Spherical silicon dioxide filler for frame sealing glue and preparation method of frame sealing glue
By combining the spherical silica filler with the resin on the surface modification, the problem of insufficient bonding performance and high moisture permeability in the liquid crystal display device is solved, and high bonding strength and low liquid crystal contamination are achieved, which is suitable for narrow Border LCD display device.
Patent Information
- Application Number
- CN202411242443.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
AI Technical Summary
The existing frame sealing glue has problems such as insufficient bonding performance, high moisture permeability and high liquid crystal contamination in liquid crystal display devices, resulting in Mura, reduced voltage retention rate and glass detachment on the display panel.
The surface-modified spherical silica filler was used to prepare a submicron spherical silica liquid by hydrolyzing and condensing tetraethyl orthosilicate and organic silicon compound under alkaline conditions, and the surface was prepared by spray drying and air flow pulverizing. The modified spherical silica filler, combined with a latent curing agent and resin, prepares a frame sealing glue with good dispersion and bonding strength.
It improves the dispersion and bonding strength of the frame sealing adhesive, reduces moisture permeability and liquid crystal contamination, enhances voltage retention and waterproofing performance, and is suitable for applications of narrow-frame liquid crystal display devices.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fillers, and specifically discloses a spherical silica filler for frame sealing adhesive and a preparation method of the frame sealing adhesive. Background Art
[0002] Liquid crystal devices are developing towards lightweight, thin, high screen-to-body ratio (narrow border). In the preparation process of liquid crystal displays (LCD), the sealant is mainly used to connect the CF substrate and the TFT substrate to seal the liquid crystal to prevent the liquid crystal from leaking out, and to prevent the external heat, moisture and dust from entering the liquid crystal display device and affecting its performance. In addition, it is also necessary to ensure that there is no small molecule precipitation inside the sealant to prevent itself from polluting the liquid crystal. Therefore, the sealant should have good bonding properties to the substrate and the alignment film, good moisture and heat resistance, excellent dispensing properties and low pollution. If the above requirements are not met, the display panel will have problems such as Mura, reduced voltage retention, bubbles in the liquid crystal, and even glass detachment. The sealant is mainly composed of resin, filler and other additives. The widely used thermosetting resin in the LCD industry is epoxy resin; the light-curing resin is mainly acrylic resin; the role of the filler is to improve the bonding strength of the resin matrix and reduce its moisture permeability and thermal expansion coefficient.
[0003] Therefore, a filler is needed that has good dispersibility and compatibility in the resin and also meets the requirements of narrow frame, low moisture permeability, low liquid crystal pollution and high bonding strength in the field of liquid crystal display. Based on this, the present application was developed. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a spherical silica filler for frame sealing glue that meets the above needs. The spherical silica filler has good dispersibility and compatibility in the resin, and can also meet the requirements of narrow frame, low moisture permeability, low liquid crystal contamination and high bonding strength in the liquid crystal display field.
[0005] The present invention also provides a frame sealing adhesive comprising the spherical silica filler for the frame sealing adhesive and a preparation method thereof.
[0006] To achieve the above object, the present invention adopts the following technical solution: A method for preparing a spherical silica filler for a frame sealant comprises the following steps: 1) Preparation of surface-modified spherical silica: Tetraethyl orthosilicate is hydrolyzed and condensed in the presence of a solvent and under alkaline conditions to prepare a submicron spherical silica liquid containing different particle sizes (300 nm~1000 nm); the organic silicon compound is reacted with the submicron spherical silica liquid containing different particle sizes obtained after distillation and concentration at 40~80℃ for 1~5h to obtain a surface-modified submicron spherical silica solution, which is then spray-dried and airflow-pulverized to obtain a surface-modified submicron spherical silica filler; 2) Preparation of in-situ surface-modified spherical silica: Tetraethyl orthosilicate and organic silicon compounds are hydrolyzed and condensed in the presence of a solvent and under alkaline conditions to prepare in-situ surface-modified submicron spherical silica liquid with different particle sizes (300 nm~1000 nm); after spray drying and air flow pulverization, in-situ surface-modified submicron spherical silica filler is obtained; The spherical silica filler for frame sealing adhesive is the filler prepared in step 1) and / or step 2).
[0007] Specifically, in step 1), the hydrolysis condensation reaction temperature is 20-60°C, and the reaction time is 1-5 hours; in step 2), the hydrolysis condensation reaction temperature is 30-50°C, and the reaction time is 2-6 hours.
