Anti-oxidation and corrosion-resistant glass mold as well as preparation method and application thereof

By using specific proportions of element composition and heat treatment process in glass molds, a dense silicate film is formed, which solves the mold oxidation and corrosion problems in the production of fluoride milk white glass wine bottles, significantly extends the service life and improves the quality.

CN118996252APending Publication Date: 2024-11-22SUZHOU DONGHAI GLASS MOLD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411039232.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing glass molds for the production of fluoride milk white wine bottles have short service life due to oxidation and corrosion, which cannot meet the quality requirements of high-end white wine bottles.

Method used

Adopt the composition of carbon 1.5%-2.5%, silicon 6%-9%, manganese 0.7%-0.8%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.6%-0.9%, nickel 0.7%-1% Oxidative corrosion-resistant glass molds, through specific formulation design and heat treatment processes, form dense silicate films to block hydrofluoric acid corrosion, and undergo nickel-based alloy powder surfacing to improve mechanical properties.

Benefits of technology

It effectively improves the anti-oxidation and corrosion resistance of glass molds, extends the service life to more than 350,000 times, and ensures the appearance quality and production efficiency of high-end liquor bottles.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an anti-oxidation corrosion-resistant glass mold and a preparation method and application thereof, the anti-oxidation corrosion-resistant glass mold comprises the following components in percentage by weight: 1.5%-2.5% of carbon, 6%-9% of silicon, 0.7%-0.8% of manganese, less than or equal to 0.08% of phosphorus, less than or equal to 0.05% of sulfur, 0.6%-0.9% of molybdenum, 0.7%-1% of nickel and the balance of iron, and the total amount is 100%. The preparation method comprises the steps of burdening, smelting, inoculation and pouring, heat treatment and machining. The corrosion resistance and the oxidation resistance of the glass mold are effectively improved, and the glass mold can effectively cope with hydrofluoric acid corrosion, so that the service life of the glass mold for producing the fluoride milky white material glass white spirit bottle is prolonged from no more than 150 thousand times in the prior art to more than 35 thousand times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of glass molds, in particular to an oxidation-resistant and corrosion-resistant glass mold and a preparation method and application thereof, which are used for producing fluoride opalescent glass liquor bottles. Background Art

[0002] In recent years, in the mid-to-high-end liquor packaging market, opal glass packaging bottles have become increasingly popular among consumers and liquor manufacturers, and the market potential is huge. This is mainly because some ingredients in high-end liquor will react chemically when exposed to light for a long time, causing changes in the flavor and quality of the liquor. The opal glass bottles have the characteristics of opacity, which can effectively block light, thereby blocking ultraviolet rays and other harmful light, and protecting the quality and flavor of the liquor. In addition, compared with ordinary glass bottles, opal glass bottles are more solid and not easy to break, which can reduce damage during packaging and transportation; opal glass bottles have a porcelain-like luster and texture, noble and exquisite appearance, and visually unique, which can help brands stand out from many products, enhance brand recognition and memory points, and improve the grade and market appeal of high-end liquor brands; the production process of opal glass bottles is complex and difficult to counterfeit, which helps prevent counterfeit and inferior products from entering the market and protect the interests of brands and consumers.

[0003] According to the different types of opacifiers, opal glass bottles can be divided into fluoride opal glass bottles, fluoride and sulfate mixed opal glass bottles and phosphate opal glass bottles. Among them, in the daily packaging glass industry, the opal glass bottles used to make liquor bottles generally use sodium fluorosilicate as the opacifier.

[0004] Ductile iron or vermicular cast iron is the base material of cast iron glass molds for producing fluoride opalescent glass liquor bottles. However, glass molds made of ductile iron will deform more at high temperatures, which will cause the seams of the bottles to be thick, which is an unacceptable quality abnormality for high-end liquor bottles that have strict requirements on the appearance of the bottles. Although glass molds made of gray cast iron can maintain dimensional stability under heat preservation and solve the defect of thick seams of bottles, they will have obvious oxide layer peeling and corrosion during use, and have a short service life of no more than 150,000 times, which is generally only about one-third of that of ordinary glass bottle molds.

