Preparation method of nano negative ion release material containing rare earth elements

By preparing rare earth element doped In2O3:Ce nanoparticles and lithium niobate powder, combined with ball milling and polarization treatment, the efficiency of rare earth element nanonegative ion release materials in air and water purification is solved, and efficient negative ion release and Improved performance, improves air and water quality, while also beneficial to human health.

CN118993147APending Publication Date: 2024-11-22HEYE HEALTH TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411156356.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

How to effectively improve the air and water quality in densely populated areas, especially in severe pollution, use materials that combine rare earth elements with In2O3 nanoparticles to regulate optical and magnetic properties to improve the performance of nano-negative ion release materials.

Method used

By preparing In2O3:Ce nanoparticles, rare earth element doped with ethyl orthosilicate, polyvinylpyrrolidone solution and lithium niobate powder, ball milling and polarization treatment are used to form nano-negative ion lithium niobate powder to ensure the dispersion of the material , uniform particle size distribution and efficient negative ion release.

Benefits of technology

The good dispersion and uniform particle size distribution of nanoparticles are achieved, the performance consistency of the material and negative ion release performance are improved, the purification capacity of air and water is enhanced, and the health benefits of improving brain function and metabolism are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993147A_ABST
    Figure CN118993147A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a nano negative ion release material containing rare earth elements, which comprises the following steps: preparing In2O3: Ce nano particles, preparing rare earth element doped tetraethoxysilane (TEOS), preparing a polyvinylpyrrolidone (PVP) solution, preparing lithium niobate powder, preparing nano negative ion lithium niobate powder and the like. The rare earth element-containing nano negative ion release material prepared by creatively combining preparation methods such as a heating method, a pressing method and a voltage applying polarization method has the advantages of simple preparation process, efficient negative ion release, air purification and the like, and can be applied to multiple fields such as the building material industry, agricultural gardens and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a nanometer negative ion releasing material containing rare earth elements. Background Art

[0002] With the continuous progress and development of society, semiconductor magnetic materials have immeasurable research value. Rare magnetic oxides such as In2O3, SnO2 and ZnO have a wide range of applications in real life due to their potential applications in magnetic, optical and electronic devices. For example, magnetic sensor devices used in the automotive and aerospace industries also use the electronic charge properties of semiconductors in electronics and computers. Rare earth elements have their unique electronic structure - 4f orbital. When rare earth elements and In2O3 nanoparticles are added together, the optical and magnetic physical properties of the main matrix can be adjusted, which expands the scope of use of materials. Due to human group living habits and extensive industrial development, a large amount of pollutants are concentratedly discharged into the atmosphere and water bodies, resulting in the unsatisfactory quality of the earth's air and water. How to effectively improve the quality of air and water in densely populated areas is a very meaningful challenge. Air negative ions, also known as negative oxygen ions, have the ability to purify air and water, destroy bacteria, degrade pollutants, and are beneficial to the human body, such as improving brain function and metabolism. Summary of the invention

[0003] In view of the above problems, the present invention provides a method for preparing a nanometer negative ion releasing material containing rare earth elements.

[0004] The first technical purpose of the present invention is nanoparticles containing rare earth elements.

[0005] The second technical purpose of the present invention is a nanometer negative ion releasing material containing rare earth elements.

[0006] The invention relates to a method for preparing a nanometer negative ion releasing material containing rare earth elements, comprising the following steps: preparing In2O3:Ce nanometer particles, preparing tetraethyl orthosilicate (TEOS) doped with rare earth elements, preparing polyvinyl pyrrolidone (PVP) solution, preparing lithium niobate powder, and preparing nanometer negative ion lithium niobate powder.

[0007] Preferably, step (1) preparation of In2O3:Ce nanoparticles First, a small amount of dysprosium acetate, cerium acetate and mercaptoethanol are dissolved in deionized water to obtain a mixed solution of a certain molar ratio of Ce (cerium) and In (indium), and the temperature of a circulating water bath is set to obtain In2S3:Ce material. The In2S3:Ce material is then washed with anhydrous ethanol, and the sample precipitate is washed with deionized water. The upper clear liquid is poured out and dried in an oven, and finally placed in a muffle furnace for high-temperature calcination to generate oxides. After annealing, In2O3:Ce nanoparticles are obtained. Step (2) Preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl4 (silicon tetrachloride) and anhydrous C2H5OH (anhydrous ethanol) are added into a reactor in a certain mass ratio, and then the In2O3:Ce nanoparticles in step (1) are added, reacted together, heated, and reacted for a period of time to obtain rare earth element doped tetraethyl orthosilicate (TEOS); Step (3) Preparation of polyvinyl pyrrolidone (PVP) solution Dissolve the rare earth element-doped tetraethyl orthosilicate (TEOS) in anhydrous ethanol, seal and stir, then dissolve the silane coupling agent and solid acid PTSA (catalyst) in the anhydrous ethanol, let stand, then take polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, stir magnetically, and prepare a polyvinyl pyrrolidone (PVP) solution; Step (4) Preparation of lithium niobate powder Li2CO3 (lithium carbonate) and Nb2O5 (niobium pentoxide) are weighed in a certain molar ratio. To make the niobium-lithium raw materials uniformly mixed, the polyvinyl pyrrolidone (PVP) solution of step (3) is added. A small amount of niobium-lithium raw materials are weighed and poured into a ball mill. Deionized water and zirconium oxide ball milling beads are added. The mixed wet materials are placed in a blast drying oven for drying. After being sieved through a large mesh sieve, a lithium niobate precursor is prepared. The sieved materials are placed in a corundum crucible for heating to obtain lithium niobate powder. Step (5) Preparation of nano-anion lithium niobate powder After the lithium niobate powder in step (4) is passed through a large mesh sieve, the prepared PVA (polyvinyl alcohol) solution is added for granulation. After the granulated powder is passed through a large mesh sieve, a certain amount of granulated lithium niobate powder is weighed for each piece, and a metal mold with a smaller diameter is used to press the pieces under a certain pressure to form lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold, and then the mold is placed in an oil bath polarization device for voltage polarization. After cooling, nano negative ion lithium niobate powder is obtained.

