Single-crystal positive electrode material precursor, spherical or sphere-like single-crystal positive electrode material and preparation method of spherical or sphere-like single-crystal positive electrode material

By using single-crystal cathode material precursors with specific morphologies and sintering processes, the problem of non-uniformity of single-crystal cathode material particles was solved, thereby improving the cycle stability and safety of lithium-ion batteries.

CN118993178AInactive Publication Date: 2024-11-22HENAN KELONG NEW ENERGY CO LTD

Patent Information

Application Number
CN202411482902.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing single-crystal cathode material precursors exhibit significant differences in particle size and shape after sintering, leading to uneven charging and discharging processes, material degradation, poor cycle performance, and potential safety hazards.

Method used

By using a single-crystal cathode material precursor with a specific morphology, and by controlling the primary particle cross-agglomeration and adjusting the reaction conditions, a single-crystal cathode material with high secondary particle uniformity is prepared. Combined with the sintering process of lithium source and doped additives, the consistency and sphericity of the material are ensured.

Benefits of technology

It improves the cycle stability and safety performance of lithium-ion batteries, avoids overcharging and over-discharging, and enhances the capacity utilization and high-temperature cycle performance of cathode materials under high voltage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993178A_ABST
    Figure CN118993178A_ABST
Patent Text Reader

Abstract

The invention discloses a single-crystal positive electrode material precursor, a spherical or sphere-like single-crystal positive electrode material and a preparation method thereof, the single-crystal positive electrode material precursor is a secondary particle formed by interlaced agglomeration of primary particles, the distribution of the primary particles is narrow, gaps exist among the primary particles, the thickness of the primary particles is 50-400nm, the precursor comprises an inner core and a shell, and the shell is a spherical or sphere-like single-crystal positive electrode material. The profile morphology inner core is loose, the particle size of the inner core is 0.5-1.5 [mu] m, the profile morphology outer shell is radial, and the thickness of the outer shell is 0.5-4.5 [mu] m. The single crystal positive electrode material prepared by sintering the single crystal positive electrode material precursor with the specific morphology is good in sphericity and high in consistency, and the lithium ion battery assembled by the single crystal positive electrode material is good in consistency and good in stability. And over-charging and over-discharging are avoided in the recycling process, so that the cycling stability and the safety performance of the lithium ion battery are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery positive electrode materials, and specifically relates to a single crystal positive electrode material precursor, a spherical or quasi-spherical single crystal positive electrode material and a preparation method thereof. Background Art

[0002] As the world's non-renewable resources continue to be consumed, countries are striving to find new energy sources. Lithium-ion batteries are currently a popular alternative product, and are increasingly attracting attention due to their safety, high discharge specific energy, and long charge and discharge life. The positive electrode material is the most critical part of lithium-ion batteries.

[0003] The positive electrode materials of lithium-ion batteries are divided into polycrystalline and single crystal. Polycrystalline is a spherical or quasi-spherical aggregate particle formed by multiple particles agglomerated together. Polycrystalline particles will be broken during the rolling process, and the anisotropy of the grains during the cycle will cause inconsistent expansion and contraction of the particles, which will lead to the rupture of the agglomerates, the exposure of internal particles, and the increase of side reactions after contact with the electrolyte, which will eventually affect the performance and safety of the battery. Single crystal particles just make up for this shortcoming. Single crystal materials have the characteristics of high mechanical strength. They will not cause inter-particle breakage during charging and discharging, and can effectively reduce side reactions at the interface between the material and the electrolyte. They can not only improve the capacity of the positive electrode material under high voltage, but also effectively improve the high temperature cycle difference, flatulence, and rapid capacity decay of the positive electrode material.

[0004] However, the single crystals of the existing technology, after sintering using the existing precursors, have large differences in size and shape between particles, or small particles may agglomerate, causing unevenness during the charge and discharge process. Then the material deteriorates, the cycle performance deteriorates, and the local temperature is too high, which poses a safety hazard to lithium-ion batteries.

[0005] Patent document CN 106450155B discloses a lithium nickel cobalt manganese composite oxide positive electrode material with a spherical or quasi-spherical layered structure, a preparation method and an application thereof. The primary single crystal particles and a small amount of secondary agglomerated particles are fired into spherical or quasi-spherical morphology. The patent document proposes the requirements that the material structure should meet, but does not have any special morphological requirements for the precursor for preparing the lithium nickel cobalt manganese composite oxide positive electrode material with a spherical or quasi-spherical layered structure. Patent document CN 108461748B discloses a lithium ion battery single crystal positive electrode material and a preparation method thereof. The method is to use radio frequency plasma treatment to recrystallize the crushed particles and then spheroidize the material morphology. The method of the patent document requires special processing equipment for production, and the cost is relatively high. Summary of the invention

[0006] In view of the above problems and the above patent literature technologies, all of which are improvements from the positive electrode material aspect, and none of them specify what kind of precursor is needed, the present invention has found through research that the morphology of the precursor has a great influence on the morphology of the positive electrode material, and the morphology of the precursor directly affects the sphericity of the positive electrode material after sintering. The present invention provides a single crystal positive electrode material precursor, a spherical or quasi-spherical single crystal positive electrode material and a preparation method thereof. By using a single crystal positive electrode material precursor with a specific morphology, the single crystal positive electrode material prepared after sintering has good sphericity and high consistency. The single crystal positive electrode material has good consistency after being assembled into a lithium-ion battery, and overcharge and over-discharge are avoided during cyclic use, thereby effectively improving the cycle stability and safety performance of the lithium-ion battery.