[0008] Furthermore, in steps 1) and 2), the solvent includes one or more of ethanol, isopropanol, n-butanol and distilled water.
[0009] Furthermore, the alkaline condition is to adjust the pH value to 8-11 by adding one or more of ammonia, diethylamine, ethylenediamine, triethylamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethylenepolyamine and pentaethylenehexamine.
[0010] Specifically, in steps 1) and 2), the organosilicon compound may be one or more of alkoxysilane or alkoxysilazane with a carbon chain length of 1 to 20; for example, it may be silane coupling agent KH560, silane coupling agent KH550, phenyltrimethoxysilane, silane coupling agent KH570, etc. The amount of the organosilicon compound added in step 1) is 0.5 to 6% of the mass of spherical silica, and the amount of the organosilicon compound added in step 2) is 1.5 to 15% of the mass of tetraethyl orthosilicate. In step 1), the slurry containing submicron spherical silica with different particle sizes is distilled and concentrated, and then the organosilicon compound is added to the slurry containing submicron spherical silica with different particle sizes obtained after distillation and concentration for reaction. In step 2), tetraethyl orthosilicate and the organosilicon compound are mixed and added to the solvent at the same time for hydrolysis and condensation reaction.
[0011] The invention provides a spherical silicon dioxide filler for frame sealing adhesive prepared by the preparation method.
[0012] The present invention also provides a frame sealant, which is composed of a mixture of the following raw materials in percentage by weight: 28-50 wt% of the spherical silica filler for the frame sealant, 46-69 wt% of the resin, 0.5-4 wt% of the latent curing agent, and 0.2-2 wt% of the latent curing accelerator. When preparing the frame sealant, a three-roller machine is used to mix the spherical silica filler, resin, latent curing agent, and latent curing accelerator for the frame sealant to obtain the frame sealant. The frame sealant of the present invention has good storage stability and can be stably stored for six months or more.
[0013] Specifically, the resin includes one or both of a heat-curing epoxy resin and a light-curing resin; the heat-curing epoxy resin is one or more of bisphenol A type, bisphenol F type, phenolic type or alicyclic epoxy resins, such as phenolic epoxy resin DEN425, bisphenol F epoxy resin 370, and phenolic epoxy resin DEN 431. The light-curing resin is one or more of polyester acrylic resin, amino acrylic resin, epoxy acrylic resin, polyurethane acrylic resin, etc., such as epoxy methacrylate resin ETERCURE6219-100 and alicyclic epoxy resin ERL 4221.
[0014] Specifically, the latent curing agent includes modified aliphatic amines, aromatic amines, dicyandiamides, imidazoles, organic anhydrides, organic hydrazides, etc. For example, it can be latent curing agent ADH, 1020, DY9577, etc. The storage temperature is 25-30°C, and the storage time is more than 6 months.
[0015] Specifically, the latent curing accelerator may be imidazole adducts, urea derivatives, amines, etc., such as latent curing agent PN-23 or PN-23J, QXE301, HS-601, DM-102, DYHARD UR400, etc.
[0016] A spherical silica filler for frame sealing adhesive and a preparation method of the frame sealing adhesive, comprising the following steps: Scheme 1: Preparation of surface-modified spherical silica filler and frame sealant 1-1) Preparation of surface-modified spherical silica filler, specifically: preparing spherical silica liquid with submicron size (300 nm~1000 nm) by hydrolysis and condensation of tetraethyl orthosilicate in the presence of a solvent and under alkaline conditions; distilling and concentrating the obtained liquid; reacting an organosilicon compound (used as a surface modifier) with the obtained spherical silica concentrated liquid at 40~80°C for 1~5h to obtain a surface-modified spherical silica solution; and finally spray drying and airflow pulverization to obtain a surface-modified spherical silica filler; 1-2) Preparation of frame sealant: The surface-modified spherical silica filler obtained in step 1-1), the latent curing agent, the latent curing accelerator and the resin are mixed using a three-roll mill to obtain a frame sealant.
[0017] Specifically, in step 1-1), the solvent used is a mixed solution of one or more of ethanol, isopropanol, and n-butanol and distilled water, and the alkaline condition is adjusted to pH 8 to 11 by adding ammonia water or one or more of organic bases such as diethylamine, ethylenediamine, triethylamine, diethylenetriamine, tetraethylenepentamine, polyethylenepolyamine, pentaethylenehexamine, etc. The particle size and sphericity of spherical silica can be adjusted by changing the solvent ratio, reaction concentration, pH value, reaction temperature and time.