[0008] The first technical purpose of the present invention is achieved through the following technical solutions: Preferably, step (1) preparation of In2O3:Ce nanoparticles First, 5-15 g of dysprosium acetate, 10-20 g of cerium acetate and 2-10 g of mercaptoethanol are dissolved in deionized water to obtain a mixed solution with a molar ratio of Ce (cerium) to In (indium) of 0.02:0.6, the temperature of the circulating water bath is set to 40-60°C to obtain In2S3:Ce material, and then the In2S3:Ce material is washed with anhydrous ethanol for 1-5 times, and then the sample is washed with deionized water for 3-8 times, and centrifuged at a speed of 10000-50000 revolutions per minute for 1-5 minutes, the supernatant is poured out, and dried in an oven at 60-80°C, and finally placed in a muffle furnace for high-temperature calcination to generate oxides at a temperature of 5-600°C. After annealing for 3-8 hours, In2O3:Ce nanoparticles are obtained.

[0009] The advantage of adopting the present invention is that the obtained In2O3:Ce nanoparticles have good dispersibility and uniform particle size distribution, and the In2O3:Ce nanoparticles are enhanced.

[0010] The second technical purpose of the present invention is achieved through the following technical solutions: Preferably, step (2) preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl4 (silicon tetrachloride) and anhydrous C2H5OH (anhydrous ethanol) are added into a reactor at a mass ratio of 1-5:1-5, and then 5-10 g of In2O3:Ce nanoparticles from step (1) are added, and the mixture is reacted at 10-15°C, and the temperature is raised to 30-40°C, and the reaction is carried out for 2-5 hours to obtain rare earth element doped tetraethyl orthosilicate (TEOS).

[0011] The advantage of the present invention is that by directly adding In2O3:Ce nanoparticles into the reaction system of SiCl4 and anhydrous ethanol, the rare earth element (Ce) can be evenly distributed in the formed tetraethyl orthosilicate structure, which is beneficial to improving the performance consistency of the final material.

[0012] Step (3) Preparation of polyvinyl pyrrolidone (PVP) solution Dissolve 10-20 g of rare earth element-doped tetraethyl orthosilicate (TEOS) in 100-300 ml of anhydrous ethanol, seal and stir for 30-50 min, then dissolve 1-5 g of silane coupling agent and 0.1-0.5 g of solid acid PTSA (catalyst) in the anhydrous ethanol, let stand for 40-60 h, then take 1-5 g of polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, stir magnetically for 30-60 min, and prepare a polyvinyl pyrrolidone (PVP) solution.

[0013] The present invention has the advantage that by dissolving TEOS containing rare earth elements in anhydrous ethanol and adding polyvinylpyrrolidone (PVP), aggregation of nanoparticles can be effectively prevented, thereby improving the dispersion stability of nanoparticles in the solution.

[0014] Step (4) Preparation of lithium niobate powder The required raw material mass is weighed in a molar ratio of Li2CO3 (lithium carbonate) and Nb2O5 (niobium pentoxide) of 1-5:1-5. In order to make the niobium-lithium raw materials evenly mixed, the polyvinyl pyrrolidone (PVP) solution of step (3) is added. 1-5 g of the niobium-lithium raw materials are weighed and poured into a ball mill. Deionized water and zirconium oxide ball milling beads are added, wherein the mass ratio of the raw materials, ball milling beads and water added is 1-5 g:1.5-6 g:0.1-0.9 g. The ball milling is carried out for 5-10 hours. The mixed wet material is placed in a forced air drying oven at 80-100° C. and dried for 24-48 hours. After passing through a 100-200 mesh sieve, a lithium niobate precursor is prepared. The sieved material is placed in a corundum crucible and stopped at 600-700° C. to obtain lithium niobate powder.

[0015] The advantage of adopting the present invention is that during the ball milling process, the high-intensity mechanical action of the zirconium oxide ball milling beads can not only accelerate the physical crushing of the raw materials, but also increase the contact area between the raw materials, promote the chemical reaction between Li2CO3 (lithium carbonate) and Nb2O5 (niobium pentoxide), ensure that the formation of lithium niobate is more complete, and reduce the residual unreacted products.