[0007] The present invention adopts the following technical solutions to solve the above technical problems: A single crystal positive electrode material precursor is a secondary particle formed by interlaced agglomeration of primary particles, and the primary particles are narrowly distributed, there are gaps between the primary particles, the thickness of the primary particles is 50-400nm, the single crystal positive electrode material precursor includes a core and a shell, the cross-sectional morphology of the core is loose, the core particle size is 0.5-1.5μm, the cross-sectional morphology of the shell is radiated, the shell thickness is 0.5-4.5μm, and the specific surface area of ​​the single crystal positive electrode material precursor is 8-20m 2 / g, tap density is 1.3~2.1g / cm 3 ; Average particle size D of secondary particles 50 The secondary particle size distribution (D 90 -D 10 ) / D 50 ≤0.8.

[0008] A method for preparing a single crystal positive electrode material precursor, the specific preparation steps of which are: Step S1, preparing a mixed salt solution of a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution, preparing a NaOH solution as a precipitant solution, and preparing an ammonia solution as a complexing agent solution; Step S2, continuously introducing nitrogen and oxygen into a sealed reactor, wherein the volume flow ratio of nitrogen to oxygen is 9-99:1, and then adding a precipitant solution and a complexing agent solution to prepare a base solution, controlling the pH value of the mixed system to be 10-12, the ammonia concentration to be 3-6 mol / L, and stirring at a speed of 300-600 r / min, and setting the temperature of the reactor to 50-70° C.; Step S3, adding a mixed salt solution into the reactor at a feed rate of 0.06-0.14 L / min to perform a nucleation reaction, and stopping the nucleation reaction when the crystal nucleus particle size grows to 0.5-1.5 μm; Step S4, adjusting the nitrogen gas to be introduced, and adjusting the feed rate of the mixed salt solution to be less than the feed rate of the mixed salt solution in step S3 before the adjustment, adjusting the pH value of the mixed system to be less than the pH value in step S2 before the adjustment, and adjusting the ammonia concentration to be greater than the ammonia concentration in step S2 before the adjustment, and performing a particle growth reaction, and stopping the reaction when the particle size grows to 2-5 μm; Step S5, dehydrating the particles by centrifuge and sequentially adding alkaline solution and pure water to remove impurities, and then drying the dehydrated material, and then sieving to obtain a single crystal positive electrode material precursor.

[0009] Furthermore, in step S1, the total concentration of the mixed salt solution is 2 mol / L, the concentration of the precipitant solution is 4 mol / L, and the concentration of the complexing agent solution is 9-12 mol / L.

[0010] A spherical or quasi-spherical single crystal positive electrode material, the single crystal positive electrode material is a single crystal spherical or quasi-spherical particle, the ratio of the long side length to the short side length of the single crystal positive electrode material is less than 1.5, and the average particle size D of the secondary sintered particles is 50 / The short side length of the once sintered particles is ≤2; the positive electrode material is made using the precursor with the above specific morphology.

[0011] A method for preparing a spherical or quasi-spherical single crystal positive electrode material, the specific preparation steps of which are: Step S1, mixing the single crystal positive electrode material precursor prepared above with a lithium source, a doping additive and a flux, sintering at 800-1000° C. for 8-16 hours, and crushing and grinding after cooling to obtain a primary sintered particle positive electrode material intermediate; Step S2, coating the cathode material intermediate and the coating agent evenly in a coating device, sintering at 300-600° C. for 8-16 hours, cooling and sieving to obtain a secondary sintered granular cathode material.

[0012] Furthermore, in step S1, the molar ratio of the single crystal positive electrode material precursor to the lithium source is 1:0.9-1.07.

[0013] Furthermore, the doping additive in step S1 is one or more compounds containing Ti, Zr, Mg, Ca, Sr, Ba, W, Nb, Mo, B, and Al, and the amount of the doping additive is 0.1wt%~0.5wt% of the total weight of the precursor and the lithium source; the flux is one or more compounds containing B, Li, and Ba, and the amount of the flux is 0.1wt%~0.3wt% of the total weight of the precursor and the lithium source.

[0014] Furthermore, the coating agent in step S2 is one or more compounds containing Al, B, Ti, Zr, W, and Co, and the amount of the coating agent is 0.05wt%~2wt% of the weight of the positive electrode material intermediate.

