Medium-carbon cold heading steel wire rod for 8.8-grade fastener and production method of medium-carbon cold heading steel wire rod

Through the direct rolling process of large square billets and multiple smelting and refining processes, the problems of high cost and high carbon emissions in traditional fasteners are solved, and the production of high-quality, low-cost and low-carbon emissions are achieved, which simplifies the production of fasteners and simplifies the production process and Reduced carbon emissions.

CN118996256APending Publication Date: 2024-11-22JIANGSU YONGGANG GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411090689.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

There are problems with high manufacturing costs and carbon emissions in the traditional 8.8-level fastener production process, especially when high-end fields such as automobiles have strict requirements on fastener quality, the traditional large square billet two-fire material process has increased carbon emissions and Complexity of the manufacturing process.

Method used

Through the redesign of the rolling process, the direct rolling process of large square billets is adopted to reduce the middle billet opening process, and the direct rolling of 240 square billets is achieved. Combined with converter smelting, LF refining, RH vacuum treatment and finishing processes, the product is ensured. and reduce carbon emissions and production costs through waste slag recycling, waste water treatment and waste gas recycling and reuse.

Benefits of technology

While keeping product quality unchanged, manufacturing costs and carbon emissions are reduced, production processes are simplified, production efficiency is improved, and high-quality, low-cost and low-carbon emissions are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996256A_ABST
    Figure CN118996256A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wire rod production, and provides a medium-carbon cold heading steel wire rod for a 8.8-grade fastener and a production method of the medium-carbon cold heading steel wire rod for the 8.8-grade fastener, and the production method comprises the procedures of converter smelting, LF refining and RH vacuum treatment, bloom continuous casting, billet finishing, heating, rolling, cooling and the like. 240 square bloom direct rolling is achieved through technical innovation, a blooming process is omitted, and cost and carbon are reduced. Through new process innovation, the cold heading steel wire rod is produced by adopting a bloom direct rolling process, so that the requirements of customers on high quality, low cost and low carbon emission are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wire rod production, and in particular to a medium carbon cold heading steel wire rod for 8.8 grade fasteners and a production method thereof. Background Art

[0002] 8.8 grade fasteners are the most widely used type of fasteners, and are widely used in the fields of automobiles, engineering machinery, home appliances, etc. 8.8 grade fasteners are generally produced using medium carbon cold heading steel such as SWRCH35K, ML35, etc. SWRCH35K is a carbon structural steel. The "S" in its name stands for Steel, "W" stands for Wire, "R" stands for Rod, "C" stands for Cold, and "H" stands for Heading. SWRCH35K products have high dimensional accuracy and good surface finish, so they are widely used in the production of bolts, nuts, and screws. They are also suitable for the production of parts in industries such as bicycles, automobiles, mechanical equipment, electrical appliances, aviation equipment, cameras, and construction. ML35 is a cold heading steel forming steel. ML35 is widely used in the production of fasteners, especially medium-strength bolts, screws, nuts, and pins.

[0003] High-end fields such as automobiles have strict quality requirements for fasteners, mainly because fasteners play a vital role in the application scenarios of high-end fields such as automobiles. The quality of fasteners is directly related to the safety, reliability and durability of the products. High-end fields such as automobiles often pursue zero defects in the quality requirements of fasteners. In order to meet the high quality requirements of high-end users, the traditional 8.8-grade fastener production process often adopts the large square billet two-fire material process route, which undoubtedly increases the manufacturing cost and carbon emissions of the manufacturing process. The carbon emissions of the billet opening process are generally above 500kg / ton.

[0004] With the implementation of the national dual carbon strategy and the rapid development of domestic new energy vehicles, competition in the automotive industry has intensified, and automobile manufacturers are paying more and more attention to the manufacturing cost and carbon emission indicators of steel. To this end, a medium carbon cold heading steel wire rod for 8.8 grade fasteners and its production method were developed. Summary of the invention

[0005] The present invention innovatively realizes the direct rolling of 240 square billets into finished products by redesigning the rolling process, reducing the intermediate billet opening step, and achieving the goals of reducing costs and carbon emissions while maintaining unchanged product quality.

[0006] The present invention adopts a new process innovation and adopts a large square billet direct rolling process to produce cold heading steel wire rods, thereby meeting the customer's needs for high quality, low cost and low carbon emissions.

