 particles to the alkaline solution is 1 g:120 mL; the alkaline solution is a sodium hydroxide solution with a concentration of 10 mol / L;
[0155] In step (6), the dispersant is PEG400, and the mass ratio of the dispersant PEG400 to the mixed crystal nano-TiO2 particles is 2:1;
[0156] In step (6), the alkali dissolution is carried out under stirring at room temperature for 2 hours;
[0157] In step (6), the hydrothermal crystallization is carried out in a polytetrafluoroethylene-lined stainless steel reactor; the hydrothermal crystallization temperature is 135° C., and the hydrothermal crystallization time is 25 h;
[0158] (7) Second filter cake cleaning and calcination
[0159] The second filter cake obtained in step (6) is washed, dried and calcined in sequence to obtain TiO2 nanowires C1; wherein,
[0160] In step (7), the cleaning includes acid washing, and the acid washing is to add the second filter cake obtained in step (6) into a hydrochloric acid solution with a concentration of 0.1 mol / L, mix the mixture to adjust the pH of the solution to pH = 1, then stir at 160° C. for 2 h, and filter to obtain the second filter cake after acid washing;
[0161] In step (7), the washing further comprises water washing, wherein the second filter cake after acid washing is placed in hot water at a temperature of 25° C. and washed 6 times, accompanied by stirring during the washing process, and then filtered to obtain the washed second filter cake;
[0162] In step (7), the cleaning further comprises ultrasonic washing, wherein the ultrasonic washing is to wash the second filter cake after washing under ultrasonic conditions until the solution conductivity is less than 600 μs / cm, and then filter to obtain the second filter cake after ultrasonic washing;
[0163] In step (7), the drying temperature is 135° C. and the drying time is 10 h;
[0164] In step (7), calcination is carried out in a muffle furnace at a calcination temperature of 520° C. and a calcination time of 3.5 h;
[0165] (8) Hydrogenation reduction
[0166] The TiO2 nanowires obtained in step (7) are subjected to surface hydrogenation reduction to obtain the defective TiO2 nanomaterial A1; wherein:
[0167] In step (8), the conditions for hydrogenation reduction include: hydrogenation reduction pressure is normal pressure; hydrogenation reduction atmosphere is 100% H2 atmosphere, hydrogen flow rate is 500ml / min; hydrogenation reduction temperature is 460°C, hydrogenation reduction time is 12h; defective TiO2 nanomaterial A1 is obtained.
[0168] The TiO2 nanowire C1 obtained in step (7) has a length of 250 nm, a diameter of 20 nm, an aspect ratio of 12, and a specific surface area of 230 m 2 / g, pore volume is 0.74cm 3 / g, pore size is 12nm.
[0169] The defective TiO2 nanomaterial A1 obtained in step (8) comprises the following components:
[0170] TiO2, 98wt%; SO3, 0.55wt%; P2O5, 0.16wt%; and has oxygen vacancy defect sites; the crystal form is anatase;
[0171] The oxygen vacancy defect site is located 2 nm below the surface of the defective TiO2 nanomaterial A1;
[0172] In the defective TiO2 nanomaterial A1, the content of the oxygen vacancy defect sites is 1 wt%.
[0173] according to Figure 2 It can be seen that the mixed-crystal nano-TiO2 particles B1 obtained in step (5) are mainly composed of anatase and rutile, and the TiO2 nanowires C1 obtained in step (7) are mainly composed of anatase.
[0174] according to Figure 3 It can be seen from the N2 adsorption-desorption curve of the TiO2 nanowire C1 obtained in step (7) that the TiO2 nanowire has mesoporous channels.
[0175] according to Figure 4 and Figure 5 It can be seen that the TiO2 nanowires C1 obtained in step (7) have a linear morphology.
[0176] according to Figure 6 It can be seen that the defective TiO2 nanomaterial A1 obtained in step (8) is a black-gray powder at room temperature and pressure.
[0177] according to Figure 7 It can be seen that the defective TiO2 nanomaterial A1 obtained in step (8) has the highest ammonia yield at a potential of -0.3 V vx RHE.