[0016] Step (5) Preparation of nano-anion lithium niobate powder After the lithium niobate powder in step (4) is passed through a 100-200 mesh sieve, a prepared 5-10 (wt)% PVA (polyvinyl alcohol) solution is added for granulation, and 1-10 ml of the PVA (polyvinyl alcohol) solution is added. After the granulated powder is passed through an 80-100 mesh sieve, 2-8 g of the granulated lithium niobate powder is weighed per piece, and a metal mold with a diameter of 20-50 mm is used to press the tablets at a pressure of 30-60 MPa to form lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold, and then the mold is placed in an oil bath polarization device for voltage polarization, and after cooling, nano negative ion lithium niobate powder is obtained.

[0017] The invention has the advantage that, through fine screening and granulation of PVA (polyvinyl alcohol) solution, not only the uniform particle size distribution of the powder is ensured, but also PVA (polyvinyl alcohol) as a binder helps to form a compact and uniform particle structure.

[0018] In summary, the present invention has the following beneficial effects: 1. The advantage of the present invention is that the obtained In2O3:Ce nanoparticles have good dispersibility and uniform particle size distribution, and the In2O3:Ce nanoparticles are enhanced.

[0019] 2. The advantage of the present invention is that by directly adding In2O3:Ce nanoparticles into the reaction system of SiCl4 and anhydrous ethanol, the rare earth element (Ce) can be evenly distributed in the formed ethyl orthosilicate structure, which is beneficial to improving the performance consistency of the final material.

[0020] 3. The present invention has the advantage that by dissolving TEOS containing rare earth elements in anhydrous ethanol and adding polyvinylpyrrolidone (PVP), the aggregation of nanoparticles can be effectively prevented and the dispersion stability thereof in the solution can be improved.

[0021] 4. The advantage of the present invention is that during the ball milling process, the high-intensity mechanical action of the zirconium oxide ball milling beads can not only accelerate the physical crushing of the raw materials, but also increase the contact area between the raw materials, promote the chemical reaction between Li2CO3 (lithium carbonate) and Nb2O5 (niobium pentoxide), ensure that the formation of lithium niobate is more complete, and reduce the residual unreacted products.

[0022] 5. The present invention has the advantage that, through fine screening and granulation of PVA (polyvinyl alcohol) solution, not only the particle size distribution of the powder is ensured to be uniform, but also PVA (polyvinyl alcohol) as a binder helps to form a compact and uniform particle structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A flow chart of a method for preparing a nanometer negative ion releasing material containing rare earth elements. DETAILED DESCRIPTION

[0024] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Without departing from the spirit and substance of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention are within the scope of the present invention.

[0025] If not specifically stated, the technical means used in the examples are conventional means known to those skilled in the art. In addition, all the raw materials used in the examples are known commercial products.

[0026] Example 1 Step (1) Preparation of In2O3:Ce nanoparticles First, 5 g of dysprosium acetate, 10 g of cerium acetate and 2 g of mercaptoethanol were dissolved in deionized water to obtain a mixed solution with a molar ratio of Ce (cerium) to In (indium) of 0.02:0.2. The temperature of the circulating water bath was set to 40°C to obtain In2S3:Ce material. The In2S3:Ce material was then washed once with anhydrous ethanol, and the sample was washed with deionized water for 3 times. The sample was centrifuged at 10,000 rpm for 1 minute, the supernatant was poured out, and dried in an oven at 60°C. Finally, the sample was placed in a muffle furnace and calcined at a high temperature of 5°C to generate oxides. After annealing for 3 hours, In2O3:Ce nanoparticles were obtained. Step (2) Preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl4 (silicon tetrachloride) and anhydrous C2H5OH (anhydrous ethanol) are added into the reactor in a mass ratio of 1:1, and then 5 g of In2O3:Ce nanoparticles from step (1) are added, and the mixture is reacted at 10°C, and the temperature is raised to 30°C and the reaction is continued for 2 hours to obtain rare earth element doped tetraethyl orthosilicate (TEOS); Step (3) Preparation of polyvinyl pyrrolidone (PVP) solution Dissolve 10g of rare earth element-doped tetraethyl orthosilicate (TEOS) prepared in step (2) in 100ml of anhydrous ethanol, and stir for 30min in a sealed container. Then, dissolve 1g of silane coupling agent and 0.1g of solid acid PTSA (catalyst) in the anhydrous ethanol, and let stand for 40h. Then, take 1g of polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, and stir magnetically for 30min to prepare a polyvinyl pyrrolidone (PVP) solution. Step (4) Preparation of lithium niobate powder Li2CO3 (lithium carbonate) and Nb2O5 (niobium pentoxide) are weighed in a molar ratio of 1:1. In order to make the niobium-lithium raw materials evenly mixed, the polyvinyl pyrrolidone (PVP) solution of step (3) is added. 1g of the niobium-lithium raw materials is weighed and poured into a ball mill. Deionized water and zirconium oxide ball milling beads are added, wherein the mass ratio of the raw materials, ball milling beads and water is 1g:1.5g:0.1g. The ball milling is carried out for 5 hours. The mixed wet material is placed in a blast drying oven at 80°C and dried for 24 hours. After passing through a 100-mesh sieve, a lithium niobate precursor is prepared. The sieved material is placed in a corundum crucible and the temperature is stopped at 600°C to obtain lithium niobate powder. Step (5) Preparation of nano-anion lithium niobate powder After the lithium niobate powder in step (4) is passed through a 100-mesh sieve, a prepared 5 (wt)% PVA (polyvinyl alcohol) solution is added for granulation. After 1 ml of the PVA (polyvinyl alcohol) solution is added, the granulated powder is passed through an 80-mesh sieve, and 2 g of the granulated lithium niobate powder is weighed per piece. A metal mold with a diameter of 20 mm is used and the tablets are pressed at a pressure of 30 MPa to form lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold. The mold is then placed in an oil bath polarization device for voltage polarization. After cooling, nano negative ion lithium niobate powder is obtained.