[0015] Compared with the prior art, the present invention has the following advantages and beneficial effects: the single crystal positive electrode material prepared by the present invention using a precursor with a specific morphology has good sphericity and high consistency. The prepared single crystal positive electrode material has good consistency after being assembled into a lithium ion battery, and overcharge and over-discharge can be avoided during the cyclic use process, thereby effectively improving the cycle stability and safety performance of the lithium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a scanning electron microscope image of the precursor in Example 1.

[0017] Figure 2 This is a thickness measurement diagram of the precursor of Example 1.

[0018] Figure 3 This is a cross-sectional view of the precursor in Example 1.

[0019] Figure 4 This is a scanning electron microscope image of the positive electrode material in Example 1.

[0020] Figure 5 This is a measurement diagram of the short side of the primary particles of the positive electrode material in Example 1.

[0021] Figure 6 This is a measurement diagram of the long side of the primary particles of the positive electrode material in Example 1. DETAILED DESCRIPTION

[0022] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.

[0023] The present invention adopts the following test method: 1) Precursor primary particle thickness: After taking a picture of the precursor using a sigma500 field emission electron microscope, the thickness of the precursor was tested using Nano Measurer software. The average thickness of 30 to 50 primary particles was taken as the thickness of the precursor primary particles. 2) Secondary particles D 10 , D 50 , D 90 :Use Malvern laser particle size analyzer (model: Mastersizer 3000) to detect the particle size of the precursor and cathode material; 3) Long and short sides of primary particles: After taking photos of the positive electrode material using a Hitachi tungsten filament scanning electron microscope (model: Hitachi 3400N), the long or short sides of a single particle of the positive electrode material were detected using Nano Measurer software, and the average value of 120-140 primary particles was detected; 4) Average particle size D of primary particles 50 : In the present invention, it is the average value of the short side of the primary particles; 5) Specific surface area: The specific surface area of ​​the precursor was tested using a 3H-2000BET-A nitrogen adsorption specific surface area tester; 6) Tap density: Use JZ-1 powder tap density tester to test the precursor; 7) Electrical performance test Preparation of buckle battery: According to the mass ratio of positive electrode material: Super-P: KS-6: PVDF of 92:3:2:3, 9.2g positive electrode material, 0.3g Super-P, 0.2g KS-6 and 0.3g 10wt% PVDF were weighed respectively, and then 4g NMP was added and mixed evenly, and then smeared on aluminum foil and dried to make a positive electrode sheet. In an inert gas protection glove box, a metal lithium sheet was used as the negative electrode, a PP material was used as the diaphragm, and 1mol / L LiPF6 / EC:DMC (volume ratio 1:1) was used as the electrolyte to assemble a CR2016 model buckle battery.

[0024] The prepared button battery is formed at a voltage of 3.0-4.4V at a rate of 0.1C and is ready for use.

[0025] Cycle test: The formed button battery is charged with constant current and constant voltage at 0.5C current, with a cut-off voltage of 4.4V and a cut-off current of 0.02C, and then discharged to 3.0V at 1C current. The battery is placed in a constant temperature control cabinet at 45℃ for testing. Example 1

[0026] Precursor preparation: 1) preparing a mixed salt solution by mixing a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution in a molar ratio of nickel sulfate:cobalt sulfate:manganese sulfate of 6:1:3, wherein the total concentration of the mixed salt solution is 2 mol / L, and preparing a NaOH solution with a concentration of 4 mol / L as a precipitant solution and an ammonia solution with a concentration of 10 mol / L as a complexing agent solution; 2) Nitrogen with a flow rate of 27 L / min and oxygen with a flow rate of 3 L / min were continuously introduced into the sealed reactor, and then the precipitant solution and the complexing agent solution were added to prepare the base solution. The pH value of the mixed system was controlled to be 12, the ammonia concentration was 5 mol / L, and the mixture was stirred at a speed of 400 r / min. The temperature of the reactor was set to 60°C; 3) Add the mixed salt solution into the reactor at a feed rate of 0.07 L / min to carry out the nucleation reaction. When the crystal nucleus particle size grows to 1.2 μm, stop the nucleation reaction; 4) The nitrogen flow rate was adjusted to 30 L / min, and the rate of the mixed salt solution was adjusted to 0.04 L / min. The pH value of the mixed system was adjusted to 11 and the ammonia concentration was adjusted to 7 mol / L to carry out the particle growth reaction. The reaction was stopped when the particle size grew to 3.0 μm. 5) The particles are dehydrated by centrifuge and alkaline solution and pure water are added in turn to remove impurities. The dehydrated material is then dried and sieved to obtain a composition of Ni 0.6 Co 0.1 Mn 0.3 Precursor B1 of (OH)2.