[0018] Furthermore, in step 1-1), the hydrolysis condensation reaction temperature is 20-60°C, and the reaction time is 1-5 hours. The mass ratio of tetraethyl orthosilicate in the entire reaction system is 10-20%, and it is added to the solvent at a uniform speed, and the time is preferably controlled within 10-30 minutes.
[0019] Furthermore, in step 1-1), atmospheric distillation is performed until the solid content of spherical silica in the feed liquid is 10-20%. The purpose of distillation is to increase the concentration of silica in the feed liquid, thereby improving the surface modification efficiency. The mother liquor after distillation can be reused, which can reduce the amount of alkali and ethanol used in the next experiment and reduce the waste of resources.
[0020] Specifically, in step 1-1), the organosilicon compound can be an organosilicon compound with a carbon chain length of 1 to 20, and the carbon chain can have an alkyl group, a double bond, an amino group, an epoxy group, a phenyl group, etc., which can be one or more of them; including but not limited to alkoxysilane, alkoxysilazane, etc.; the amount of the organosilicon compound added is 0.5 to 5% of the weight of the spherical silica.
[0021] Scheme 2: Preparation of in-situ surface-modified spherical silica filler and frame sealant 2-1) Preparation of in-situ surface-modified spherical silica filler, specifically: after tetraethyl orthosilicate and an organic silicon compound are uniformly mixed, hydrolysis and condensation are carried out in the presence of a solvent and under alkaline conditions to prepare in-situ surface-modified submicron spherical silica liquid with different particle sizes (300 nm~1000 nm); after spray drying and air flow pulverization, in-situ surface-modified submicron spherical silica filler is obtained; 2-2) Preparation of frame sealant: The in-situ surface-modified spherical silica filler obtained in step 2-1), the latent curing agent, the latent curing accelerator and the resin are mixed using a three-roll mill to obtain a frame sealant.
[0022] Furthermore, in step 2-1), the solvent used is a mixed solution of one or more of ethanol, isopropanol, and n-butanol and distilled water, and the alkaline condition is adjusted to pH 8 to 11 by adding ammonia water or one or more of organic bases such as diethylamine, ethylenediamine, triethylamine, diethylenetriamine, tetraethylenepentamine, polyethylenepolyamine, pentaethylenehexamine, etc. The particle size and sphericity of spherical silica can be adjusted by changing the solvent ratio, reaction concentration, pH value, reaction temperature and time.
[0023] Specifically, in step 2-1), the hydrolysis condensation reaction temperature is 30-50°C, and the reaction time is 2-6h. The mass ratio of tetraethyl orthosilicate to the entire reaction system is 10-20%; the organosilicon compound can be an organosilicon compound with a carbon chain length of 1-20, and the carbon chain can have an alkyl group, a double bond, an amino group, an epoxy group, a phenyl group, etc., which can be one or more of them; including but not limited to alkoxysilane, alkoxysilazane, etc.; the amount of the organosilicon compound added is 1.5-15% of the weight of tetraethyl orthosilicate. The mixed solution of tetraethyl orthosilicate and organosilicon compound is added to the solvent at a uniform speed, and the time is preferably controlled at 10-30min.
[0024] Further, in step 1-2) combined with step 2-2), the resin is one or both of a heat-curing epoxy resin and a light-curing resin. The epoxy resin is a bisphenol A type, bisphenol F type, phenolic type or alicyclic epoxy resin; the light-curing resin is a polyester acrylic resin, an amino acrylic resin, an epoxy acrylic resin, and a polyurethane acrylic resin. Preferably, the mass ratio of epoxy resin, light-curing resin, and spherical silica is (6-8): (2-4): (4-10). The latent curing agent is a modified aliphatic amine, an aromatic amine, a dicyandiamide, an imidazole, an organic acid anhydride, and an organic hydrazide. Preferably, the mass ratio of epoxy resin to latent curing agent and latent curing accelerator is 10: (0.5-1): (0.3-0.5).
