Efficient metal ytterbium target material production process

By carefully selecting raw materials, vacuum melting and directional solidification, and precision machining, the problems of low production efficiency and unstable quality of ytterbium metal have been solved, producing high-purity, high-density ytterbium metal targets to meet the application needs of high-end electronic devices.

CN118996350APending Publication Date: 2024-11-22ZHIDONG TIANDI (BEIJING) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121125.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing ytterbium production processes suffer from low production efficiency and unstable product quality, making it difficult to meet the demands of high-end applications.

Method used

By employing carefully selected raw materials, vacuum melting and directional solidification, mechanical processing, and precision machining steps, and strictly controlling process parameters, high-purity, high-density metallic ytterbium targets with excellent crystalline structure are produced.

Benefits of technology

It improves the production efficiency and product quality of ytterbium sputtering targets, meets the application needs of high-end fields such as semiconductors and OLED displays, reduces power consumption, and improves device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996350A_ABST
    Figure CN118996350A_ABST
Patent Text Reader

Abstract

The invention discloses an efficient production process of a metal ytterbium target material. The invention belongs to the technical field of metal material preparation, the technology comprises the steps of raw material selection, vacuum melting directional solidification, mechanical treatment and precision machining, and the metal ytterbium target material with high purity, high density and excellent crystal structure is produced by strictly controlling technological parameters of all links. The application requirements of high-end fields such as semiconductors and oled display are met; the production efficiency and the product quality of the metal ytterbium target material are improved, and the method has good market application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material preparation, and specifically refers to an efficient production process of metal ytterbium target material. Background Art

[0002] With the deepening of modern engineering application research, ytterbium sensors have broad application prospects in many fields such as aerospace, military, and oil exploration. Metal ytterbium has low hardness and good cold processing performance, and can be processed into wide and thin foils. However, metal ytterbium is a rare earth metal, and has disadvantages such as high activity and easy oxidation during processing. To ensure the purity of the finished foil, the processing is difficult.

[0003] Ytterbium targets have important applications in electronics, semiconductors, optics, etc. However, the existing production process has problems such as low production efficiency, unstable product quality, and performance that cannot meet the needs of high-end applications. Summary of the invention

[0004] The purpose of the present invention is to provide an efficient metal ytterbium target production process, including raw material selection, vacuum melting and directional solidification, mechanical treatment and precision processing steps. By strictly controlling the process parameters of each link, a metal ytterbium target with high purity, high density and excellent crystalline structure is produced to meet the application needs of high-end fields such as semiconductors and OLED displays, improve the production efficiency and product quality of the metal ytterbium target, and have good market application prospects.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: an efficient metal ytterbium target production process, the production process comprising the following steps:

[0006] (1) Raw material selection: Select ytterbium metal raw materials of a certain purity, conduct strict component analysis and impurity detection, shear and load them into a specially made cylindrical mold, and then extrude them to make the raw materials evenly filled in the mold to form a green billet;

[0007] (2) Vacuum melting (heat treatment): Place the green embryo in a special impurity filtering and processing box, put it into a vacuum heat treatment furnace, evacuate it, and gradually increase the temperature in four sections. The temperature is raised to 1200 degrees for melting to densify the green embryo, ensure that the raw materials are fully melted and evenly mixed, and make the impurities adsorbed on the surface of the filtering box. The metal ytterbium with a purity of more than 99.99% and a total impurity element content of less than 80 ppm is obtained in the mold;

[0008] (3) Directional solidification: After the smelting is completed, high-purity argon gas is introduced for gas protection after cooling and solidification treatment to effectively control the entry of other impurity elements such as oxygen and hydrogen, so as to ensure that there are no pores inside the target material and no shrinkage holes on the surface. The metal ytterbium forms a columnar structure in the mold, which improves the crystal orientation and performance of the target material. The uniformity and high density of the target material have a density of 6.972-6.98 g / cm3 and a grain size of 0.5-2 μm.

[0009] (4) Mold removal: Using lathe equipment, the solidified material is molded with a special tool and cut into blank materials of the required height;

[0010] (5) Precision machining: Use CNC equipment to precisely machine the blank of the required size into a target of the required size;

[0011] (6) Cleaning, inspection, and packaging: The processed target material is wiped clean with anhydrous alcohol to remove tiny processing debris, and the qualified target material is vacuum-packaged in a vacuum bag.