[0027] Example 2 Step (1) Preparation of In2O3:Ce nanoparticles First, 8 g of dysprosium acetate, 12 g of cerium acetate and 4 g of mercaptoethanol were dissolved in deionized water to obtain a mixed solution with a molar ratio of Ce (cerium) to In (indium) of 0.04:0.3, and the temperature of the circulating water bath was set to 45°C to obtain In2S3:Ce material. The In2S3:Ce material was then washed twice with anhydrous ethanol, and the sample was washed with deionized water for 4 times. The sample was centrifuged at 20,000 rpm for 2 minutes, the supernatant was poured out, and dried in an oven at 65°C. Finally, it was placed in a muffle furnace and calcined at a high temperature of 150°C to generate oxides. After annealing for 4 hours, In2O3:Ce nanoparticles were obtained. Step (2) Preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl4 (silicon tetrachloride) and anhydrous C2H5OH (anhydrous ethanol) are added into the reactor in a mass ratio of 2:2, and then 6 g of In2O3:Ce nanoparticles from step (1) are added, and the mixture is reacted together at 12°C, and the temperature is raised to 32°C, and the reaction is carried out for 2.5 hours to obtain rare earth element doped tetraethyl orthosilicate (TEOS); Step (3) Preparation of polyvinyl pyrrolidone (PVP) solution Dissolve 12g of rare earth element-doped tetraethyl orthosilicate (TEOS) prepared in step (2) in 150ml of anhydrous ethanol, and stir in a sealed container for 35min. Then, dissolve 2g of silane coupling agent and 0.2g of solid acid PTSA (catalyst) in the anhydrous ethanol, and let stand for 42h. Then, take 2g of polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, and stir under magnetic stirring for 35min to prepare a polyvinyl pyrrolidone (PVP) solution. Step (4) Preparation of lithium niobate powder Li2CO3 (lithium carbonate) and Nb2O5 (niobium pentoxide) are weighed in a molar ratio of 2:2. To ensure that the niobium-lithium raw materials are evenly mixed, the polyvinyl pyrrolidone (PVP) solution of step (3) is added. 2 g of the niobium-lithium raw materials are weighed and poured into a ball mill. Deionized water and zirconium oxide ball milling beads are added, wherein the mass ratio of the raw materials, ball milling beads, and water is 2g:2g:0.4g. The ball milling is performed for 6 hours. The mixed wet materials are placed in a forced air drying oven at 85°C and dried for 30 hours. After being sieved through a 120-mesh sieve, a lithium niobate precursor is prepared. The sieved materials are placed in a corundum crucible and the temperature is stopped at 650°C to obtain lithium niobate powder. Step (5) Preparation of nano-anion lithium niobate powder After the lithium niobate powder in step (4) is passed through a 120-mesh sieve, a prepared 6 (wt)% PVA (polyvinyl alcohol) solution is added for granulation. After 2 ml of the PVA (polyvinyl alcohol) solution is added, the granulated powder is passed through an 85-mesh sieve, and 4 g of the granulated lithium niobate powder is weighed per piece. A metal mold with a diameter of 25 mm is used and tablets are pressed at a pressure of 40 MPa to form lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold. The mold is then placed in an oil bath polarization device for voltage polarization. After cooling, nano negative ion lithium niobate powder is obtained.

