Flexible metal-metal oxide / conducting layer confinement composite nanofiber membrane for X-ray shielding and preparation method of flexible metal-metal oxide / conducting layer confinement composite nanofiber membrane
By combining electrospinning and hydrothermal synthesis technology in nanofiber membranes, the interface boundary structure is constructed, and the problems of heavy and harmful substances of existing X-ray shielding materials are solved, achieving high efficiency , lightweight, flexible and environmentally friendly X-ray shielding effect.
Patent Information
- Application Number
- CN202411120990.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
The existing X-ray shielding materials are heavy, bulky and contain harmful substance lead. The flexible and lightweight non-toxic materials have not been effectively developed, making it difficult to meet the efficient shielding needs for X-rays.
Electrospinning technology is used to load conductive multi-wall carbon nanotubes inside and outside the nanofiber, and the electrospinned nanofiber membrane is constructed to form an interface by hydrothermal synthesis and continuous ion layer adsorption reduction method. The limiting effect is used to enhance the X-ray shielding performance.
The prepared metal-metal oxide/conductive layer limited-domain composite nanofiber membrane is lightweight and flexible, and can achieve efficient X-ray shielding at low cost, with a mass attenuation coefficient of more than 85%, avoiding the risk of using harmful lead materials.
Smart Images

Figure CN118996841A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of X-ray shielding materials, and in particular relates to a flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding and a preparation method thereof. Background Art
[0002] X-rays are electromagnetic waves with extremely short wavelengths, extremely high frequencies, high energy, and strong penetrating power. Its wavelength is about 0.001 to 100nm, and its energy is as high as 0.1 to 10GeV. With the deepening and development of X-ray research, X-rays are widely used in various fields such as hospitals, semiconductor processing, electronic components, nuclear industry, and aerospace industry. For example, transmission imaging, tomography, and cardiovascular shaping technology used in hospitals all use X-rays, while space exploration, nuclear power generation, and nuclear weapons are inseparable from X-rays. Workers who are exposed to X-rays for a long time will suffer great harm to their bodies, which can inhibit, damage, or even necrotize biological cells, causing different degrees of pathological changes in the body. The development of X-ray shielding materials is imperative.
[0003] Literature shows that the existing X-ray shielding medical clothing is mainly made of lead-containing vulcanized rubber with a thickness of 2.5 to 5 mm. Its disadvantage is that it has strong X-ray scattering, and each piece weighs more than 15 kg. It is heavy, bulky, airtight, and uncomfortable. In addition, lead is toxic and is not conducive to contact with the skin. The waste has a great impact on the environment. Therefore, the search for a flexible, lightweight, non-toxic X-ray shielding material has continuously attracted the attention of scientists.
[0004] In 2017, Wang Ce's team from Jilin University selected Ag, Bi2WO6, and BiOX (X=CI\Br\I) to compound with tungsten oxide respectively, and used chemical deposition method to make them grow on PAN-PU nanofiber membrane loaded with silver seeds to obtain electrospun composite nanofiber membrane. At 30keV, the attenuation rate of X-ray energy can reach 70-90% with different membrane thickness (ZL 2017 10051718.7; ADVANCED MATERIALS INTERFACES, 8, 7, 2021; COMMUNICATIONS MATERIALS, 2, 1, 2021; ACS APPLIED NANO MATERIALS, vol 5(3), 4157-69, 2022). The reason is that electrospun composite nanofibers have large specific surface area and high porosity, and inorganic nanoparticles are conducive to the absorption of X-rays and make it difficult for incident X-rays to overflow. Effective X-ray shielding can be achieved through multiple absorption and reflection. However, the use of carbon materials (such as carbon nanotubes, graphene, etc.) and high atomic number bismuth nanoparticles to further restrict the flow and overflow of electrons, that is, electrospun nanocomposites with confinement effects have not yet been involved. Summary of the invention
[0005] The object of the present invention is to provide a flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding and a preparation method thereof.