[0027] Cathode material preparation: 6) Precursor B1 and lithium carbonate are mixed in a molar ratio of 1:1.07, as well as 0.3wt% of ZrO2 and 0.2wt% of boron oxide based on the total weight of the precursor and lithium carbonate, and sintered at 960°C for 10h in an oxygen atmosphere. After sintering, the mixture is crushed and pulverized to obtain a corresponding primary sintered particle positive electrode material intermediate; 7) The positive electrode material intermediate and 0.15wt% of the weight of the positive electrode material intermediate Al2O3 are uniformly coated in a coating device, and then sintered at 550°C for 10 hours in an air atmosphere. After cooling, the primary sintered granular positive electrode material C1 is sieved.

[0028] The precursor B1 and the positive electrode material C1 were tested. The test results of the precursor B1 are in Appendix 1, the test results of the positive electrode material C1 are in Appendix 2, and the electrical performance test results of the positive electrode material C1 are in Appendix 3. The cross-sectional view of the precursor B1 is shown in Figure 3 shown. Example 2

[0029] Precursor preparation: 1) preparing a mixed salt solution by mixing a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution at a molar ratio of nickel sulfate:cobalt sulfate:manganese sulfate of 8:1:1, wherein the total concentration of the mixed salt solution is 2 mol / L, and preparing a NaOH solution with a concentration of 4 mol / L as a precipitant solution and an ammonia solution with a concentration of 10 mol / L as a complexing agent solution; 2) Nitrogen with a flow rate of 29.7 L / min and oxygen with a flow rate of 0.3 L / min were continuously introduced into the sealed reactor, and then the precipitant solution and the complexing agent solution were added to prepare the base solution. The pH value of the mixed system was controlled to be 11.0, the ammonia concentration was 5 mol / L, and the mixture was stirred at a speed of 400 r / min. The temperature of the reactor was set to 60°C; 3) Add the mixed salt solution into the reactor at a feed rate of 0.12 L / min to carry out the nucleation reaction. When the crystal nucleus particle size grows to 1.4 μm, stop the nucleation reaction; 4) The nitrogen flow rate was adjusted to 30 L / min, and the feed rate of the mixed salt solution was adjusted to 0.08 L / min. The pH value of the mixed system was adjusted to 10.5 and the ammonia concentration was adjusted to 9 mol / L to carry out the particle growth reaction. The reaction was stopped when the particle size grew to 3.5 μm. 5) The particles are dehydrated by centrifuge and alkaline solution and pure water are added in turn to remove impurities. The dehydrated material is then dried and sieved to obtain a composition of Ni 0.8 Co 0.1 Mn 0.1 (OH)2 precursor B2.

[0030] Cathode material preparation: Precursor B2 and lithium hydroxide are mixed in a molar ratio of 1:1.03, as well as 0.3wt% of ZrO2 based on the total weight of the precursor and lithium hydroxide, and 0.2wt% of boron oxide based on the total weight of the precursor and lithium hydroxide, and sintered at 860°C for 10h in an oxygen atmosphere, and crushed and pulverized after sintering to obtain a corresponding primary sintered particle positive electrode material intermediate; 7) The positive electrode material intermediate and 0.05 wt% of boron oxide by weight of the positive electrode material intermediate are uniformly coated in a coating device, and then sintered at 350° C. for 15 h in an oxygen atmosphere. After cooling, the secondary sintered granular positive electrode material C2 is sieved.

[0031] The precursor B2 and the positive electrode material C2 were tested. The test results of the precursor B2 are in Appendix 1, the test results of the positive electrode material C2 are in Appendix 2, and the electrical performance test results of the positive electrode material C2 are in Appendix 3. Example 3

[0032] Precursor preparation: 1) preparing a mixed salt solution by mixing a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution in a molar ratio of nickel sulfate:cobalt sulfate:manganese sulfate of 4:2:4, wherein the total concentration of the mixed salt solution is 2 mol / L, and preparing a NaOH solution with a concentration of 4 mol / L as a precipitant solution and an ammonia solution with a concentration of 9 mol / L as a complexing agent solution; 2) Nitrogen with a flow rate of 28 L / min and oxygen with a flow rate of 2 L / min were continuously introduced into the sealed reactor, and then the precipitant solution and the complexing agent solution were added to prepare the base solution. The pH value of the mixed system was controlled to be 10.8, the ammonia concentration was 5 mol / L, and the mixture was stirred at a speed of 400 r / min. The temperature of the reactor was set to 55°C; 3) Add the mixed salt solution into the reactor at a feed rate of 0.09 L / min to carry out nucleation reaction. When the crystal nucleus particle size grows to 0.8 μm, stop the nucleation reaction; 4) The nitrogen flow rate was adjusted to 30 L / min, and the feed rate of the mixed salt solution was adjusted to 0.05 L / min. The pH value of the mixed system was adjusted to 10.3 and the ammonia concentration was adjusted to 7 mol / L to carry out the particle growth reaction. The reaction was stopped when the particle size grew to 3.17 μm. 5) The particles are dehydrated by centrifuge and alkaline solution and pure water are added in turn to remove impurities. The dehydrated material is then dried and sieved to obtain a composition of Ni 0.4 Co 0.2 Mn 0.4 Precursor B3 of (OH)2.