[0012] Preferably, the purity of the ytterbium metal selected in step (1) is not less than 99.99%.

[0013] Preferably, the columnar mold used in step (1) should be cleaned.

[0014] Preferably, the pressure of the extrusion treatment in step (1) is 100-200 MPa.

[0015] Preferably, the vacuum degree in the vacuum heat treatment furnace in step (2) is -5 to -10 Pa.

[0016] Preferably, the smelting time in step (2) is 2-6 hours.

[0017] Preferably, the temperature of the solidification treatment in step (3) is lowered to 500 degrees and high-purity argon gas is introduced.

[0018] Preferably, the high-purity argon in step (3) cannot be replaced by nitrogen.

[0019] Preferably, the solidification rate in step (3) is 1-10 mm / min.

[0020] Preferably, in step (5), the surface roughness Ra of the target material is less than 1.5 micrometers.

[0021] Furthermore, all the above steps need to be performed when the air humidity is below 40%.

[0022] The beneficial effects achieved by the present invention using the above structure are as follows:

[0023] (1) The process of the present invention includes raw material selection, vacuum melting and directional solidification, mechanical treatment and precision processing steps. By strictly controlling the process parameters of each link, a metal ytterbium target with high purity, high density and excellent crystalline structure is produced to meet the application requirements of high-end fields such as semiconductors and OLED displays.

[0024] (2) The inconsistency between the work function of the gate material and the substrate material will cause electron flow and form an electric field. If the work function of the gate material is higher than that of the substrate, the electrons will flow from the gate to the substrate region, forming an electric field pointing from the gate to the substrate. This electric field enhances the effect of the gate voltage and improves the utilization rate of the gate voltage, so that a lower gate voltage can be used while maintaining the device performance unchanged, thereby reducing power consumption. Before this application, a Yb nanometal thin layer is deposited to reduce the cathode work function, reduce the contact barrier, and improve device efficiency;

[0025] Among them, the charge transfer balance,

[0026] The work function value of Yb is between 2.5eV and 3eV;

[0027] The work function value of Ag is between 4.26-4.74ev.

[0028] (3) The present invention improves the production efficiency and product quality of metal ytterbium targets and has good market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Roughness of Ytterbium metal target.

[0030] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0032] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0033] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials and test strains used in the following examples are purchased from commercial channels unless otherwise specified.

[0034] Example 1

[0035] Raw material selection

[0036] The metal ytterbium raw material with a purity of not less than 99.99% is selected, and strict component analysis and impurity detection are carried out. It is sheared and loaded into a specially made cylindrical mold (after cleaning), and then extruded (pressure is 100-200MPa) to make the raw material evenly filled in the mold to form a green billet.

[0037] Example 2

[0038] Vacuum melting (heat treatment)

[0039] The green embryo is placed in a special impurity filtering and processing box, and then placed in a vacuum heat treatment furnace with a vacuum degree better than 10-3Pa. The vacuum is evacuated to a vacuum degree of -5 to -10Pa, and the temperature is gradually increased in four intervals. The temperature is increased to 1200 degrees for smelting, and the smelting time is 2-6 hours to densify the green embryo, ensure that the raw materials are fully melted and evenly mixed, and that the impurities are adsorbed on the surface of the filtering box, so that the metal ytterbium with a purity of more than 99.99% and a total impurity element content of less than 80ppm is obtained in the mold.

[0040] Example 3

[0041] Directional solidification

[0042] After the smelting is completed, the temperature is cooled down to 500 degrees and then high-purity argon is connected for gas protection to effectively control the entry of other impurity elements such as oxygen and hydrogen, and the solidification rate is controlled at 1-10mm / min, so as to ensure that there are no pores inside the target material and no shrinkage holes on the surface. The metal ytterbium forms a columnar structure in the mold, which improves the crystal orientation and performance of the target material. The uniformity and high density of the target material are 6.972-6.98 g / cm3, and the grain size of the mold blank is between 0.5-2 microns.

[0043] Example 4

[0044] Mold Removal

[0045] Using lathe equipment, the solidified material is removed from the mold with a special tool and cut into blank materials of the required height.