[0028] Example 3 Step (1) Preparation of In2O3:Ce nanoparticles First, 10 g of dysprosium acetate, 15 g of cerium acetate and 6 g of mercaptoethanol were dissolved in deionized water to obtain a mixed solution with a molar ratio of Ce (cerium) to In (indium) of 0.05:0.4, and the temperature of the circulating water bath was set to 50 ° C to obtain In2S3:Ce material. The In2S3:Ce material was then washed with anhydrous ethanol for 3 times, and the sample was washed with deionized water for 5 times. The sample was centrifuged at 30,000 revolutions per minute for 3 minutes, the supernatant was poured out, and dried in an oven at 70 ° C. Finally, it was placed in a muffle furnace for high-temperature calcination to generate oxides at a temperature of 300 ° C. After annealing for 5 hours, In2O3:Ce nanoparticles were obtained. Step (2) Preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl4 (silicon tetrachloride) and anhydrous C2H5OH (anhydrous ethanol) are added into the reactor in a mass ratio of 3:3, and then 7 g of In2O3:Ce nanoparticles from step (1) are added, and the mixture is reacted at 13°C, and the temperature is raised to 35°C and the reaction is continued for 3 hours to obtain rare earth element doped tetraethyl orthosilicate (TEOS); Step (3) Preparation of polyvinyl pyrrolidone (PVP) solution Dissolve 15g of rare earth element-doped tetraethyl orthosilicate (TEOS) prepared in step (2) in 200ml of anhydrous ethanol, and stir in a sealed container for 40min. Then, dissolve 3g of silane coupling agent and 0.3g of solid acid PTSA (catalyst) in the anhydrous ethanol, and let stand for 50h. Then, take 3g of polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, and stir magnetically for 40min to prepare a polyvinyl pyrrolidone (PVP) solution. Step (4) Preparation of lithium niobate powder The required raw materials of Li2CO3 (lithium carbonate) and Nb2O5 (niobium pentoxide) are weighed in a molar ratio of 3:3. In order to make the niobium-lithium raw materials evenly mixed, the polyvinyl pyrrolidone (PVP) solution of step (3) is added. 3 g of the niobium-lithium raw materials are weighed and poured into a ball mill. Deionized water and zirconium oxide ball milling beads are added, wherein the mass ratio of the raw materials, ball milling beads and water is 3g:3g:0.6g. The ball milling is carried out for 7 hours. The mixed wet materials are placed in a blast drying oven at 90°C and dried for 35 hours. After passing through a 150-mesh sieve, a lithium niobate precursor is prepared. The sieved materials are placed in a corundum crucible and stopped at 670°C to obtain lithium niobate powder. Step (5) Preparation of nano-anion lithium niobate powder After the lithium niobate powder in step (4) is passed through a 130-mesh sieve, a prepared 7 (wt)% PVA (polyvinyl alcohol) solution is added for granulation. After 5 ml of the PVA (polyvinyl alcohol) solution is added, the granulated powder is passed through a 90-mesh sieve, and 6 g of the granulated lithium niobate powder is weighed per piece. A metal mold with a diameter of 30 mm is used and tablets are pressed at a pressure of 50 MPa to form lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold. The mold is then placed in an oil bath polarization device for voltage polarization. After cooling, nano negative ion lithium niobate powder is obtained.

[0029] Example 4 Step (1) Preparation of In2O3:Ce nanoparticles First, 14 g of dysprosium acetate, 17 g of cerium acetate and 8 g of mercaptoethanol were dissolved in deionized water to obtain a mixed solution with a molar ratio of Ce (cerium) to In (indium) of 0.08:0.5, and the temperature of the circulating water bath was set to 55°C to obtain In2S3:Ce material. The In2S3:Ce material was then washed with anhydrous ethanol for 4 times, and the sample was washed with deionized water for 6 times. The sample was centrifuged at 40,000 revolutions per minute for 5 minutes, the supernatant was poured out, and dried in an oven at 75°C. Finally, the sample was placed in a muffle furnace and calcined at a high temperature of 500°C to generate oxides. After annealing for 8 hours, In2O3:Ce nanoparticles were obtained. Step (2) Preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl4 (silicon tetrachloride) and anhydrous C2H5OH (anhydrous ethanol) are added into a reactor at a mass ratio of 4:4, and then 8 g of In2O3:Ce nanoparticles from step (1) are added, and the mixture is reacted together at 15°C, and the temperature is raised to 40°C and the reaction is carried out for 5 hours to obtain rare earth element doped tetraethyl orthosilicate (TEOS); Step (3) Preparation of polyvinyl pyrrolidone (PVP) solution Dissolve 18g of rare earth element-doped tetraethyl orthosilicate (TEOS) prepared in step (2) in 300ml of anhydrous ethanol, and stir in a sealed container for 45min. Then, dissolve 4g of silane coupling agent and 0.4g of solid acid PTSA (catalyst) in the anhydrous ethanol, and let stand for 55h. Then, take 4g of polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, and stir magnetically for 50min to prepare a polyvinyl pyrrolidone (PVP) solution. Step (4) Preparation of lithium niobate powder The required raw materials of Li2CO3 (lithium carbonate) and Nb2O5 (niobium pentoxide) are weighed in a molar ratio of 4:4. In order to make the niobium-lithium raw materials evenly mixed, the polyvinyl pyrrolidone (PVP) solution of step (3) is added. 4 g of the niobium-lithium raw materials are weighed and poured into a ball mill. Deionized water and zirconium oxide ball milling beads are added, wherein the mass ratio of the raw materials, ball milling beads and water is 5g:6g:0.9g. The ball milling is carried out for 9 hours. The mixed wet materials are placed in a blast drying oven at 95°C and dried for 48 hours. After passing through a 170-mesh sieve, a lithium niobate precursor is prepared. The sieved materials are placed in a corundum crucible and the temperature is stopped at 700°C to obtain lithium niobate powder. Step (5) Preparation of nano-anion lithium niobate powder After the lithium niobate powder in step (4) is passed through a 180-mesh sieve, the prepared 8 (wt)% PVA (polyvinyl alcohol) solution is added for granulation. 8 ml of the PVA (polyvinyl alcohol) solution is added, and the granulated powder is passed through a 100-mesh sieve. The granulated lithium niobate powder is weighed at 8 g per piece, and a metal mold with a diameter of 50 mm is used to press the tablets at a pressure of 60 MPa to prepare lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold. The mold is then placed in an oil bath polarization device for voltage polarization. After cooling, nano negative ion lithium niobate powder is obtained.