[0033] Cathode material preparation: 6) Precursor B3 and lithium carbonate are mixed in a molar ratio of 1:1.04, as well as 0.3wt% of ZrO2 based on the total weight of the precursor and lithium carbonate, and 0.2wt% of boron oxide based on the total weight of the precursor and lithium carbonate, and sintered at 1000°C for 10h in an oxygen atmosphere. After sintering, the mixture is crushed and pulverized to obtain a corresponding primary sintered particle positive electrode material intermediate; 7) The cathode material intermediate and 0.15 wt% of the cathode material intermediate weight of Al2O3 are uniformly coated in a coating device, and then sintered at 550°C for 8 hours in an air atmosphere. After cooling, the secondary sintered granular cathode material C3 is sieved.

[0034] The precursor B3 and the positive electrode material C3 were tested. The test results of the precursor B3 are in Appendix 1, the test results of the positive electrode material C3 are in Appendix 2, and the electrical performance test results of the positive electrode material C3 are in Appendix 3. Example 4

[0035] Precursor preparation: 1) preparing a mixed salt solution by mixing a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution in a molar ratio of nickel sulfate:cobalt sulfate:manganese sulfate of 5:2:3, wherein the total concentration of the mixed salt solution is 2 mol / L, and preparing a NaOH solution with a concentration of 4 mol / L as a precipitant solution and an ammonia solution with a concentration of 10 mol / L as a complexing agent solution; 2) Nitrogen with a flow rate of 29 L / min and oxygen with a flow rate of 1 L / min were continuously introduced into the sealed reactor, and then the precipitant solution and the complexing agent solution were added to prepare the base solution. The pH value of the mixed system was controlled to be 11.5, the ammonia concentration was 5 mol / L, and the mixture was stirred at a speed of 400 r / min. The temperature of the reactor was set to 55°C; 3) Add the mixed salt solution into the reactor at a feed rate of 0.10 L / min to carry out the nucleation reaction. When the crystal nucleus particle size grows to 1.1 μm, stop the nucleation reaction; 4) The nitrogen flow rate was adjusted to 30 L / min, the feed rate of the mixed salt solution was adjusted to 0.06 L / min, the pH value of the mixed system was adjusted to 11, and the ammonia concentration was adjusted to 7 mol / L, and the particle growth reaction was carried out. When the particle size grew to 4.8 μm, the reaction was stopped; 5) The particles are dehydrated by centrifuge and alkaline solution and pure water are added in turn to remove impurities. The dehydrated material is then dried and sieved to obtain a composition of Ni 0.5 Co 0.2 Mn 0.3 Precursor B4 of (OH)2.

[0036] Cathode material preparation: 6) Precursor B4 and lithium carbonate are mixed in a molar ratio of 1:1.05, as well as 0.25wt% of ZrO2 and 0.2wt% of lithium sulfate based on the total weight of the precursor and lithium carbonate, and sintered at 940°C for 10h in an oxygen atmosphere. After sintering, the mixture is crushed and pulverized to obtain a corresponding primary sintered particle positive electrode material intermediate; 7) The cathode material intermediate and 0.15 wt% of the cathode material intermediate weight of Al2O3 are uniformly coated in a coating device, and then sintered at 550°C for 8 hours in an air atmosphere. After cooling, the secondary sintered granular cathode material C4 is sieved.

[0037] Precursor B4 and positive electrode material C4 were tested. The test results of precursor B4 are in Appendix 1, the test results of positive electrode material C4 are in Appendix 2, and the electrical performance test results of positive electrode material C4 are in Appendix 3.

[0038] Comparative Example 1 Precursor preparation: 1) preparing a mixed salt solution by mixing a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution in a molar ratio of nickel sulfate:cobalt sulfate:manganese sulfate of 5:2:3, wherein the total concentration of the mixed salt solution is 2 mol / L, and preparing a NaOH solution with a concentration of 4 mol / L as a precipitant solution and an ammonia solution with a concentration of 10 mol / L as a complexing agent solution; 2) Nitrogen with a flow rate of 25 L / min and oxygen with a flow rate of 5 L / min were continuously introduced into the sealed reactor, and then the precipitant solution and the complexing agent solution were added to prepare the base solution. The pH value of the mixed system was controlled to be 12, the ammonia concentration was 5 mol / L, and the mixture was stirred at a speed of 400 r / min. The temperature of the reactor was set to 60°C; 3) Add the mixed salt solution into the reactor at a feed rate of 0.07 L / min to carry out the nucleation reaction. When the crystal nucleus particle size grows to 1.2 μm, stop the nucleation reaction; 4) Without adjusting the gas flow rate, continue to introduce nitrogen at a flow rate of 25 L / min and oxygen at a flow rate of 5 L / min, and at the same time adjust the feed rate of the mixed salt solution to 0.04 L / min, adjust the pH value of the mixed system to 11, and the ammonia concentration to 8 mol / L, and carry out the particle growth reaction. When the particle size grows to 3.0 μm, stop the reaction; 5) The particles are dehydrated by centrifuge and alkaline solution and pure water are added in turn to remove impurities. The dehydrated material is then dried and sieved to obtain a composition of Ni 0.5 Co 0.2 Mn 0.3 (OH)2 precursor B5.