[0005] Therefore, developing a glass mold that is resistant to oxidation, corrosion, and has good high-temperature dimensional stability has extremely important technical and economic significance. Summary of the invention

[0006] The invention provides an oxidation-resistant and corrosion-resistant glass mold and a preparation method and application thereof, which can solve the problem of short service life of glass molds used for producing fluoride opalescent glass liquor bottles in the prior art due to oxidation and corrosion.

[0007] In order to solve the above technical problems, the present invention provides an oxidation-resistant and corrosion-resistant glass mold, comprising the following components in percentage by weight:

[0008] Carbon 1.5%-2.5%, silicon 6%-9%, manganese 0.7%-0.8%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.6%-0.9%, nickel 0.7%-1%, the balance is iron, the total amount is 100%.

[0009] In a preferred embodiment of the present invention, the combined amount of carbon and silicon is: C+1 / 3Si=4.3-4.4%.

[0010] In a preferred embodiment of the present invention, the components are as follows in parts by weight: carbon 1.8%-2.2%, silicon 7%-8%, manganese 0.7%-0.8%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.7%-08%, nickel 0.8%-0.9%, and the balance is iron, with a total amount of 100%.

[0011] In order to solve the above technical problems, the present invention also provides a method for preparing an oxidation-resistant and corrosion-resistant glass mold, comprising the following steps:

[0012] (1) Ingredients: Use foundry pig iron, scrap steel, ferrosilicon, ferromanganese, ferromolybdenum and electrolytic nickel as raw materials, weigh and mix according to the above mass percentages:

[0013] (2) Melting: Heat and melt the weighed cast iron, scrap iron and electrolytic nickel, then add weighed ferrosilicon, ferromanganese and ferromolybdenum to melt into molten iron, and adjust the temperature of the molten iron to 1550-1580°C;

[0014] (3) Inoculation and casting: After inoculation and slagging, the molten iron is cast into a mold under a heat preservation state, and after cooling, the material is cleaned and discharged to obtain a casting;

[0015] (4) Heat treatment: The casting is heated from room temperature to 950°C to 980°C at a rate not exceeding 100°C per hour, kept at this temperature for 8 hours, then cooled to 500°C at a rate not exceeding 25°C per hour, and air-cooled to room temperature;

[0016] (6) Mechanical processing: The casting after the above heat treatment is subjected to rough machining, fine machining and polishing to obtain the glass mold.

[0017] In a preferred embodiment of the present invention, in step (3), the inoculation method is: evenly spreading the silicon-barium inoculant on the bottom of the molten iron ladle, and then inoculating the molten iron by a ladle method.

[0018] In a preferred embodiment of the present invention, the amount of the silicon-barium inoculant is 0.6-0.8% of the total weight of the molten iron.

[0019] In a preferred embodiment of the present invention, the incubation temperature is 1420°C-1320°C, and the time is 2-10 minutes.

[0020] In a preferred embodiment of the present invention, in step (5), after the rough machining, a nickel-based alloy powder surfacing treatment step is also included.

[0021] In order to solve the above technical problems, the present invention also provides an application of an oxidation-resistant and corrosion-resistant glass mold for producing fluoride opalescent glass liquor bottles.

[0022] The beneficial effects of the present invention are as follows: the present invention provides an antioxidant and corrosion-resistant glass mold and a preparation method thereof, which effectively improves the corrosion resistance and antioxidant properties of the glass mold through formula design, especially the carbon content design and the high silicon content design, and can effectively cope with hydrofluoric acid corrosion, thereby increasing the service life of the glass mold for producing fluoride opalescent glass liquor bottles from no more than 150,000 times in the prior art to more than 350,000 times, and has strong practicality. DETAILED DESCRIPTION

[0023] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0024] The present invention has found that sodium fluorosilicate (Na2SiF6) causes oxidation and corrosion of gray cast iron at high temperatures. At the glass bottle molding temperature (about 530°C), the oxidation mechanism of sodium fluorosilicate on gray cast iron is as follows:

[0025] 1. Decomposition of sodium fluorosilicate

[0026] Under high temperature conditions, sodium fluorosilicate decomposes to produce fluoride and silicon oxide:

[0027] Na2SiF6→2NaF+SiF4

[0028] 2. Reaction of fluoride with iron

[0029] The generated fluorides (such as sodium fluoride NaF and silicon tetrafluoride SiF4) react with the iron in the cast iron to form iron fluoride and other fluorine-containing compounds:

[0030] 3SiF4+2Fe→2FeF3+3SiO2

[0031] 3. Oxidation process

[0032] At high temperatures, the iron on the surface of gray cast iron will be further oxidized to form an iron oxide layer (Fe2O3 or Fe3O4):

[0033] 4Fe+3O2→2Fe2O3

[0034] The generated oxide layer can play a certain protective role, but due to the presence of fluoride, this protective layer will be destroyed;

[0035] 4. Formation of Silicon Oxide

[0036] Silicon tetrafluoride (SiF4) generated by the decomposition of sodium fluorosilicate can be further hydrolyzed at high temperature to form silicon oxide (SiO2):

[0037] SiF4+2H2O→SiO2+4HF

[0038] 5. Corrosive effect of hydrogen fluoride

[0039] The generated hydrogen fluoride (HF) is a highly corrosive gas that will further corrode the gray cast iron, destroy the oxide layer, and undergo complex chemical reactions with elements such as iron and carbon:

[0040] Fe+2HF→FeF2+H2

[0041] 6. Changes in microstructure

[0042] At high temperatures, the microstructure of gray cast iron undergoes significant changes, mainly manifested in the peeling of the oxide layer. This is due to the presence of fluoride and hydrogen fluoride. The oxide layer formed is unstable and easily peels off, exposing new metal surfaces, leading to continuous oxidation and corrosion.

[0043] In view of the above findings, the present invention discloses an antioxidant and corrosion-resistant glass mold for the production of fluoride opal glass liquor bottles, which can effectively prevent the glass mold from being oxidized and corroded during the production of fluoride opal glass, thereby increasing its service life.

[0044] Specifically, an oxidation-resistant and corrosion-resistant glass mold has the following components in percentage by weight:

[0045] Carbon 1.5%-2.5%, preferably 1.8%-2.2%; silicon 6%-9%, preferably 7%-8%; and the combined amount of carbon and silicon is: C+1 / 3Si=4.3%-4.4%. The silicon content of up to 6%-9% enables the gray cast iron to have both casting performance and mechanical processing performance, and the high-silicon glass mold made of it can form a dense silica film on the surface in a hydrofluoric acid environment, the main component of which is silicon dioxide, which effectively blocks the corrosion of hydrofluoric acid to the base metal, thereby improving the corrosion resistance of the glass mold and playing a role of primary corrosion protection. The silicon content increases the eutectoid temperature of the glass mold to 800-900°C, which is higher than the operating temperature of the glass mold, and can effectively prevent the glass mold from undergoing phase change during use, thereby greatly reducing its oxidation phenomenon and increasing its service life.

[0046] In addition, the silicon and carbon components are designed near the eutectic composition, and the eutectic state is biased to achieve the following effects: 1. Good casting performance. The gray cast iron with eutectic composition has a low melting point and good fluidity, which can fill complex molds well and is suitable for manufacturing complex-shaped castings; 2. Good thermal conductivity. The graphite flake structure of gray cast iron gives it excellent thermal conductivity. The gray cast iron with eutectic composition maintains this advantage and is suitable for applications requiring good heat dissipation performance; 3. High dimensional stability. The gray cast iron with eutectic composition has good dimensional stability during heating and cooling, and is suitable for castings requiring high precision; 4. Good machinability. The gray cast iron with eutectic composition has good cutting machinability due to its graphite flake structure. And graphite plays a self-lubricating role, reducing tool wear, extending tool life, and making the machined surface smooth. The above properties make the prepared glass mold have excellent dimensional accuracy, thermal conductivity, high-temperature dimensional stability and service life, which helps to improve the production quality and appearance of fluoride milky white glass liquor bottles.