[0007] In a first aspect, the present invention provides a medium carbon cold heading steel wire rod for 8.8 grade fasteners, comprising: the chemical element composition of the medium carbon cold heading steel wire rod is as follows by weight percentage: C 0.33-0.37%, Si 0.15-0.30%, Mn 0.70-0.90%, P≤0.015%, S≥0.010%, Cr≤0.20%, Ni≤0.20%, Cu≤0.20%, Mo≤0.10%, Al≥0.02%, N≤0.0060%, O≤0.0015%, and the rest is Fe and unavoidable impurities.

[0008] In a second aspect, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, which is applied to produce a medium carbon cold heading steel wire rod for 8.8 grade fasteners, comprising:

[0009] Step S1: raw material preparation, the raw materials include iron ore, alloy elements, slag forming agent, deoxidizer and carbonaceous material;

[0010] Iron ore, alloying elements, slag-making agents, deoxidizers and carbonaceous materials are selected as raw materials. These raw materials are properly stored after strict inspection and are ready for subsequent smelting.

[0011] Step S2: converter smelting, smelting the raw materials in a converter;

[0012] After the raw materials are ready, they are sent to the converter for smelting. The raw materials are melted at high temperature and undergo chemical reactions to eventually form preliminary molten steel, laying the foundation for subsequent refining processes.

[0013] Step S3: LF refining, performing LF refining on the molten steel after converter smelting to further adjust the chemical composition of the molten steel and remove impurities;

[0014] The molten steel after converter smelting enters the LF refining furnace. By adding alloy elements and adjusting smelting parameters, the chemical composition of the molten steel is controlled, impurities and excess gases are removed, and the quality of the molten steel is significantly improved.

[0015] Step S4: RH vacuum treatment, using RH vacuum treatment technology to vacuum degas the refined molten steel to remove gas and inclusions in the molten steel;

[0016] The refined molten steel is then subjected to RH vacuum treatment to further degas and remove inclusions, thereby improving the purity and quality stability of the molten steel and laying the foundation for the continuous casting process.

[0017] Step S5: bloom continuous casting, the refined and vacuum-treated molten steel is cast into blooms through a continuous casting machine, and the bloom cross-section is 240 mm×240 mm;

[0018] The molten steel after vacuum treatment is continuously cast into large square billets, and the size and shape are strictly controlled to meet the requirements of subsequent direct rolling into finished products.

[0019] Step S6: Finishing of the steel billet: Fully peeling and magnetic particle inspection are performed on the large square billet, and the steel billet is sent into the equipment to use mechanical action to peel off the oxide scale and impurities on its surface. After the oxide scale and impurities of the steel billet are removed, the surface of the steel billet is immediately cleaned to remove all residues, and a visual inspection is performed to ensure that there are no obvious defects on the surface. The steel billet is placed in the equipment for magnetization, and magnetic powder is evenly applied to the magnetized steel billet. The magnetic powder will be adsorbed to the defect to form a magnetic mark. By observing the magnetic mark, it is determined whether the steel billet has defects and the mark is recorded. Then, the steel billet is demagnetized to eliminate the residual magnetic field to obtain a finished steel billet;

[0020] After continuous casting, the large square billets are fully finished, including stripping of oxide scale and impurities, and visual and internal quality inspections to ensure that the billet surface is smooth and the internal quality is stable.

[0021] Step S7: heating, heating the finished steel billet to a temperature suitable for rolling, the temperature suitable for rolling is 1050-1150°C;

[0022] The finished billet is sent into the heating furnace and evenly heated to a temperature suitable for rolling, preparing for the subsequent rolling process.

[0023] Step S8: Controlling rolling, using 34 rolling mills to roll the heated steel billet according to a preset rolling coefficient and deformation amount, and controlling the sizing temperature at 820-850° C. to obtain a rolled wire rod;

[0024] The heated steel billet enters the rolling stage, where multiple rolling mills are used for controlled rolling to roll the large square billet into wire rod products that meet the requirements.

[0025] Step S9: controlled cooling. The rolled wire rod enters the controlled cooling stage and adopts a delayed cooling mode. The spinning temperature is controlled at 800-850°C and cooled through a Stelmor cooling line. During the cooling process of the rolled wire rod, the insulation cover remains fully covered and all fans are turned off. When the cooling of the rolled wire rod is completed, the rolled wire rod is removed from the cooling line to obtain the rolled and cooled wire rod.