[0039] Cathode material preparation: 6) Precursor B5 and lithium hydroxide are mixed in a molar ratio of 1:1.02, Al2O3 of 0.1wt% of the total weight of the precursor and lithium hydroxide, and lithium sulfate of 0.25wt% of the total weight of the precursor and lithium hydroxide, and sintered at 920°C for 10h in an oxygen atmosphere. After sintering, the mixture is crushed and pulverized to obtain a corresponding primary sintered particle positive electrode material intermediate; 7) The cathode material intermediate and 0.1wt% of the cathode material intermediate weight of Al2O3 are uniformly coated in a coating device, and then sintered at 550°C for 8h in an air atmosphere. After cooling, the secondary sintered granular cathode material C5 is sieved.

[0040] The precursor B5 and the positive electrode material C5 were tested. The test results of the precursor B5 are in Appendix 1, the test results of the positive electrode material C5 are in Appendix 2, and the electrical performance test results of the positive electrode material C5 are in Appendix 3.

[0041] Comparative Example 2 The same as comparative example 1, except that in step 4) of preparing the precursor, the gas flow rate is adjusted to 20 L / min of nitrogen and 10 L / min of oxygen. The final prepared precursor B6, positive electrode material C6.

[0042] The precursor B6 and the positive electrode material C6 were tested. The test results of the precursor B6 are in Appendix 1, the test results of the positive electrode material C6 are in Appendix 2, and the electrical performance test results of the positive electrode material C6 are in Appendix 3.

[0043] Comparative Example 3 Precursor preparation: 1) preparing a mixed salt solution by mixing a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution in a molar ratio of nickel sulfate:cobalt sulfate:manganese sulfate of 6:1:3, wherein the total concentration of the mixed salt solution is 2 mol / L, and preparing a NaOH solution with a concentration of 4 mol / L as a precipitant solution and an ammonia solution with a concentration of 10 mol / L as a complexing agent solution; 2) Nitrogen with a flow rate of 28 L / min and oxygen with a flow rate of 2 L / min were continuously introduced into the sealed reactor, and then the precipitant solution and the complexing agent solution were added to prepare the base solution. The pH value of the mixed system was controlled to be 11.8, the ammonia concentration was 5 mol / L, and the mixture was stirred at a speed of 400 r / min. The temperature of the reactor was set to 60°C; 3) Add the mixed salt solution into the reactor at a feed rate of 0.07 L / min to carry out the nucleation reaction. When the crystal nucleus particle size grows to 1.2 μm, stop the nucleation reaction; 4) The nitrogen flow rate was adjusted to 30 L / min, and the feed rate of the mixed salt solution was adjusted to 0.04 L / min. The pH value of the mixed system was still 11.8, and the ammonia concentration was adjusted to 8 mol / L. The particle growth reaction was carried out, and the reaction was stopped when the particle size grew to 4.1 μm; 5) The particles are dehydrated by centrifuge and alkaline solution and pure water are added in turn to remove impurities. The dehydrated material is then dried and sieved to obtain a composition of Ni 0.6 Co 0.1 Mn 0.3 (OH)2 precursor B7.

[0044] Cathode material preparation: 6) Precursor B7 and lithium carbonate are mixed in a molar ratio of 1:1.07, as well as 0.3wt% of ZrO2 and 0.3wt% of boron oxide based on the total weight of the precursor and lithium carbonate, and sintered at 950°C for 10h in an oxygen atmosphere. After sintering, the mixture is crushed and pulverized to obtain a corresponding primary sintered particle cathode material intermediate; 7) The cathode material intermediate and 0.15 wt% of the cathode material intermediate weight of Al2O3 are uniformly coated in a coating device, and then sintered at 550°C for 8 hours in an air atmosphere. After cooling, the secondary sintered granular cathode material C7 is sieved.

[0045] The precursor B7 and the positive electrode material C7 were tested. The test results of the precursor B7 are in Appendix 1, the test results of the positive electrode material C7 are in Appendix 2, and the electrical performance test results of the positive electrode material C7 are in Appendix 3.