[0047] Manganese 0.7% - 0.8%. Manganese can form a stable oxide film (MnO) covering the surface of gray cast iron. This oxide film can play a protective role in high-temperature corrosion environments, slowing down the oxidation rate of the iron matrix of the glass mold and playing a secondary anti-corrosion protection role.

[0048] In addition, manganese is an effective solid solution strengthening element, which can promote solid solution strengthening in the ferrite matrix and improve the mechanical properties of gray cast iron, thereby improving the hardness and strength of the glass mold. Under high temperature conditions, it helps to enhance the wear resistance and deformation resistance of the material. This is especially important under high temperature conditions because high temperature will weaken the strength and hardness of the material. During the smelting process, manganese also has a desulfurization and deoxidation effect, which can reduce the effect of harmful elements sulfur and oxygen on the corrosiveness of gray cast iron at high temperatures, thereby further improving the high temperature corrosion resistance of the glass mold.

[0049] Molybdenum 0.6%-0.9%, preferably 0.7%-0.8%. The addition of molybdenum can improve the corrosion resistance of gray cast iron in acidic environment, especially in fluorine acid environment, can improve the alloy's resistance to pitting and crevice corrosion, and play a role in three-level corrosion protection. In addition, molybdenum can also improve the oxidation resistance and thermal fatigue performance of glass molds in high temperature environment.

[0050] Nickel 0.7%-1.0%, preferably 0.8%-0.9%. Nickel can form stable intermetallic compounds with the iron matrix, and these compounds have high oxidation resistance at high temperatures, thereby delaying the oxidation process and increasing the service life of the glass mold. Nickel can inhibit the spheroidization tendency of graphite, causing graphite to exist in the form of flakes or worms, which helps to improve the thermal conductivity of gray cast iron while maintaining good mechanical properties. In addition, the addition of nickel can also reduce the thermal expansion coefficient of gray cast iron, reduce thermal stress and deformation at high temperatures, help improve the dimensional stability and structural integrity of glass molds under high temperature conditions, and improve the appearance quality of fluoride opal glass liquor bottles.

[0051] Phosphorus ≤ 0.08%, sulfur ≤ 0.05%, the rest is iron, the total amount is 100%.

[0052] Example 1

[0053] A glass mold was prepared according to the following formula components in percentage by weight:

[0054] Carbon 2.0%, silicon 7%, manganese 0.7%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.7%, nickel 0.8%, the balance is iron, the total amount is 100%, and C+1 / 3Si=4.3-4.4%.

[0055] The specific preparation method is as follows:

[0056] (1) Ingredients: The raw materials are cast Q12 pig iron, national standard No. 45 scrap steel, ferrosilicon, ferromanganese, ferromolybdenum and electrolytic nickel. After chemical analysis, the ingredients are weighed and mixed according to the above formula:

[0057] (2) Melting: Place weighed cast Q12 pig iron, national standard No. 45 scrap iron and electrolytic nickel into a medium frequency melting furnace and heat until completely melted, then add weighed ferrosilicon, ferromanganese and ferromolybdenum charges, continue heating until completely melted into molten iron, and adjust the molten iron temperature to 1560°C;

[0058] (3) Inoculation and pouring: Weigh 0.7% of the total weight of the molten iron with a silicon-barium inoculant, evenly spread it on the bottom of the molten iron ladle, and inoculate the molten iron at a temperature of 1560° C. by a ladle method. After standing for 5 minutes, the molten iron in the ladle is deslagging, covered with perlite for insulation, and then poured at 1400° C. for 8 minutes;

[0059] After pouring, the casting is cooled to below 750℃ in the mold, and the casting is obtained after sand dropping, separation of pouring and riser, and sand cleaning and shot blasting.