[0030] Comparative Example 1 Step (1) Preparation of In2O3:Ce nanoparticles First, 17 g of dysprosium acetate, 19 g of cerium acetate and 9 g of mercaptoethanol were dissolved in deionized water to obtain a mixed solution with a molar ratio of Ce (cerium) to In (indium) of 0.09:0.2, and the temperature of the circulating water bath was set to 60°C to obtain In2S3:Ce material. The In2S3:Ce material was then washed with anhydrous ethanol for 6 times, and the sample was washed with deionized water for 7 times. The sample was centrifuged at 50,000 revolutions per minute for 8 minutes, the supernatant was poured out, and dried in an oven at 80°C. Finally, the sample was placed in a muffle furnace and calcined at a high temperature of 600°C to generate oxides. After annealing for 9 hours, In2O3:Ce nanoparticles were obtained. Step (2) Preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl4 (silicon tetrachloride) and anhydrous C2H5OH (anhydrous ethanol) are added into a reactor at a mass ratio of 6:8, and then 9 g of In2O3:Ce nanoparticles from step (1) are added, and the mixture is reacted together at 20°C, and the temperature is raised to 45°C and the reaction is carried out for 6 hours to obtain rare earth element doped tetraethyl orthosilicate (TEOS); Step (3) Preparation of polyvinyl pyrrolidone (PVP) solution Dissolve 19g of rare earth element-doped tetraethyl orthosilicate (TEOS) prepared in step (2) in 350ml of anhydrous ethanol, and stir in a sealed container for 50min. Then, dissolve 5g of silane coupling agent and 0.5g of solid acid PTSA (catalyst) in the anhydrous ethanol, and let stand for 60h. Then, take 5g of polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, and stir under magnetic stirring for 55min to prepare a polyvinyl pyrrolidone (PVP) solution. Step (4) Preparation of nano-anion lithium niobate powder After the lithium niobate powder is passed through a 180-mesh sieve, the prepared 8 wt% PVA (polyvinyl alcohol) solution is added for granulation, 8 ml of the PVA (polyvinyl alcohol) solution is added, and then 10 ml of the polyvinyl pyrrolidone (PVP) solution of step (3) is added. After the granulated powder is passed through a 100-mesh sieve, 8 g of the granulated lithium niobate powder is weighed per piece, and a metal mold with a diameter of 50 mm is used to press the tablets at a pressure of 60 MPa to form lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold. The mold is then placed in an oil bath polarization device for voltage polarization. After cooling, nano negative ion lithium niobate powder is obtained.

[0031] Comparative Example 2 Step (1) Preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl4 (silicon tetrachloride) and anhydrous C2H5OH (anhydrous ethanol) were added into the reactor at a mass ratio of 6:4, and then 9g of In2O3:Ce nanoparticles were added, and the mixture was reacted at 20°C, and the temperature was raised to 50°C and the reaction was continued for 6h to obtain rare earth element doped tetraethyl orthosilicate (TEOS); Step (2) Preparation of polyvinylpyrrolidone (PVP) solution Dissolve 20g of rare earth element-doped tetraethyl orthosilicate (TEOS) prepared in step (1) in 390ml of anhydrous ethanol, and stir in a sealed container for 50min. Then, dissolve 8g of silane coupling agent and 0.9g of solid acid PTSA (catalyst) in the anhydrous ethanol, and let stand for 60h. Then, take 1g of polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, and stir under magnetic stirring for 60min to prepare a polyvinyl pyrrolidone (PVP) solution. Step (3) Preparation of lithium niobate powder The required raw materials of Li2CO3 (lithium carbonate) and Nb2O5 (niobium pentoxide) are weighed in a molar ratio of 6:3. In order to make the niobium-lithium raw materials evenly mixed, the polyvinyl pyrrolidone (PVP) solution of step (2) is added. 5 g of the niobium-lithium raw materials are weighed and poured into a ball mill. Deionized water and zirconium oxide ball milling beads are added, wherein the mass ratio of the raw materials, ball milling beads and water added is 6g:7g:1g. The ball milling is carried out for 10 hours. The mixed wet materials are placed in a blast drying oven at 100° C. and dried for 50 hours. After passing through a 190-mesh sieve, a lithium niobate precursor is prepared. The sieved materials are placed in a corundum crucible and stopped at 800° C. to obtain lithium niobate powder. Step (4) Preparation of nano-anion lithium niobate powder After the lithium niobate powder in step (3) is passed through a 200-mesh sieve, a prepared 9 (wt)% PVA (polyvinyl alcohol) solution is added for granulation. After 10 ml of the PVA (polyvinyl alcohol) solution is added, the granulated powder is passed through a 200-mesh sieve, and 10 g of the granulated lithium niobate powder is weighed per piece. A metal mold with a diameter of 60 mm is used and the tablets are pressed at a pressure of 70 MPa to form lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold. The mold is then placed in an oil bath polarization device for voltage polarization. After cooling, nano negative ion lithium niobate powder is obtained.