[0046] Comparative Example 4 Precursor preparation: 1) preparing a mixed salt solution by mixing a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution in a molar ratio of nickel sulfate:cobalt sulfate:manganese sulfate of 6:1:3, wherein the total concentration of the mixed salt solution is 2 mol / L, and preparing a NaOH solution with a concentration of 4 mol / L as a precipitant solution and an ammonia solution with a concentration of 10 mol / L as a complexing agent solution; 2) Nitrogen with a flow rate of 27 L / min and oxygen with a flow rate of 3 L / min were continuously introduced into the sealed reactor, and then the precipitant solution and the complexing agent solution were added to prepare the base solution. The pH value of the mixed system was controlled to be 12, the ammonia concentration was 5 mol / L, and the mixture was stirred at a speed of 400 r / min. The temperature of the reactor was set to 60°C; 3) Add the mixed salt solution into the reactor at a feed rate of 0.07 L / min to carry out the nucleation reaction. When the crystal nucleus particle size grows to 1.2 μm, stop the nucleation reaction; 4) The nitrogen flow rate was adjusted to 30 L / min, the feed rate of the mixed salt solution was not adjusted, the feed rate of the mixed salt solution was still 0.07 L / min, the pH value of the mixed system was adjusted to 11.5, the ammonia concentration was adjusted to 7 mol / L, and the particle growth reaction was carried out. When the particle size grew to 2.5 μm, the reaction was stopped; 5) The particles are dehydrated by centrifuge and alkaline solution and pure water are added in turn to remove impurities. The dehydrated material is then dried and sieved to obtain a composition of Ni 0.6 Co 0.1 Mn 0.3 (OH)2 precursor B8.

[0047] Cathode material preparation: 6) Precursor B8 and lithium carbonate are mixed in a molar ratio of 1:1.06, as well as 0.3wt% of ZrO2 and 0.2wt% of lithium fluoride based on the total weight of the precursor and lithium carbonate, and sintered at 960°C for 10h in an oxygen atmosphere. After sintering, the mixture is crushed and pulverized to obtain a corresponding primary sintered particle positive electrode material intermediate; 7) The cathode material intermediate and 0.15wt% of the cathode material intermediate weight of Al2O3 are uniformly coated in a coating device, and then sintered at 550°C for 8h in an air atmosphere. After cooling, the secondary sintered granular cathode material C8 is sieved.

[0048] The precursor B8 and the positive electrode material C8 were tested. The test results of the precursor B8 are in Appendix 1, the test results of the positive electrode material C8 are in Appendix 2, and the electrical performance test results of the positive electrode material C8 are in Appendix 3.

[0049] Schedule 1

[0050] During the growth stage of precursor B5, an oxidizing atmosphere was still passed, resulting in fine primary particles in the shell of the precursor, with a thickness of only 70nm. During the growth stage of precursor B6, too much oxidizing atmosphere was passed, which not only resulted in finer primary particles in the shell of the precursor, but also a wide size distribution of secondary particles. The pH of the growth stage of precursor B7 was not adjusted, which was the same as the nucleation stage of the precursor. Although the primary particles of the precursor were larger, the outer shell was denser. During the growth stage of precursor B8, the feed flow rate of the mixed salt solution was not adjusted, resulting in continued nucleation during the growth stage of the precursor and a wider distribution of secondary particles of the precursor.

[0051] Schedule 2

[0052] The cathode material C5 sample has fine primary particles in the precursor shell, so the primary particles are not easy to fuse during sintering. The particles after sintering are not close to spherical. The length of the long side of the primary sintered particles / the length of the short side of the primary sintered particles>1.5, and the average particle size D 50 / length of the short side of the primary particle > 2; the value of the long side length of the primary sintered particle / the short side length of the primary sintered particle and the average particle size D50 of the primary sintered particle after sintering of the positive electrode material C6 sample are larger than those of the positive electrode material C5 sample; the outer shell of the precursor of the positive electrode material C7 sample is relatively dense, and it is not easy for lithium salt to enter and disperse during sintering, resulting in the primary particles of the positive electrode material being not smooth, the long side length of the primary sintered particle / the short side length of the primary sintered particle > 1.5, and the average particle size D 50 / Short side length of primary sintered particles>2; The secondary particles of the positive electrode material C8 precursor are widely distributed and difficult to fuse during sintering, resulting in smaller primary particles after sintering, with an average particle size of D 50 The long side length of the first sintered particle / the short side length of the first sintered particle>1.5, and the average particle size D of the first sintered particle 50 / The short side length of the once sintered particles is >2.

[0053] Schedule 3

[0054] Since the positive electrode materials C5, C6, C7 and C8 samples are not within the requirement of long side length of primary sintered particles / short side length of primary sintered particles < 1.5, the average particle size D 50 / In the range of the short side length of the primary sintered particles <2, the high temperature cycle performance of the positive electrode material C5 and the positive electrode material C6 samples is poorer than that of the positive electrode material C4 sample; the high temperature cycle performance of the positive electrode material C7 and the positive electrode material C8 samples is poorer than that of the positive electrode material C1 sample.

[0055] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.

Claims

1. A single crystal cathode material precursor, characterized in that: The single crystal positive electrode material precursor is a secondary particle formed by the interlaced agglomeration of primary particles, and the primary particles are narrowly distributed, there are gaps between the primary particles, the thickness of the primary particles is 50-400nm, the single crystal positive electrode material precursor includes a core and a shell, the cross-sectional morphology of the core is loose, the core particle size is 0.5-1.5μm, the cross-sectional morphology of the shell is radiating, the shell thickness is 0.5-4.5μm, and the specific surface area of ​​the single crystal positive electrode material precursor is 8-20m 2 / g, tap density is 1.3~2.1g / cm 3 ; Average particle size D of secondary particles 50 The secondary particle size distribution (D 90 -D 10 ) / D 50 ≤0.