[0060] (4) Heat treatment: In a heating furnace, the casting is heated from room temperature to 960°C at a rate of 80°C per hour, kept at this temperature for 8 hours, then cooled to 500°C at a rate of 20°C per hour, the furnace door is opened, air cooled to room temperature, and then taken out of the furnace;

[0061] The purpose of the above heat treatment is to perform graphitization annealing and casting stress relief annealing on the casting.

[0062] After heat treatment, shot blasting and burr grinding are carried out to remove the oxide scale and burrs generated during graphitization annealing and reduce the wear of the tool in subsequent machining.

[0063] (5) Mechanical processing: According to the design drawings and specifications of the glass mold of the designed milky white glass liquor bottle, the obtained casting is subjected to rough machining, nickel-based alloy powder surfacing treatment, fine machining and polishing treatment. After the finished product passes the inspection, the glass mold is obtained.

[0064] The hardness tested by Brinell hardness tester is 245HB.

[0065] The obtained anti-oxidation and corrosion-resistant glass mold is used to produce fluoride opal glass liquor bottles. Calculated at 10 times per minute per mold to produce fluoride opal glass liquor bottles, the service life of the glass mold is more than 350,000 times. There is no obvious corrosion or oxidation during use.

[0066] Example 2

[0067] The difference from Example 1 is that the formula components of the glass mold in weight percentage are different, as follows:

[0068] Carbon 1.6%, silicon 8%, manganese 0.8%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.8%, nickel 1.0%, the balance is iron, the total amount is 100%, and C+1 / 3Si=4.3-4.4%.

[0069] The hardness tested by Brinell hardness tester is 245HB.

[0070] The obtained anti-oxidation and corrosion-resistant glass mold is used to produce fluoride opal glass liquor bottles. Calculated at 10 times per minute per mold to produce fluoride opal glass liquor bottles, the service life of the glass mold is more than 350,000 times. No corrosion or oxidation is obvious during use.

[0071] Example 3

[0072] The difference from Example 1 is that the formula components of the glass mold in weight percentage are different, as follows:

[0073] Carbon 2.4%, silicon 6%, manganese 0.8%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.8%, nickel 0.9%, the balance is iron, the total amount is 100%, and C+1 / 3Si=4.3-4.4%.

[0074] The hardness tested by Brinell hardness tester is 245HB.

[0075] The obtained anti-oxidation and corrosion-resistant glass mold is used to produce fluoride opal glass liquor bottles. Calculated at 10 times per minute per mold to produce fluoride opal glass liquor bottles, the service life of the glass mold is more than 350,000 times. No corrosion or oxidation is obvious during use.

[0076] Comparative Example 1

[0077] The difference from Example 1 is that the glass mold is prepared according to the following formula components in percentage by weight:

[0078] Carbon 2.3%, silicon 2.0%, manganese 0.7%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.7%, nickel 0.8%, the balance is iron, the total amount is 100%, and C+1 / 3Si=4.3-4.4%.

[0079] The hardness tested by Brinell hardness tester is 236HB.

[0080] The obtained anti-oxidation and corrosion-resistant glass mold is used to produce fluoride opal glass liquor bottles. Based on the calculation that the fluoride opal glass liquor bottles are produced 10 times per mold per minute, the service life of the glass mold is 150,000 times. Obvious corrosion occurs during use.

[0081] Comparative Example 2

[0082] The difference from Example 1 is that the glass mold is prepared according to the following formula components in percentage by weight:

[0083] Carbon 2.3%, silicon 1.5%, manganese 0.8%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.8%, nickel 0.9%, the balance is iron, the total amount is 100%.

[0084] The hardness tested by Brinell hardness tester is 236HB.

[0085] The obtained anti-oxidation and corrosion-resistant glass mold is used to produce fluoride opal glass liquor bottles. The service life of the glass mold is less than 120,000 times, calculated based on the production of fluoride opal glass liquor bottles at 10 times per minute. There is obvious corrosion during use, and the sizes of the produced fluoride opal glass liquor bottles vary greatly, and the appearance quality is low.