[0178] Application Example 1
[0179] The defective TiO2 nanomaterial A1 obtained in Example 1 was applied to the reaction of electrocatalytic reduction of nitrate to produce ammonia, as follows:
[0180] In a typical H-type electrolytic cell, a Nafion 117 membrane and a three-electrode system were used to perform the electrocatalytic reduction of nitrate to produce ammonia; the three-electrode system included the obtained defective TiO2 nanomaterial A1 / CP electrode, a platinum electrode, and an Ag / AgCl electrode, which were used as the working electrode, counter electrode, and reference electrode, respectively, on a CHI 760E electrochemical analyzer from CH Instrument Co., Ltd. in Shanghai, China; during the process, the 0.1 mol / L KOH electrolyte was first purified by N2 for 30 minutes, and then the electrocatalytic reduction of nitrate was performed in a 0.1 mol / L KOH solution saturated with N2; after 2 hours of controlled potential electrolysis, the electrolyte in the cathode cell was collected for color development, and its absorbance was measured by an ultraviolet spectrophotometer to calculate its ammonia yield and Faraday efficiency (FE). The results are as follows:
[0181] Ammonia yield was 2.52 mmol·g cat -1 ·h -1 ;
[0182] The Faradaic efficiency (FE) was 10.2%.
[0183] Example 2
[0184] Defective TiO2 nanomaterial A2 was prepared according to the method of Example 1; wherein the defective TiO2 nanomaterial A2 differs from Example 1 only in the following aspects:
[0185] In step (1), the acid dissolution reaction temperature is 120° C. and the acid dissolution reaction time is 12 h;
[0186] In step (1), the concentration of concentrated sulfuric acid is 12 mol / L;
[0187] In step (1), the mass ratio of ilmenite to concentrated sulfuric acid is 1:1.176;
[0188] In step (6), the ratio of mixed crystal nano-TiO2 particles to alkaline solution is 1 g:100 mL;
[0189] In step (6), the mass ratio of the dispersant to the mixed crystal nano-TiO2 particles is 3:1;
[0190] In step (6), the hydrothermal crystallization temperature is 120° C. and the hydrothermal crystallization time is 30 h;
[0191] In step (8), the hydrogen flow rate is 100 ml / min; the hydrogenation reduction temperature is 450° C., and the hydrogenation reduction time is 2 h; and defective TiO2 nanomaterial A2 is obtained.
[0192] The TiO2 nanowire C2 obtained in step (7) has a length of 262 nm, a diameter of 21 nm, an aspect ratio of 12.5, and a specific surface area of 252 m 2 / g, pore volume is 0.82cm 3 / g, and the pore size is 14.3nm.
[0193] The obtained defective TiO2 nanomaterial A2 comprises the following components:
[0194] TiO2, 98.6wt%; SO3, -0.20wt%; P2O5, 0.18wt%; and has oxygen vacancy defect sites; the crystal form is anatase;
[0195] The oxygen vacancy defect site is located 0.12 nm below the surface of the defective TiO2 nanomaterial A2;
[0196] In the defective TiO2 nanomaterial A2, the content of the oxygen vacancy defect sites is 0.1 wt%.
[0197] Application Example 2
[0198] According to the method of Application Example 1, the defective TiO2 nanomaterial A2 obtained in Example 2 was applied to the reaction of electrocatalytic reduction of nitrate to produce ammonia, and its ammonia yield and Faraday efficiency (FE) were calculated. The results are as follows:
[0199] Ammonia yield was 1.44 mmol·g cat -1 ·h -1 ;
[0200] The Faradaic efficiency (FE) was 7.3%.
[0201] Example 3
[0202] Defective TiO2 nanomaterial A3 was prepared according to the method of Example 1; wherein the defective TiO2 nanomaterial A3 differs from Example 1 only in the following aspects:
[0203] In step (1), the acid dissolution reaction temperature is 160° C. and the acid dissolution reaction time is 1 h;
[0204] In step (1), the concentration of concentrated sulfuric acid is 18 mol / L;
[0205] In step (1), the mass ratio of ilmenite to concentrated sulfuric acid is 1:1.568;
[0206] In step (6), the ratio of mixed crystal nano-TiO2 particles to alkaline solution is 1 g:150 mL;
[0207] In step (6), the mass ratio of the dispersant to the mixed crystal nano-TiO2 particles is 1:1;
[0208] In step (6), the hydrothermal crystallization is carried out in a polytetrafluoroethylene-lined stainless steel reactor; the hydrothermal crystallization temperature is 150° C., and the hydrothermal crystallization time is 20 h;
[0209] In step (8), the hydrogen flow rate is 1000 ml / min; the hydrogenation reduction temperature is 600° C., and the hydrogenation reduction time is 2 h; and defective TiO2 nanomaterial A3 is obtained.