[0026] The wire rod is immediately cooled after rolling, and a delayed cooling mode is adopted to ensure the stability of its structure and performance.

[0027] Furthermore, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, further comprising:

[0028] Step 10: Inspection: quality inspection of the rolled and cooled wire rods, including low center porosity, center porosity, ingot segregation, inclusions, decarburization layer depth, grain size, tensile strength, surface reduction, cold upsetting qualification and surface defects;

[0029] Step 11: Packaging: Packaging the qualified wire rods;

[0030] Step 12: Weighing and marking: weigh the packaged wire rods and mark relevant information;

[0031] Step 13: Warehouse, store the weighed and marked wire rods.

[0032] Finally, the wire rod undergoes subsequent processing steps such as quality inspection, packaging, weighing and marking, and warehousing and storage, and finally becomes a product that meets the standards.

[0033] Furthermore, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, which comprises, in step S9;

[0034] During the cooling process, the temperature change of the wire rod is monitored by an infrared thermometer, and the organizational transformation of the wire rod is monitored by a metallographic microscope. If an abnormal situation occurs during the monitoring process, the cooling parameters are adjusted to ensure product quality.

[0035] Furthermore, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, further comprising:

[0036] Waste slag recovery step, waste slag is generated during the LF refining process, the waste slag is collected by mechanical equipment, and is transported to the waste slag treatment area by mechanical equipment;

[0037] The collected waste residues are classified and processed to separate the recyclable waste residues, which include alloy elements and slag-forming agents. The recyclable waste residues are used for reuse;

[0038] For non-recyclable waste residue, solidify and landfill;

[0039] The wastewater treatment step collects the wastewater generated during the refining and continuous casting processes, introduces it into the wastewater treatment pool through the wastewater collection system, precipitates, filters and adsorbs the wastewater, removes oil, impurities and harmful substances in the wastewater, and tests the treated wastewater. It will be discharged or recycled after it meets the emission standards.

[0040] Furthermore, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, further comprising:

[0041] Waste gas generated during refining and continuous casting is collected and introduced into a waste gas treatment system through a waste gas collection pipeline. The waste gas is subjected to desulfurization, denitrification and dust removal treatments to obtain treated waste gas. The treated waste gas is tested to obtain the composition and properties of the waste gas, and the treated waste gas is reused as fuel based on its composition and properties.

[0042] Furthermore, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, which comprises, in step S8:

[0043] Preset rolling parameter setting: before starting rolling, obtain production process requirement information, set preset rolling coefficient and deformation amount according to the production process requirement information, and store the parameters in the controller;

[0044] Temperature monitoring and control: the controller monitors the temperature of the heated steel billet in real time through an infrared sensor. The temperature range of the steel billet temperature monitoring is 1050-1150℃. If the temperature is too low or too high, the controller automatically adjusts the heating or insulation to ensure that the steel billet enters the rolling mill at the best temperature;

[0045] Rolling process control: During the rolling process, the controller controls the running speed and reduction amount of the 34 rolling mills to make the rolling mills roll the steel billets according to the preset rolling coefficient and deformation amount. At the same time, the controller also controls the sizing temperature to be within the range of 820-850℃ to ensure the quality and performance of the wire rod.

[0046] The beneficial effects of the present invention are as follows:

[0047] Process innovation: Through the redesign of the rolling process, the present invention innovatively realizes the direct rolling of 240 square billets into finished products. This innovation reduces the traditional billet opening process, thereby simplifying the production process.

[0048] Cost reduction and emission reduction: Under the premise of maintaining product quality unchanged, by reducing the blanking process, the present invention achieves the goal of reducing manufacturing costs and reducing carbon emissions, which helps enterprises improve economic benefits while reducing negative impacts on the environment.

[0049] Stable product quality: The present invention ensures the stability and consistency of product quality by precisely controlling various parameters in the rolling process, such as rolling temperature, rolling coefficient and deformation, etc. The produced 8.8-grade medium carbon cold heading steel wire rod for fasteners has excellent mechanical properties and processing properties.

[0050] Resource recycling: The present invention also includes the steps of waste residue recovery, wastewater treatment and waste gas recovery and reuse. These measures not only help to reduce environmental pollution, but also achieve effective recycling of resources and further reduce production costs.

[0051] Intelligent control: By introducing an advanced control system, the present invention realizes intelligent control of the rolling process, thereby improving production efficiency and controllability of product quality.