[0086] Comparative Example 3

[0087] The difference from Example 1 is that the glass mold is prepared according to the following formula components in percentage by weight:

[0088] Carbon 2.0%, silicon 7%, manganese 0.3%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.3%, nickel 0.8%, the balance is iron, the total amount is 100%, and C+1 / 3Si=4.3-4.4%.

[0089] The hardness tested by Brinell hardness tester is 210HB.

[0090] The obtained anti-oxidation and corrosion-resistant glass mold is used to produce fluoride opal glass liquor bottles. The service life of the glass mold is less than 200,000 times, based on the production of fluoride opal glass liquor bottles 10 times per minute per mold. The corrosion and oxidation phenomenon during use is more obvious than that of Examples 1-3.

[0091] From the data comparison of the above embodiments 1-3 and comparative examples 1-3, it can be seen that the formula design with high silicon content effectively improves the corrosion resistance and oxidation resistance of the glass mold, can effectively cope with hydrofluoric acid corrosion, and effectively improves the service life of the glass mold in the production of fluoride opalescent glass liquor bottles.

[0092] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. An oxidation-resistant and corrosion-resistant glass mold, characterized in that: The composition comprises the following weight percentages: Carbon 1.5%-2.5%, silicon 6%-9%, manganese 0.7%-0.8%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.6%-0.9%, nickel 0.7%-1%, the balance is iron, the total amount is 100%.

2. The oxidation-resistant and corrosion-resistant glass mold according to claim 1, characterized in that: The combined amount of carbon and silicon is: C+1 / 3Si=4.3-4.4%.

3. The oxidation-resistant and corrosion-resistant glass mold according to claim 2, characterized in that: It includes the following components by weight: carbon 1.8%-2.2%, silicon 7%-8%, manganese 0.7%-0.8%, phosphorus ≤0.08%, sulfur ≤0.05%, molybdenum 0.7%-08%, nickel 0.8%-0.9%, and the balance is iron, and the total amount is 100%.

4. A method for preparing an oxidation-resistant and corrosion-resistant glass mold according to any one of claims 1 to 3, characterized in that: The steps include: (1) Ingredients: Use foundry pig iron, scrap steel, ferrosilicon, ferromanganese, ferromolybdenum and electrolytic nickel as raw materials, weigh and mix according to the above mass percentages: (2) Melting: Heat and melt the weighed cast iron, scrap iron and electrolytic nickel, then add weighed ferrosilicon, ferromanganese and ferromolybdenum to melt into molten iron, and adjust the temperature of the molten iron to 1550-1580°C; (3) Inoculation and casting: After inoculation and slagging, the molten iron is cast into a mold under a heat preservation state, and after cooling, the material is cleaned and discharged to obtain a casting; (4) Heat treatment: The casting is heated from room temperature to 950°C-980°C at a rate not exceeding 100°C per hour, kept at this temperature for 6-8 hours, then cooled to 450°C-500°C at a rate not exceeding 25°C per hour, and air-cooled to room temperature; (5) Mechanical processing: The casting after the above heat treatment is subjected to rough machining, fine machining and polishing to obtain the glass mold.

5. The method for preparing an oxidation-resistant and corrosion-resistant glass mold according to claim 4, characterized in that: In step (3), the inoculation method is: the silicon-barium inoculant is evenly spread on the bottom of the molten iron ladle, and then the molten iron is inoculated by the ladle method.

6. The method for preparing an oxidation-resistant and corrosion-resistant glass mold according to claim 5, characterized in that: The amount of the silicon-barium inoculant is 0.6-0.8% of the total weight of the molten iron.

7. The method for preparing an oxidation-resistant and corrosion-resistant glass mold according to claim 5, characterized in that: The incubation temperature is 1420° C.-1320° C., and the incubation time is 2-10 minutes.

8. The method for preparing an oxidation-resistant and corrosion-resistant glass mold according to claim 4, characterized in that: In step (5), after the rough machining, a nickel-based alloy powder surfacing treatment step is also included.

9. An application of the oxidation-resistant and corrosion-resistant glass mold according to claim 1, characterized in that: Used for producing fluoride opalescent glass liquor bottles.