8.

2. A method for preparing a single crystal positive electrode material precursor according to claim 1, characterized in that The specific preparation steps are: Step S1, preparing a mixed salt solution of a nickel sulfate aqueous solution, a cobalt sulfate aqueous solution and a manganese sulfate aqueous solution, preparing a NaOH solution as a precipitant solution, and preparing an ammonia solution as a complexing agent solution; Step S2, continuously introducing nitrogen and oxygen into a sealed reactor, wherein the volume flow ratio of nitrogen to oxygen is 9-99:1, and then adding a precipitant solution and a complexing agent solution to prepare a base solution, controlling the pH value of the mixed system to be 10-12, the ammonia concentration to be 3-6 mol / L, and stirring at a speed of 300-600 r / min, and setting the temperature of the reactor to 50-70° C.; Step S3, adding a mixed salt solution into the reactor at a feed rate of 0.06-0.14 L / min to perform a nucleation reaction, and stopping the nucleation reaction when the crystal nucleus particle size grows to 0.5-1.5 μm; Step S4, adjusting the nitrogen gas to be introduced, and adjusting the feed rate of the mixed salt solution to be less than the feed rate of the mixed salt solution in step S3 before the adjustment, adjusting the pH value of the mixed system to be less than the pH value in step S2 before the adjustment, and adjusting the ammonia concentration to be greater than the ammonia concentration in step S2 before the adjustment, and performing a particle growth reaction, and stopping the reaction when the particle size grows to 2-5 μm; Step S5, dehydrating the particles by centrifuge and sequentially adding alkaline solution and pure water to remove impurities, and then drying the dehydrated material, and then sieving to obtain a single crystal positive electrode material precursor.

3. The method for preparing a single crystal positive electrode material precursor according to claim 2, characterized in that: The total concentration of the mixed salt solution in step S1 is 2 mol / L, the concentration of the precipitant solution is 4 mol / L, and the concentration of the complexing agent solution is 9-12 mol / L.

4. A spherical or quasi-spherical single crystal positive electrode material, characterized in that: The single crystal positive electrode material is a single crystal spherical or quasi-spherical particle, the ratio of the long side length to the short side length of the single crystal positive electrode material is less than 1.5, and the average particle size D of the secondary sintered particles is 50 / The short side length of the primary sintered particles is ≤2; the single crystal positive electrode material is made using the single crystal positive electrode material precursor according to claim 1.

5. A method for preparing a spherical or quasi-spherical single crystal positive electrode material according to claim 4, characterized in that The specific preparation steps are: Step S1, uniformly mixing the single crystal positive electrode material precursor prepared by the method of claim 2 or 3 with a lithium source, a doping additive and a flux, sintering at 800-1000° C. for 8-16 hours, and crushing and pulverizing after cooling to obtain a primary sintered granular positive electrode material intermediate; Step S2, coating the cathode material intermediate and the coating agent evenly in a coating device, sintering at 300-600° C. for 8-16 hours, cooling and sieving to obtain a secondary sintered granular cathode material.

6. The method for preparing a spherical or quasi-spherical single crystal positive electrode material according to claim 5, characterized in that: The molar ratio of the single crystal positive electrode material precursor to the lithium source in step S1 is 1:0.9-1.

07.

7. The method for preparing a spherical or quasi-spherical single crystal positive electrode material according to claim 5, characterized in that: The doping additive in step S1 is one or more compounds containing Ti, Zr, Mg, Ca, Sr, Ba, W, Nb, Mo, B, and Al, and the amount of the doping additive is 0.1wt%~0.5wt% of the total weight of the precursor and the lithium source; the flux is one or more compounds containing B, Li, and Ba, and the amount of the flux is 0.1wt%~0.3wt% of the total weight of the precursor and the lithium source.

8. The method for preparing a spherical or quasi-spherical single crystal positive electrode material according to claim 5, characterized in that: The coating agent in step S2 is one or more compounds containing Al, B, Ti, Zr, W, and Co, and the amount of the coating agent is 0.05wt%~2wt% of the weight of the positive electrode material intermediate.

Citation Information

Patent Citations

  • Spherical or near-spherical lithium-ion battery cathode materials, their preparation methods and applications

    CN106450155B

  • A single-crystal cathode material for lithium-ion batteries and its preparation method

    CN108461748B

  • Single-crystal lithium nickel cobalt manganate precursor and preparation method thereof and single-crystal lithium nickel cobalt manganate

    CN112226820A

  • Preparation method of nickel-cobalt-manganese hydroxide with granularity in single-peak width distribution

    CN114436343A

  • Low-cobalt ternary single-crystal positive electrode material, preparation method thereof and lithium ion battery

    CN115477333A

Cited By

  • Positive electrode, battery, energy-storage apparatus, and electricity-consumption device