[0052] In summary, the present invention achieves the multiple goals of reducing costs, reducing emissions and improving product quality through process innovation, resource recycling and utilization, and intelligent control. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] In order to more clearly illustrate the technical solution of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0054] Figure 1 A schematic diagram of a method flow chart provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0055] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The technical solutions provided by the embodiments of the present invention are described in detail below in conjunction with the drawings.

[0056] In a first aspect, the present invention provides a medium carbon cold heading steel wire rod for 8.8 grade fasteners, comprising: the chemical element composition of the medium carbon cold heading steel wire rod is as follows by weight percentage: C 0.33-0.37%, Si 0.15-0.30%, Mn 0.70-0.90%, P≤0.015%, S≥0.010%, Cr≤0.20%, Ni≤0.20%, Cu≤0.20%, Mo≤0.10%, Al≥0.02%, N≤0.0060%, O≤0.0015%, and the rest is Fe and unavoidable impurities.

[0057] See also Figure 1 In a second aspect, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, which is applied to produce a medium carbon cold heading steel wire rod for 8.8 grade fasteners, comprising:

[0058] Step S1: raw material preparation, the raw materials include iron ore, alloy elements, slag forming agent, deoxidizer and carbonaceous material;

[0059] Step S2: converter smelting, smelting the raw materials in a converter;

[0060] Step S3: LF refining, performing LF refining on the molten steel after converter smelting to further adjust the chemical composition of the molten steel and remove impurities;

[0061] LF refining is a kind of refining technology outside the furnace, the full name of which is Ladle Furnace refining. It is mainly used in the steel smelting process to further refine the primary molten steel to improve the quality and purity of the steel.

[0062] During the LF refining process, the primary molten steel is poured into a special ladle (or ladle), where it is then heated, stirred, and alloyed. This process can effectively remove impurities, adjust the chemical composition, and reduce the gas content in the steel, such as hydrogen, oxygen, and nitrogen. Through LF refining, the internal quality of the steel can be improved, its purity can be increased, and better raw materials can be provided for subsequent processing such as continuous casting or rolling.

[0063] LF refining furnace is usually equipped with electrode heating system, bottom blowing argon stirring system and alloy and slag adding system. The electrode heating system is used to heat the molten steel to maintain the appropriate refining temperature; the bottom blowing argon stirring system promotes the stirring and mixing of the molten steel by blowing argon into the bottom of the ladle, which is helpful for the chemical reaction and the removal of impurities; the alloy and slag adding system is used to add necessary alloy elements and slag-forming agents to the molten steel to adjust the chemical composition of the steel and improve the refining effect.

[0064] Step S4: RH vacuum treatment, using RH vacuum treatment technology to vacuum degas the refined molten steel to remove gas and inclusions in the molten steel;

[0065] RH vacuum treatment, full name Ruhrstahl-Heraeus vacuum treatment, is a secondary refining technology used in steel smelting. RH is the abbreviation of the German "Ruhrstahl-Heraeus", and this technology was jointly developed by the German companies Ruhrstahl and Heraeus.

[0066] During the RH vacuum treatment process, the molten steel is placed in a vacuum chamber and the ambient pressure is reduced by evacuation, so that the dissolved gases (such as hydrogen, nitrogen, etc.) and inclusions in the molten steel can be released more easily from the molten steel. This can significantly improve the purity and quality of the steel.

[0067] Specifically, RH vacuum treatment includes the following key steps:

[0068] Molten steel transfer: Molten steel after preliminary refining (such as LF refining) is transferred to the vacuum chamber of the RH vacuum treatment equipment.

[0069] Evacuation: Start the vacuum system and reduce the pressure in the vacuum chamber, usually to a vacuum degree of several millibars (mbar).

[0070] Removal of gases and inclusions: Under low pressure, the gas dissolved in the molten steel will quickly precipitate and form bubbles that float upwards. At the same time, non-metallic inclusions will be brought to the surface of the molten steel and then removed.

[0071] Treatment completed: When the gas and inclusion content in the molten steel is reduced to a predetermined level, the vacuum treatment process is completed and the molten steel is transferred to the next production link.

[0072] Key benefits of RH vacuum processing include:

[0073] Improved purity: Significantly improves steel purity by removing dissolved gases and inclusions.

[0074] Improve steel performance: Improved purity helps improve the mechanical properties, processing performance and corrosion resistance of steel.