[0025] The present invention aims to provide a spherical silica filler for frame sealant and a preparation method of frame sealant, which has easy-to-control reaction conditions, simple preparation process, easy storage, is suitable for large-scale production and has low cost. The prepared spherical silica filler can react with hydroxyl or epoxy groups in the resin to form chemical bonds due to the organic surface; or because the surface polarity of the spherical silica changes, it can be stably dispersed in a variety of resins. Compared with the prior art, the present invention has the following beneficial effects: The spherical silicon dioxide particles prepared by the method of the present invention have a size between 300 nm and 1000 nm, good sphericity and narrow particle size distribution. Surface modification effectively prevents nanoparticles from agglomerating, increases their dispersibility in organic media and polymer materials, reduces the viscosity of the frame sealant, and improves the uniformity and reliability of the glue coating. In addition, the lower viscosity improves the wettability of the interface between the frame sealant and the substrate, and improves the bonding strength between the colloid and the substrate; the surface of the silicon dioxide after surface modification carries a reactive group, which can react with the resin during light / heat curing, and the two are covalently bonded to improve the bonding strength and thermal curing efficiency of the spherical silicon dioxide and the resin matrix, thereby improving the water-proof performance and voltage holding rate of the frame sealant and reducing liquid crystal contamination. The viscosity and silicon oxide content of the frame sealant can be regulated by changing the reaction concentration, the particle size of the spherical silicon dioxide, the type of modifier, the amount of modifier, the type of resin, etc., and has good application prospects. The preparation process provided by the present invention is simple, the reaction conditions are easy to control, the cost is low, and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 TEM photos of spherical silica fillers of different sizes obtained in Examples 1-4; Figure 2 The cross-sectional SEM images of the frame sealant prepared with unmodified 700 nm spherical silica filler after thermal curing (left) and the cross-sectional SEM images of the frame sealant prepared with in-situ modified 700 nm spherical silica filler in Example 5 after thermal curing (right, curing temperature 130°C 2h). DETAILED DESCRIPTION
[0027] The technical solution of the present invention is further described in detail below in conjunction with the embodiments, but the protection scope of the present invention is not limited thereto.
[0028] In the present invention, the raw materials involved are all common commercial products that can be directly purchased.
[0029] The operation steps involved in the experimental steps, such as spray drying and air flow milling, which are not described in detail, can be carried out using conventional techniques in the art. Since they are not the core and innovation of this application, they will not be described in detail.
[0030] Embodiment 1: A method for preparing a 300 nm spherical silica filler and a single-component frame-sealing adhesive thereof comprises the following steps: 1) Weigh 40g of ammonia water (concentration of 25-28%), 300g of ethanol, and 100g of distilled water into a 1L three-necked flask (pH of the mixed solution is 11), add 70g of tetraethyl orthosilicate under stirring at 45°C, add dropwise for 10min, and react at constant temperature for 2h; distill under atmospheric pressure to concentrate the feed liquid to a silicon oxide solid content of 10%. In this step, 300 nm spherical silica with a mass of 20.6g is obtained.
[0031] 2) Add 1 g of silane coupling agent KH560 to the concentrated solution obtained in step 1) and react at 60° C. for 4 h to obtain a surface-modified spherical silica solution; spray dry and air flow crush to obtain a 300 nm spherical silica filler.
[0032] 3) 15 g of the 300 nm spherical silica filler prepared in step 2), 23.3 g of phenolic epoxy resin DEN425, 0.23 g of latent curing agent ADH, and 0.11 g of latent curing accelerator PN-23 were mixed uniformly to obtain a white slurry, which is a single-component frame sealing adhesive containing 300 nm spherical silica.
[0033] Embodiment 2: A method for preparing a 500 nm spherical silica filler and a single-component frame-sealing adhesive thereof comprises the following steps: 1) Weigh 45 g of ethylenediamine, 280 g of ethanol, and 51 g of distilled water into a 1L three-necked flask (pH of the mixed solution is 11), add 48 g of tetraethyl orthosilicate under stirring at 35 °C, add for 15 min, and react at constant temperature for 2 h; distill under atmospheric pressure to concentrate the feed liquid to a silicon oxide solid content of 10%. In this step, 500 nm spherical silica with a mass of 13.8 g was obtained.
[0034] 2) Add 0.4 g of silane coupling agent KH550 to the concentrated solution obtained in step 1), react at 60° C. for 3 h to obtain a surface-modified spherical silica solution; spray dry and air flow crush to obtain a 500 nm spherical silica filler.
[0035] 3) 13 g of the 500 nm spherical silica prepared in step 2), 23.3 g of bisphenol F epoxy resin 370, 0.23 g of modified amine latent curing agent 1020, and 0.11 g of latent curing accelerator QXE301 were mixed evenly to obtain a white slurry, which is a single-component frame sealing adhesive containing 500 nm spherical silica.