[0210] The obtained TiO2 nanowire C3 has a length of 297nm, a diameter of 20nm, an aspect ratio of 14.85, and a specific surface area of 318m 2 / g, pore volume is 0.89cm 3 / g, and the pore size is 14.8nm.
[0211] The obtained defective TiO2 nanomaterial A3 comprises the following components:
[0212] TiO2, 98.8wt%; SO3, 1wt%; P2O5, -0.2wt%; and has oxygen vacancy defect sites; the crystal form is anatase;
[0213] The oxygen vacancy defect site is located 0.42 nm below the surface of the defective TiO2 nanomaterial A3;
[0214] In the defective TiO2 nanomaterial A3, the content of the oxygen vacancy defect sites is 0.44 wt%.
[0215] Application Example 3
[0216] According to the method of Application Example 1, the defective TiO2 nanomaterial A3 obtained in Example 3 was applied to the reaction of electrocatalytic reduction of nitrate to produce ammonia, and its ammonia yield and Faraday efficiency (FE) were calculated. The results are as follows:
[0217] Ammonia yield was 2.65 mmol·g cat -1 ·h -1 ;
[0218] The Faradaic efficiency (FE) was 8.8%.
[0219] Comparative Example 1
[0220] Commercially available titanium oxide P25 is directly used to carry out the surface hydrogenation reduction of step (8) to obtain defective TiO2 nanomaterial A1'; wherein the conditions of the hydrogenation reduction are the same as those in Example 1.
[0221] The obtained defective TiO2 nanomaterial A1' comprises the following components:
[0222] TiO2, 100wt%; and having oxygen vacancy defect sites; the crystal form is anatase;
[0223] The oxygen vacancy defect site is located 0.03 nm below the surface of the defective TiO2 nanomaterial A1';
[0224] In the defective TiO2 nanomaterial A1', the content of the oxygen vacancy defect sites is 0.02 wt%.
[0225] Application Comparative Example 1
[0226] According to the method of Application Example 1, the defective TiO2 nanomaterial A1' obtained in Comparative Example 1 was applied to the reaction of electrocatalytic reduction of nitrate to produce ammonia, and its ammonia yield and Faraday efficiency (FE) were calculated. The results are as follows:
[0227] Ammonia yield was 0.23 mmol·g cat -1 ·h -1 ;
[0228] The Faradaic efficiency (FE) is 1.4%.
[0229] Comparative Example 2
[0230] The TiO2 nanomaterial A2' was prepared according to the method of Example 1; wherein the only differences from Example 1 are as follows:
[0231] Only steps (1) to (7) are performed, and the surface hydrogenation reduction of step (8) is not performed.
[0232] The obtained TiO2 nanomaterial A2' is the TiO2 nanowire C1 obtained in step (7). There is no oxygen vacancy defect site.
[0233] Application Comparative Example 2
[0234] According to the method of Application Example 1, the TiO2 nanomaterial A2' obtained in Comparative Example 2 was applied to the reaction of electrocatalytic reduction of nitrate to produce ammonia, and its ammonia yield and Faraday efficiency (FE) were calculated. The results are as follows:
[0235] Ammonia yield is 0;
[0236] The Faradaic efficiency (FE) is 0.
[0237] According to the comparison between Examples 1-3 and the application of Examples 1-3 and Comparative Examples 1-2 and the application of Comparative Examples 1-2, it can be seen that the defective TiO2 nanomaterial of the present invention has abundant oxygen vacancy defect sites. When it is applied to the reaction of electrocatalytic synthesis of ammonia, the NH3 yield is high and the Faraday efficiency is high.
Claims
1. A defective TiO2 nanomaterial, characterized in that: The defective TiO2 nanomaterial comprises the following components: TiO2, 98-99.8wt%; SO3, 0.2-1wt%; P2O5, 0.1-0.2wt%; and The defective TiO2 nanomaterial has oxygen vacancy defect sites.
2. The defective TiO2 nanomaterial according to claim 1, characterized in that: The crystal form of the defective TiO2 nanomaterial is anatase; Preferably, the oxygen vacancy defect site is located 0.1-2 nm below the surface of the defective TiO2 nanomaterial; Preferably, in the defective TiO2 nanomaterial, the content of the oxygen vacancy defect sites is 0.1-1 wt%.