[0075] Flexibility: RH vacuum treatment can be closely coordinated with the continuous casting machine to achieve fast-paced, continuous production.

[0076] RH vacuum treatment technology is widely used in the production of high-quality steel, especially for steel types that require strict control of gas content and inclusions, such as bearing steel, spring steel, stainless steel, etc. It is an indispensable part of the modern steel industry and plays an important role in improving the overall quality of steel.

[0077] Step S5: bloom continuous casting, the refined and vacuum-treated molten steel is cast into blooms through a continuous casting machine, and the bloom cross-section is 240 mm×240 mm;

[0078] Step S6: Finishing of the steel billet: Fully peeling and magnetic particle inspection are performed on the large square billet, and the steel billet is sent into the equipment to use mechanical action to peel off the oxide scale and impurities on its surface. After the oxide scale and impurities of the steel billet are removed, the surface of the steel billet is immediately cleaned to remove all residues, and a visual inspection is performed to ensure that there are no obvious defects on the surface. The steel billet is placed in the equipment for magnetization, and magnetic powder is evenly applied to the magnetized steel billet. The magnetic powder will be adsorbed to the defect to form a magnetic mark. By observing the magnetic mark, it is determined whether the steel billet has defects and the mark is recorded. Then, the steel billet is demagnetized to eliminate the residual magnetic field to obtain a finished steel billet;

[0079] Step S7: heating, heating the finished steel billet to a temperature suitable for rolling, the temperature suitable for rolling is 1050-1150°C;

[0080] Step S8: Controlling rolling, using 34 rolling mills to roll the heated steel billet according to a preset rolling coefficient and deformation amount, and controlling the sizing temperature at 820-850° C. to obtain a rolled wire rod;

[0081] Step S9: controlled cooling. The rolled wire rod enters the controlled cooling stage and adopts a delayed cooling mode. The spinning temperature is controlled at 800-850°C and cooled through a Stelmor cooling line. During the cooling process of the rolled wire rod, the insulation cover remains fully covered and all fans are turned off. When the cooling of the rolled wire rod is completed, the rolled wire rod is removed from the cooling line to obtain the rolled and cooled wire rod.

[0082] Specifically, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, further comprising:

[0083] Step 10: Inspection: quality inspection of the rolled and cooled wire rods, including low center porosity, center porosity, ingot segregation, inclusions, decarburization layer depth, grain size, tensile strength, surface reduction, cold upsetting qualification and surface defects;

[0084] Step 11: Packaging: Packaging the qualified wire rods;

[0085] Step 12: Weighing and marking: weigh the packaged wire rods and mark relevant information;

[0086] Step 13: Warehouse, store the weighed and marked wire rods.

[0087] Specifically, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, which comprises, in step S9;

[0088] During the cooling process, the temperature change of the wire rod is monitored by an infrared thermometer, and the organizational transformation of the wire rod is monitored by a metallographic microscope. If an abnormal situation occurs during the monitoring process, the cooling parameters are adjusted to ensure product quality.

[0089] Specifically, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, further comprising:

[0090] Waste slag recovery step, waste slag is generated during the LF refining process, the waste slag is collected by mechanical equipment, and is transported to the waste slag treatment area by mechanical equipment;

[0091] The collected waste residues are classified and processed to separate the recyclable waste residues, which include alloy elements and slag-forming agents. The recyclable waste residues are used for reuse;

[0092] For non-recyclable waste residue, solidify and landfill;

[0093] The wastewater treatment step collects the wastewater generated during the refining and continuous casting processes, introduces it into the wastewater treatment pool through the wastewater collection system, precipitates, filters and adsorbs the wastewater, removes oil, impurities and harmful substances in the wastewater, and tests the treated wastewater. It will be discharged or recycled after it meets the emission standards.

[0094] Specifically, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, further comprising:

[0095] Waste gas generated during refining and continuous casting is collected and introduced into a waste gas treatment system through a waste gas collection pipeline. The waste gas is subjected to desulfurization, denitrification and dust removal treatments to obtain treated waste gas. The treated waste gas is tested to obtain the composition and properties of the waste gas, and the treated waste gas is reused as fuel based on its composition and properties.