[0046] Example 5

[0047] Precision Machining

[0048] Using CNC equipment, the blank of the required size is precisely processed into the target of the required size, ensuring that the surface roughness Ra of the target is less than 1.5 microns.

[0049] Example 6

[0050] Cleaning, inspection, and packaging: The processed target is wiped clean with anhydrous alcohol to remove tiny processing debris, and the qualified target is vacuum-packed in a vacuum bag according to the indicators in Table 1.

[0051] Table 1 Target material qualification criteria

[0052]

[0053] Experimental Example 1

[0054] A batch of 100 samples of metal ytterbium targets prepared by the preparation process of the present invention were selected, and 9 of them were selected as test samples, 3 in a group, and randomly divided into three groups, which were recorded as groups A, B, and C. The surface roughness of group A, group B, and group C was tested using a metal surface roughness measuring instrument, and the average value was taken.

[0055] Result analysis: Figure 1 As shown, the average roughness of groups A, B and C are all at a low level, and are all less than 1.5 microns, which can meet the application requirements of high-end fields.

[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0057] The present invention and its embodiments are described above, and such description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design a structure and embodiment similar to the technical solution without creativity, which should belong to the protection scope of the present invention.

Claims

1. An efficient metal ytterbium target production process, characterized by: The production process comprises the following steps: (1) Raw material selection: Select ytterbium metal raw materials, conduct component analysis and impurity detection, shear and load them into a cylindrical mold, and then extrude them to make the raw materials evenly filled in the mold to form a green billet; (2) Vacuum melting: Place the green embryo in an impurity filtering treatment box, put it into a vacuum heat treatment furnace, evacuate it, and gradually increase the temperature in four sections until the temperature reaches 1200 degrees for melting to densify the green embryo, ensure that the raw materials are fully melted and evenly mixed, and allow impurities to be adsorbed on the surface of the filtering box, so that metal ytterbium with a purity of more than 99.99% and a total impurity element content of less than 80 ppm is obtained in the mold; (3) Directional solidification: After the smelting is completed, high-purity argon gas is introduced for gas protection after cooling and solidification treatment to control the entry of oxygen, hydrogen and other impurities, so as to ensure that there are no pores inside the target material and no shrinkage holes on the surface. The metal ytterbium forms a columnar structure in the mold with a density of 6.972-6.98 g / cm3 and a grain size of 0.5-2 μm. (4) Mold removal: Using lathe equipment, the solidified material is molded with a special tool and cut into blank materials of the required height; (5) Precision machining: Use CNC equipment to precisely machine the blank of the required size into a target of the required size; (6) Cleaning, inspection, and packaging: The processed target material is wiped clean with anhydrous alcohol to remove tiny processing debris, and the qualified target material is vacuum-packaged in a vacuum bag.

2. The efficient metal ytterbium target production process according to claim 1, characterized in that: The purity of the ytterbium metal selected in step (1) is not less than 99.99%.

3. The efficient metal ytterbium target production process according to claim 2, characterized in that: The columnar mold used in the step (1) should be cleaned.

4. The efficient metal ytterbium target production process according to claim 3, characterized in that: The pressure of the extrusion treatment in step (1) is 100-200 MPa.

5. The efficient metal ytterbium target production process according to claim 4, characterized in that: The vacuum degree in the vacuum heat treatment furnace in step (2) is -5 to -10 Pa.

6. The efficient metal ytterbium target production process according to claim 5, characterized in that: The smelting time in step (2) is 2-6 hours.

7. The efficient metal ytterbium target production process according to claim 6, characterized in that: The temperature of the solidification treatment in step (3) is lowered to 500 degrees and high-purity argon gas is introduced. The high-purity argon gas in step (3) cannot be replaced by nitrogen.

8. The efficient metal ytterbium target production process according to claim 7, characterized in that: The solidification rate in step (3) is 1-10 mm / min.

9. The efficient metal ytterbium target production process according to claim 8, characterized in that: The surface roughness Ra of the target material in step (5) is less than 1.5 microns.

10. The efficient metal ytterbium target production process according to claim 9, characterized in that: The production process needs to be carried out when the air humidity is below 40%.