3. The defective TiO2 nanomaterial according to claim 1 or 2, characterized in that: The defective TiO2 nanomaterial is obtained by hydrogenating TiO2 nanowires; Preferably, the length of the TiO2 nanowire is 250-300nm; and / or The diameter of the TiO2 nanowires is 20-30 nm; and / or The aspect ratio of the TiO2 nanowires is 12-15; and / or The specific surface area of the TiO2 nanowires is 230-320 m 2 / g; and / or The pore volume of the TiO2 nanowire is 0.74-0.90 cm 3 / g; and / or The pore diameter of the TiO2 nanowire is 12-15 nm.
4. A method for preparing a defective TiO2 nanomaterial as claimed in any one of claims 1 to 3, characterized in that: The method comprises the following steps: (1) Dissolution of Fe from ilmenite 2+ , Fe 3+ and TiO 2+ Mix ilmenite with concentrated sulfuric acid and undergo acid dissolution reaction, and filter out the Fe 2+ , Fe 3+ and TiO 2+ a first filtrate; (2)Fe 3+ Reduction to Fe 2+ Add iron powder to the first filtrate obtained in step (1) to cause a reduction reaction, and filter to obtain a filtrate containing Fe 2+ and TiO 2+ a second filtrate; (3) Crystallization to remove Fe 2+ The second filtrate obtained in step (2) is cooled and crystallized, and FeSO4·7H2O crystals and TiO-containing 2+ The third filtrate; (4)TiO 2+ Converted to H2TiO3 Slowly adding the third filtrate obtained in step (3) into deionized water for hydrolysis reaction; then aging and filtering in sequence at room temperature to obtain a first filter cake containing H2TiO3 precipitate; (5) H2TiO3 Calcination The first filter cake obtained in step (4) is sequentially washed, dried and calcined to obtain mixed crystal nano-TiO2 particles; (6) Alkali dissolution + hydrothermal crystallization Adding the mixed crystal nano-TiO2 particles obtained in step (5) into an alkaline solution for alkaline dissolution to obtain an alkaline-dissolved mixed solution; then subjecting the obtained alkaline-dissolved mixed solution to hydrothermal crystallization, and filtering to obtain a second filter cake; (7) Second filter cake cleaning and calcination The second filter cake obtained in step (6) is sequentially washed, dried and calcined to obtain TiO2 nanowires; (8) Hydrogenation reduction The TiO2 nanowires obtained in step (7) are subjected to surface hydrogenation reduction to obtain the defective TiO2 nanomaterial.
5. The method according to claim 4, characterized in that: In step (1), the acid dissolution reaction conditions include: a reaction temperature of 120-160° C., and / or a reaction time of 1-12 h; and / or In step (1), the concentration of the concentrated sulfuric acid is 12-18 mol / L; and / or In step (1), the mass ratio of ilmenite to concentrated sulfuric acid is 1:(1.176-1.568).
6. The method according to claim 4 or 5, characterized in that: In step (6), the ratio of mixed crystal nano-TiO2 particles to alkaline solution is 1g: (100-150)mL; and / or In step (6), a dispersant needs to be added before alkali dissolution, and the mass ratio of the dispersant to the mixed crystal nano-TiO2 particles is (1-3):1; and / or In step (6), the hydrothermal crystallization conditions include: a hydrothermal crystallization temperature of 120-150° C., and / or a hydrothermal crystallization time of 20-30 h.
7. The method according to any one of claims 4 to 6, characterized in that: In step (8), the conditions for hydrogenation reduction include: the hydrogenation reduction pressure is normal pressure, and / or the hydrogenation reduction atmosphere is H2 atmosphere, and / or the hydrogen flow rate is 100-1000 ml / min, and / or the hydrogenation reduction temperature is 450-600°C, and / or the hydrogenation reduction time is 2-12 h.
8. A defective TiO2 nanomaterial prepared according to the method according to any one of claims 4 to 7.
9. Use of the defective TiO2 nanomaterial as claimed in any one of claims 1 to 3 and any one of claims 8 in the electrocatalytic reduction of nitrogen oxides to synthesize ammonia, preferably in a reaction system of NO oxidation and electrocatalytic reduction of nitrates.
10. The use according to claim 9, characterized in that: The application is to use the defective TiO2 nanomaterial as a catalyst in the electrocatalytic reduction of nitrogen oxides to synthesize ammonia.
Citation Information
Cited By
Ruthenium-based defect TiO2 photocatalytic synthesis ammonia catalyst as well as preparation method and application thereof
CN118767954A