[0096] Specifically, the present invention provides a method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, which comprises, in step S8:

[0097] Preset rolling parameter setting: before starting rolling, obtain production process requirement information, set preset rolling coefficient and deformation amount according to the production process requirement information, and store the parameters in the controller;

[0098] Temperature monitoring and control: the controller monitors the temperature of the heated billet in real time through an infrared sensor. The temperature range of the billet temperature monitoring is 1050-1150°C. If the temperature is too low or too high, the controller automatically adjusts the heating or insulation to ensure that the billet enters the rolling mill at the optimal temperature.

[0099] Rolling process control: During the rolling process, the controller controls the running speed and reduction amount of the 34 rolling mills to make the rolling mills roll the steel billets according to the preset rolling coefficient and deformation amount. At the same time, the controller also controls the sizing temperature to be within the range of 820-850℃ to ensure the quality and performance of the wire rod.

[0100] The present invention innovatively realizes direct rolling of 240 square billets into finished products by redesigning the rolling process. The specific implementation method is as follows:

[0101] First, the present invention carefully selects high-quality raw materials such as iron ore and alloy elements in the raw material preparation stage to ensure the quality of the initial molten steel. In the links of converter smelting, LF refining and RH vacuum treatment, the present invention further adjusts the chemical composition of the molten steel and effectively removes impurities, gases and inclusions, thereby obtaining pure molten steel with qualified composition.

[0102] Next, the present invention adopts the bloom continuous casting technology to cast the refined and vacuum-treated molten steel into a 240mm×240mm bloom. The key to this step is to control the size and shape of the bloom to ensure that it can meet the requirements of subsequent direct rolling into products.

[0103] In the billet finishing stage, the present invention performs full peeling and magnetic particle inspection on the large square billet to remove the oxide scale and impurities on the surface and detect whether there are defects inside the billet. This step not only improves the surface quality of the billet, but also ensures the internal quality of the billet, laying a solid foundation for the subsequent rolling process.

[0104] Then, in the heating stage, the present invention heats the finished steel billet to a temperature range suitable for rolling of 1050-1150° C. The key to this step is to control the heating temperature and time to ensure that the steel billet can be evenly heated and reach a suitable rolling temperature.

[0105] In the controlled rolling stage, the present invention uses 34 rolling mills to roll the heated steel billet according to the preset rolling coefficient and deformation. By accurately controlling the running speed, reduction amount and other parameters of the rolling mill, the present invention successfully rolls the 240 square billet directly into finished products. The innovation of this step is that the traditional billet opening link is reduced, thereby simplifying the production process and reducing production costs. At the same time, since the energy consumption and waste emissions in the billet opening link are reduced, the goal of reducing carbon emissions is also achieved.

[0106] Finally, in the controlled cooling stage, the invention adopts a delayed cooling mode to cool the rolled wire rod. By monitoring the temperature change and structural transformation of the wire rod, the invention ensures product quality and improves the mechanical properties of the product.

[0107] In summary, the present invention realizes an innovative production method of directly rolling 240 square billets into products by redesigning the rolling process. This method not only reduces the intermediate billet opening link, reduces production costs and carbon emissions, but also maintains the stability and consistency of product quality.

[0108] The main difference between the present invention and the large square billet two-fire timber process route is that the present invention innovatively realizes the direct rolling of 240 square large square billets, thereby omitting the intermediate billet opening link. This innovation not only simplifies the production process, but also effectively reduces manufacturing costs and reduces carbon emissions while maintaining product quality. In contrast, the large square billet two-fire timber process route includes more production steps and higher costs. Therefore, the present invention better meets the market demand for high-quality, low-cost and low-carbon emission products through direct rolling technology.

[0109] The present invention realizes direct rolling of 240 square billets into products through a series of innovative production steps. These steps include:

[0110] Raw material preparation: Select appropriate iron ore, alloy elements, slag-forming agents, deoxidizers and carbonaceous materials to lay the foundation for the subsequent smelting process.

[0111] Converter smelting: The raw materials are smelted in the converter to form molten steel.

[0112] LF refining: Further refining of the molten steel after smelting to adjust the chemical composition of the molten steel and remove impurities to improve the purity of the steel.

[0113] RH vacuum treatment: Use vacuum treatment technology to remove gas and inclusions in molten steel to further improve steel quality.

[0114] Continuous casting machine casting: The refined and vacuum-treated molten steel is cast into large square billets through a continuous casting machine.