[0032] The nanometer negative ion releasing materials containing rare earth elements obtained in Examples 1 to 4 and Comparative Example Products 1 and 2 were tested, and the specific testing method is as follows: Negative ion release performance test method In order to test the negative ion release performance of nano negative ion releasing materials containing rare earth elements, the amount of negative ions released after polarization is more, and vice versa. The more negative ion release amount indicates that polarization has endowed the nano negative ion releasing materials containing rare earth elements with negative ion release performance. This time, polarized and unpolarized nano negative ion releasing materials containing rare earth elements were used for comparison to measure the negative ion release amounts of the two.

[0033] PL spectroscopy test method The photoluminescence property test method of nanoparticles is used to analyze the luminescence efficiency of indium oxide (In2O3) nanoparticles in nano-anion releasing materials containing rare earth elements when they are excited by light. A high luminescence efficiency value indicates that the luminescence efficiency of the nano-anion releasing materials containing rare earth elements is good, otherwise it is poor.

[0034] Table 1 Negative ion release performance test results

[0035] Table 2 Negative ion release performance test results

[0036] Combining Table 1 and Table 2, it can be seen that Example 1 in Table 1 is the best, and Comparative Example 1 in Table 2 is the worst. Example 1 in Table 1 performs best because it can release the most negative ions after polarization treatment, which shows that the rare earth elements contained in Example 1 in Table 1 optimize the performance of the nano negative ion releasing material, so that it can effectively release negative ions into the surrounding environment. The high negative ion release has certain benefits in air purification, improving living comfort, and being beneficial to human health.

[0037] Table 3 PL spectrum test results

[0038] As can be seen from Table 3, Example 1 is the best and Comparative Example 2 is the worst. The wavelength in Example 1 is 500 nm, which means there is a luminescence peak. In the photoluminescent material of the nano-anion releasing material containing rare earth elements, the longer wavelength is related to the fluorescence quantum yield of the nano-anion releasing material, indicating that the nano-anion releasing material containing rare earth elements in Example 1 has a better energy level structure, fewer defects and more efficient energy conversion.

[0039] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art can make non-creative modifications to the present embodiment as needed, but they are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A method for preparing a nanometer negative ion releasing material containing rare earth elements, It is characterized in that Includes: 2 O 3 : Preparation of Ce nanoparticles, preparation of rare earth element doped tetraethyl orthosilicate (TEOS), preparation of polyvinyl pyrrolidone (PVP) solution, preparation of lithium niobate powder, preparation of nano negative ion lithium niobate powder.

2. The method for preparing the rare earth element-containing nanometer negative ion releasing material according to claim 1, Features : Step (1) In 2 O 3 Preparation of Ce nanoparticles First, a small amount of dysprosium acetate, cerium acetate and mercaptoethanol were dissolved in deionized water to obtain a mixed solution of Ce (cerium) and In (indium) in a certain molar ratio. The temperature of the circulating water bath was set to obtain In 2 S 3 :Ce material, then clean In with anhydrous ethanol 2 S 3 :Ce material, then use deionized water to wash the sample precipitate, pour out the supernatant, dry it in an oven, and finally calcine it at high temperature in a muffle furnace to generate oxide. After annealing, In 2 O 3 :Ce nanoparticles; Step (2) Preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl 4 (Silicon tetrachloride) and anhydrous C 2 H 5 OH (anhydrous ethanol) is added to the reactor at a certain mass ratio, and then In 2 O 3 : Ce nanoparticles, react together, heat up, react for a period of time, and obtain rare earth element doped tetraethyl orthosilicate (TEOS); Step (3) Preparation of polyvinyl pyrrolidone (PVP) solution Dissolve the rare earth element-doped tetraethyl orthosilicate (TEOS) in anhydrous ethanol, seal and stir, then dissolve the silane coupling agent and solid acid PTSA (catalyst) in the anhydrous ethanol, let stand, then take polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, stir magnetically, and prepare a polyvinyl pyrrolidone (PVP) solution; Step (4) Preparation of lithium niobate powder Li 2 CO 3 (Lithium carbonate) and Nb 2 O 5 (Niobium pentoxide) The required raw material mass is weighed according to a certain molar ratio. In order to make the niobium and lithium raw materials evenly mixed, the polyvinyl pyrrolidone (PVP) solution of step (3) is added. A small amount of niobium and lithium raw materials is weighed and poured into a ball mill. Deionized water and zirconium oxide ball milling beads are added. The mixed wet materials are placed in a blast drying oven for drying. After passing through a large mesh sieve, a lithium niobate precursor is prepared. The sieved materials are placed in a corundum crucible and heated to obtain lithium niobate powder. Step (5) Preparation of nano-anion lithium niobate powder After the lithium niobate powder in step (4) is passed through a large mesh sieve, the prepared PVA (polyvinyl alcohol) solution is added for granulation. After the granulated powder is passed through a large mesh sieve, a certain amount of granulated lithium niobate powder is weighed for each piece, and a metal mold with a smaller diameter is used to press the pieces under a certain pressure to form lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold, and then the mold is placed in an oil bath polarization device for voltage polarization. After cooling, nano negative ion lithium niobate powder is obtained.