[0036] Embodiment 3: A method for preparing a 700 nm spherical silica filler and a frame sealant thereof comprises the following steps: 1) Weigh 50g of diethylamine, 128g of ethanol, 130g of isopropanol, and 48g of distilled water into a 1L three-necked flask (pH of the mixed solution is 10), add 63g of tetraethyl orthosilicate under stirring at room temperature, add dropwise for 25min, heat to 30°C, and react at constant temperature for 2h; distill and concentrate the feed liquid to a silicon oxide solid content of 15%. The mass of 700nm spherical silica obtained in this step is 18.14g.
[0037] 2) Add 0.5 g of silane coupling agent KH560 and 0.5 g of phenyltrimethoxysilane to the concentrated solution obtained in step 1), react at 60° C. for 3 h to obtain a surface-modified spherical silica solution; spray dry and air flow crush to obtain a 700 nm spherical silica filler.
[0038] 3) 10 g of the 700 nm spherical silica prepared in step 2), 18.64 g of phenolic epoxy resin DEN 431, 4.66 g of epoxy methacrylate resin ETERCURE 6219-100, 0.19 g of latent curing agent ADH, and 0.56 g of latent curing accelerator PN-23J were mixed uniformly to obtain a white slurry, which is a frame sealant containing 700 nm spherical silica.
[0039] Embodiment 4: A method for preparing a 1000 nm spherical silica filler and a single-component frame-sealing adhesive thereof comprises the following steps: 1) Weigh 35 g of triethylenetetramine, 100 g of ethanol, 50 g of isopropanol, 50 g of n-butanol, and 39 g of distilled water into a 1L three-necked flask (pH of the mixed solution is 10), add 45 g of tetraethyl orthosilicate under stirring at room temperature, add for 15 min, heat to 30 °C, react at constant temperature for 2 h, distill, and concentrate the feed liquid to a silicon oxide solid content of 18%. The mass of 1000 nm spherical silica obtained in this step is 12.96 g.
[0040] 2) Add 0.65 g of silane coupling agent KH570 to the concentrated solution obtained in step 1) and react at 60° C. for 3 h to obtain a surface-modified spherical silica solution; spray dry and air flow crush to obtain a 1000 nm spherical silica filler.
[0041] 3) 10 g of the 1000 nm spherical silica prepared in step 2), 23.3 g of alicyclic epoxy resin ERL4221, 0.2 g of latent curing agent DY9577, and 0.1 g of latent curing accelerator HS-601 were mixed evenly to obtain a white slurry, which is a frame sealant containing 1000 nm spherical silica.
[0042] Figure 1 TEM photos of spherical silica fillers of different sizes prepared in Examples 1-4 are given. Figure 1 It can be seen that the prepared spherical silica of various typical sizes have regular morphology and uniform particle size.
[0043] Embodiment 5: A method for preparing a 700 nm in-situ modified spherical silica filler and a frame sealant, comprising the following steps: 1) Weigh 50g of diethylamine, 128g of ethanol, 130g of isopropanol, and 48g of distilled water into a 1L three-necked flask (pH of the mixed solution is 10), add a mixed solution of 63g of tetraethyl orthosilicate, 0.5g of silane coupling agent KH560, and 0.5g of phenyltrimethoxysilane under stirring at room temperature, add for 25min, heat to 30℃, and react at constant temperature for 4h; then spray dry and air flow crush. The mass of 700nm in-situ modified spherical silica obtained in this step is 18.14g.
[0044] 2) 10 g of the 700 nm spherical silica prepared in step 1), 18.64 g of phenolic epoxy resin DEN 431, 4.66 g of epoxy methacrylate resin ETERCURE 6219-100, 0.19 g of latent curing agent ADH, and 0.56 g of latent curing accelerator PN-23J were mixed uniformly to obtain a white slurry, which is a sealant containing 700 nm in-situ modified spherical silica.
[0045] Figure 2 The cross-sectional SEM images of the frame sealant prepared by the unmodified 700 nm spherical silica and the 700 nm in-situ modified spherical silica filler obtained in Example 5 after curing are given. Figure 2 It can be seen that the cross section of the frame sealant prepared by the unmodified filler has obvious holes, indicating that the interfacial force with the resin is very weak and there is obvious agglomeration. On the contrary, the sample prepared in Example 5 has significantly better dispersibility of silicon oxide in the resin, and silicon oxide is tightly coated by the epoxy resin. The sample is embedded in the epoxy resin matrix, indicating excellent interfacial compatibility and strong interfacial bonding between it and the epoxy resin matrix.