[0115] Billet finishing: The large square billet is fully peeled and subjected to magnetic particle inspection to ensure that there are no obvious defects on the surface, providing guarantee for the subsequent rolling process.

[0116] Heating: Heat the finished billet to a temperature suitable for rolling to prepare for the rolling process.

[0117] Rolling: 34 rolling mills are used to roll the heated steel billets to directly obtain the rolled wire rods without the need for billet opening.

[0118] Controlled cooling: The rolled wire rod is cooled in a controlled manner, and a delayed cooling mode is adopted to ensure the structure and performance of the product.

[0119] The above steps not only simplify the production process, but also reduce manufacturing costs and carbon emissions, while maintaining product quality and realizing direct rolling of large square billets into finished products.

[0120] The main technical indicators of the medium carbon cold heading steel wire rod for 8.8 grade fasteners of the present invention are equivalent to those of the two-fire cold heading steel wire rod. The wire rod has low-power general looseness, central looseness and ingot segregation ≤0.5 level; inclusion A+B+C+D fine system ≤5 level, DS ≤1.5 level; total decarburization layer depth ≤0.7%D; grain size 9-10 level; 1 / 3 cold forging qualified; tensile strength 560-620MPa, surface reduction rate ≥50%; surface defect depth ≤0.05mm, meeting the low-cost and high-quality requirements of high-end customers.

[0121] In the traditional process, after the large square billet is cast, it is usually necessary to carry out initial rolling to open the billet, roll the large square billet into an intermediate billet with a smaller cross-section, and then heat it to the rolling temperature again for final rolling. However, the innovative method of the present invention realizes the direct rolling of the 240 square large square billet into finished products.

[0122] The technical solution of the present invention omits the process of opening the billet, and directly casts the refined and vacuum-treated large square billets into 240mm×240mm large square billets through a continuous casting machine. The finished large square billets are directly heated to a temperature suitable for rolling (1050-1150°C), and then rolled using 34 rolling mills according to preset parameters to obtain the final size of the wire rod in one step.

[0123] The present invention reduces the number of heating times. The traditional process requires two heating processes, while the innovative method of the present invention only requires one heating process, thereby significantly reducing energy consumption.

[0124] The present invention reduces equipment use time and labor costs by omitting the blanking step, and also reduces metal loss caused by blanking.

[0125] The present invention also brings significant environmental benefits. By reducing the number of heating times and omitting the process of opening the blank, the present invention successfully reduces carbon emissions. Specifically, the combustion of fuel used in the heating process will produce carbon emissions, and each heating will increase this part of emissions. Therefore, reducing the number of heating times directly reduces carbon emissions. At the same time, the operation of equipment such as the blank opening machine and intermediate transportation will also produce indirect carbon emissions.

[0126] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A medium carbon cold heading steel wire rod for 8.8 grade fasteners, characterized in that: include: The chemical element composition of the medium carbon cold heading steel wire rod is as follows by weight percentage: C 0.33-0.37%, Si 0.15-0.30%, Mn 0.70-0.90%, P≤0.015%, S≥0.010%, Cr≤0.20%, Ni≤0.20%, Cu≤0.20%, Mo≤0.10%, Al≥0.02%, N≤0.0060%, O≤0.0015%, and the rest is Fe and unavoidable impurities.