3. The method for preparing the rare earth element-containing nanometer negative ion releasing material according to claim 2, Features : Step (1) In 2 O 3 Preparation of Ce nanoparticles First, 5-15 g of dysprosium acetate, 10-20 g of cerium acetate and 2-10 g of mercaptoethanol were dissolved in deionized water to obtain a mixed solution with a molar ratio of Ce (cerium) to In (indium) of 0.02:0.

6. The temperature of the circulating water bath was set to 40-60 ° C to obtain In 2 S 3 :Ce material, then clean In with anhydrous ethanol 2 S 3 :Ce material 1-5 times, then use deionized water to wash the sample precipitation 3-8 times, centrifuge at a speed of 10000-50000 revolutions per minute for 1-5 minutes, pour out the supernatant, dry in an oven at 60-80℃, and finally calcine in a muffle furnace at high temperature to generate oxides at a temperature of 5-600℃. After annealing for 3-8 hours, In 2 O 3 :Ce nanoparticles.

4. The method for preparing the rare earth element-containing nanometer negative ion releasing material according to claim 3, Features : Step (2) Preparation of rare earth element doped tetraethyl orthosilicate (TEOS) SiCl 4 (Silicon tetrachloride) and anhydrous C 2 H 5 OH (anhydrous ethanol) is added to the reactor at a mass ratio of 1-5:1-5, and then 5-10g of In step (1) is added. 2 O 3 :Ce nanoparticles, react together at 10-15°C, heat to 30-40°C, react for 2-5h, and obtain rare earth element doped tetraethyl orthosilicate (TEOS).

5. The method for preparing the rare earth element-containing nanometer negative ion releasing material according to claim 4, Features : Step (3) Preparation of polyvinyl pyrrolidone (PVP) solution Dissolve 10-20 g of rare earth element-doped tetraethyl orthosilicate (TEOS) in 100-300 ml of anhydrous ethanol, seal and stir for 30-50 min, then dissolve 1-5 g of silane coupling agent and 0.1-0.5 g of solid acid PTSA (catalyst) in the anhydrous ethanol, let stand for 40-60 h, then take 1-5 g of polyvinyl pyrrolidone (PVP) and dissolve it in the anhydrous ethanol, stir magnetically for 30-60 min, and prepare a polyvinyl pyrrolidone (PVP) solution.

6. The method for preparing the rare earth element-containing nanometer negative ion releasing material according to claim 5, Features : Step (4) Preparation of lithium niobate powder Li 2 CO 3 (Lithium carbonate) and Nb 2 O 5 The required raw materials are weighed in a molar ratio of 1-5:1-5. In order to make the niobium and lithium raw materials evenly mixed, the polyvinyl pyrrolidone (PVP) solution of step (3) is added. 1-5 g of the niobium and lithium raw materials are weighed and poured into a ball mill. Deionized water and zirconium oxide ball milling beads are added, wherein the mass ratio of the raw materials, ball milling beads and water is 1-5 g:1.5-6 g:0.1-0.9 g. The ball milling is carried out for 5-10 hours. The mixed wet materials are placed in a forced air drying oven at 80-100° C. and dried for 24-48 hours. After being sieved through a 100-200 mesh sieve, a lithium niobate precursor is prepared. The sieved materials are placed in a corundum crucible and the temperature is stopped at 600-700° C. to obtain lithium niobate powder.

7. The method for preparing the rare earth element-containing nanometer negative ion releasing material according to claim 6, Features : Step (5) Preparation of nano-anion lithium niobate powder After the lithium niobate powder in step (4) is passed through a 100-200 mesh sieve, a prepared 5-10 (wt)% PVA (polyvinyl alcohol) solution is added for granulation, and 1-10 ml of the PVA (polyvinyl alcohol) solution is added. After the granulated powder is passed through an 80-100 mesh sieve, 2-8 g of the granulated lithium niobate powder is weighed per piece, and a metal mold with a diameter of 20-50 mm is used to press the tablets at a pressure of 30-60 MPa to form lithium niobate powder green sheets. Silicone oil is used as an insulating medium, and the pressed lithium niobate powder green sheets are placed in a polarization mold, and then the mold is placed in an oil bath polarization device for voltage polarization, and after cooling, nano negative ion lithium niobate powder is obtained.