[0046] The frame sealants obtained in Examples 3 and 5 were subjected to thermal curing and light curing, and then reliability performance tests were performed, and the test results are shown in Table 1. As can be seen from the table, the adhesion of the prepared modified spherical silica filler to the substrate, moisture permeability, water absorption, voltage holding rate and the pot life of the frame sealant all passed the standard test.
[0047] Table 1 Reliability test of the frame sealants prepared in Examples 3 and 5 The modified spherical silica filler prepared by the present invention has good dispersibility in the frame sealant matrix, reduces liquid crystal contamination, improves the water-proof performance, voltage holding rate and bonding strength to the glass substrate of the frame sealant, can be compounded with other light-curing potting adhesives, has a storage temperature of 25-30°C and a storage time of more than 6 months.
[0048] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes that do not deviate from the present invention should be equivalent replacement modes and are included in the protection scope of the present invention.
Claims
1. A method for preparing a spherical silica filler for a frame sealant, It is characterized in that The steps include: 1) Preparation of surface-modified spherical silica: tetraethyl orthosilicate is hydrolyzed and condensed in the presence of a solvent and under alkaline conditions to prepare a spherical silica liquid containing submicron particles of different sizes; the organic silicon compound is reacted with the spherical silica liquid containing submicron particles of different sizes obtained after distillation and concentration at 40-80°C for 1-5h to obtain a surface-modified submicron spherical silica solution, which is then spray-dried and airflow-pulverized to obtain a surface-modified submicron spherical silica filler; 2) Preparation of in-situ surface-modified spherical silica: Tetraethyl orthosilicate and organic silicon compounds are hydrolyzed and condensed in the presence of a solvent and under alkaline conditions to prepare in-situ surface-modified submicron spherical silica liquid containing different particle sizes; after spray drying and air flow pulverization, in-situ surface-modified submicron spherical silica filler is obtained; The spherical silica filler for frame sealing adhesive is the filler prepared in step 1) and / or step 2).
2. The method for preparing the spherical silica filler for frame sealant according to claim 1, It is characterized in that In step 1), the hydrolysis condensation reaction temperature is 20-60°C, and the reaction time is 1-5 hours; in step 2), the hydrolysis condensation reaction temperature is 30-50°C, and the reaction time is 2-6 hours.
3. The method for preparing the spherical silica filler for frame sealant according to claim 1, It is characterized in that In steps 1) and 2), the solvent includes one or more of ethanol, isopropanol, n-butanol and distilled water.
4. The method for preparing the spherical silica filler for frame sealant according to claim 1, It is characterized in that The alkaline condition is to adjust the pH value to 8-11 by adding one or more of ammonia, diethylamine, ethylenediamine, triethylamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethylenepolyamine and pentaethylenehexamine.
5. The method for preparing the spherical silica filler for frame sealant according to claim 1, It is characterized in that In steps 1) and 2), the organosilicon compound is one or more of alkoxysilane or alkoxysilazane with a carbon chain length of 1 to 20; the amount of the organosilicon compound added in step 1) is 0.5 to 6% of the mass of the spherical silica, and the amount of the organosilicon compound added in step 2) is 1.5 to 15% of the mass of tetraethyl orthosilicate.
6. A spherical silica filler for frame sealing adhesive prepared by the preparation method according to any one of claims 1 to 5.
7. A frame sealing adhesive, It is characterized in that The invention is composed of a mixture of the following raw materials in percentage by weight: 28-50 wt% of the spherical silica filler for the frame sealant according to claim 6, 46-69 wt% of resin, 0.5-4 wt% of a latent curing agent, and 0.2-2 wt% of a latent curing accelerator.
8. The frame sealant according to claim 7, It is characterized in that The resin includes one or both of a heat-curing epoxy resin and a light-curing resin; the heat-curing epoxy resin is one or more of bisphenol A type, bisphenol F type, phenolic type or alicyclic epoxy resin; the light-curing resin is one or more of polyester acrylic resin, amino acrylic resin, epoxy acrylic resin, polyurethane acrylic resin.
9. The frame sealant according to claim 7, It is characterized in that The latent curing agent is modified aliphatic amines, aromatic amines, dicyandiamide, imidazoles, organic acid anhydrides, and organic hydrazides.
10. The frame sealant according to claim 7, It is characterized in that The latent curing accelerator is imidazole adduct, urea derivative, and amine.