2. A method for producing a medium carbon cold heading steel wire rod for 8.8 grade fasteners, applied to produce the medium carbon cold heading steel wire rod for 8.8 grade fasteners as claimed in claim 1, characterized in that: include; Step S1: raw material preparation, the raw materials include iron ore, alloy elements, slag forming agent, deoxidizer and carbonaceous material; Step S2: converter smelting, smelting the raw materials in a converter; Step S3: LF refining, performing LF refining on the molten steel after converter smelting to further adjust the chemical composition of the molten steel and remove impurities; Step S4: RH vacuum treatment, using RH vacuum treatment technology to vacuum degas the refined molten steel to remove gas and inclusions in the molten steel; Step S5: bloom continuous casting, the refined and vacuum-treated molten steel is cast into blooms through a continuous casting machine, and the bloom cross-section is 240 mm×240 mm; Step S6: Finishing of the steel billet: Fully peeling and magnetic particle inspection are performed on the large square billet, and the steel billet is sent into the equipment to use mechanical action to peel off the oxide scale and impurities on its surface. After the oxide scale and impurities of the steel billet are removed, the surface of the steel billet is immediately cleaned to remove all residues, and a visual inspection is performed to ensure that there are no obvious defects on the surface. The steel billet is placed in the equipment for magnetization, and magnetic powder is evenly applied to the magnetized steel billet. The magnetic powder will be adsorbed to the defect to form a magnetic mark. By observing the magnetic mark, it is determined whether the steel billet has defects and the mark is recorded. Then, the steel billet is demagnetized to eliminate the residual magnetic field to obtain a finished steel billet; Step S7: heating, heating the finished billet to a temperature suitable for rolling, the temperature suitable for rolling is 1050-1150°C; Step S8: Controlling rolling, using 34 rolling mills to roll the heated steel billet according to a preset rolling coefficient and deformation amount, and controlling the sizing temperature at 820-850° C. to obtain a rolled wire rod; Step S9: controlled cooling. The rolled wire rod enters the controlled cooling stage and adopts a delayed cooling mode. The spinning temperature is controlled at 800-850°C and cooled through a Stelmor cooling line. During the cooling process of the rolled wire rod, the insulation cover remains fully covered and all fans are turned off. When the cooling of the rolled wire rod is completed, the rolled wire rod is removed from the cooling line to obtain the rolled and cooled wire rod.

3. The method for producing medium carbon cold heading steel wire rod for 8.8 grade fasteners according to claim 2, characterized in that: Also includes; Step 10: Inspection: quality inspection of the rolled and cooled wire rods, including low-power general porosity, center porosity, ingot segregation, inclusions, decarburization layer depth, grain size, tensile strength, surface reduction, cold upsetting qualification and surface defects; Step 11: Packaging: Packaging the qualified wire rods; Step 12: Weighing and marking: weigh the packaged wire rods and mark relevant information; Step 13: Warehouse, store the weighed and marked wire rods.

4. The method for producing medium carbon cold heading steel wire rod for 8.8 grade fasteners according to claim 2, characterized in that: In step S9, it includes: During the cooling process, the temperature change of the wire rod is monitored by an infrared thermometer, and the organizational transformation of the wire rod is monitored by a metallographic microscope. If an abnormal situation occurs during the monitoring process, the cooling parameters are adjusted to ensure product quality.

5. The method for producing medium carbon cold heading steel wire rod for 8.8 grade fasteners according to claim 2, characterized in that: Also includes; Waste slag recovery step, waste slag is generated during the LF refining process, the waste slag is collected by mechanical equipment, and is transported to the waste slag treatment area by mechanical equipment; The collected waste residues are classified and processed to separate the recyclable waste residues, which include alloy elements and slag-forming agents. The recyclable waste residues are used for reuse; For non-recyclable waste residue, solidify and landfill; The wastewater treatment step collects the wastewater generated during the refining and continuous casting processes, introduces it into the wastewater treatment pool through the wastewater collection system, precipitates, filters and adsorbs the wastewater, removes oil, impurities and harmful substances in the wastewater, and tests the treated wastewater. It will be discharged or recycled after it meets the emission standards.

6. The method for producing medium carbon cold heading steel wire rod for 8.8 grade fasteners according to claim 2, characterized in that: Also includes; Waste gas generated during refining and continuous casting is collected and introduced into a waste gas treatment system through a waste gas collection pipeline. The waste gas is subjected to desulfurization, denitrification and dust removal treatments to obtain treated waste gas. The treated waste gas is tested to obtain the composition and properties of the waste gas, and the treated waste gas is reused as fuel based on its composition and properties.

7. The method for producing medium carbon cold heading steel wire rod for 8.8 grade fasteners as claimed in claim 2, characterized in that: In step S8, it includes: Preset rolling parameter setting: before starting rolling, obtain production process requirement information, set preset rolling coefficient and deformation amount according to the production process requirement information, and store the parameters in the controller; Temperature monitoring and control: the controller monitors the temperature of the heated steel billet in real time through an infrared sensor. The temperature range of the steel billet temperature monitoring is 1050-1150℃. If the temperature is too low or too high, the controller automatically adjusts the heating or insulation to ensure that the steel billet enters the rolling mill at the best temperature; Rolling process control: During the rolling process, the controller controls the operating speed and reduction amount of the 34 rolling mills to make the rolling mills roll the steel billets according to the preset rolling coefficient and deformation amount. At the same time, the controller also controls the sizing temperature to be within the range of 820-850℃ to ensure the quality and performance of the wire rod.