[0006] The metal-metal oxide / conductive layer confined composite nanofiber membrane of the present invention is a nanofiber membrane material filled with conductive aggregates by loading conductive multi-walled carbon nanotubes (MWCNT) inside and outside the nanofibers through electrostatic spinning technology; then the high atomic number element W oxide and Bi nanoparticles are loaded on the outer layer of the fiber respectively by hydrothermal synthesis and continuous ion layer adsorption reduction method, forming an interface constraint, and constructing a multilayer nanostructured material of MWCNT, Bi single substance and W-based compound loaded by electrospun nanofiber membrane. An interface confinement effect is generated between the three inorganic components, and a heterojunction is formed between the MWCNT and the W layer, which can enhance the transfer and separation of photogenerated charges at the contact interface, and the Schottky contact between the W layer and the Bi layer will cause electrons to move from the W layer to the Bi layer, thereby effectively increasing the electron density of the outermost Bi layer, further enhancing the photoelectric effect, and improving the material's shielding performance against X-rays. After the layers of composite membranes are stacked layer by layer, a confined composite nanofiber membrane material for X-ray shielding is prepared. The composite nanofiber membrane is light and has excellent flexibility, but when the MWCNT exceeds 15wt% of the composite membrane weight, the composite membrane will crack.
[0007] The method for preparing a flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding described in the present invention comprises the following steps:
[0008] (1) Preparation of MWCNT-filled polymer nanofiber membrane by high-voltage electrospinning: 0.027-0.12 g MWCNT was ultrasonically dispersed in 6-8 g N, N-dimethylformamide (DMF) is added to obtain a dispersion; then 0.8-0.9g of polyacrylonitrile (PAN) is dissolved in the dispersion, and the spinning precursor solution is obtained by stirring; the spinning solution is extracted with a syringe, and the syringe is fixed on a propulsion pump, and the syringe is provided with a stainless steel needle with a diameter of 0.8-1.2mm; the positive electrode of the high-voltage power supply is connected to the needle, and the negative electrode is connected to a roller covered with silicone oil paper, the positive electrode voltage is set to 7-14kV, the negative electrode voltage is set to -4--10kV, the receiving distance is set to 10-15cm, the propulsion speed of the propulsion pump stepper motor is set to 0.5-1.0mL / h, the roller speed is 300-1000r / min, the ambient temperature is 20-25℃, the ambient humidity is 30%-50%, and the fiber membrane is collected after spinning for 4-15h and placed in a 45-65℃ oven for drying for 5-10h to obtain a MWCNT-filled polymer nanofiber membrane, which is recorded as a MWCNT / PAN composite nanofiber membrane;
[0009] (2) Solvothermal reaction: 1-2 g of tungsten chloride is dissolved in 150-300 mL of anhydrous ethanol and transferred to a polytetrafluoroethylene liner. The MWCNT / PAN composite nanofiber membrane obtained in step (1) is cut into a size of (8-10) cm×(8-10) cm and completely immersed in the above solution. The polytetrafluoroethylene liner is then placed in a reactor and sealed and heated at 160-200° C. for 4-15 h. After the reactor is naturally cooled to room temperature, the nanofiber membrane is taken out and cleaned with anhydrous ethanol and deionized water in ultrasound in turn, and then placed in a 45-55° C. oven for drying for 1.5-3.0 h to obtain W 18 O 49 / MWCNT / PAN composite nanofiber membrane;
[0010] (3) Continuous ion layer adsorption reduction reaction: prepare 60-200 mL of 10-50 mmol / L potassium bismuth citrate aqueous solution, referred to as solution A; then prepare 60-200 mL of 10-50 mmol / L KBH4 solution, referred to as solution B; 18 O 49 The / MWCNT / PAN composite nanofiber membrane was immersed in solution A for 1 to 3 minutes and then rinsed with deionized water to remove excess Bi. 3+ ions; then the nanofiber membrane is immersed in solution B for 1 to 3 minutes to generate Bi nanostructures on the surface of the nanofibers, and then removed and rinsed with deionized water to remove excess BH4 - ions; the above "immersing in solution A-taking out-immersing in solution B-taking out" process is a continuous ion layer adsorption reaction (SILAR) cycle, and the loading amount of Bi nanoparticles is adjusted by the number of cycles, and the number of cycles is set to 8 to 16 times. Finally, the obtained nanofiber membrane is cleaned with anhydrous ethanol and deionized water in ultrasound in turn, and then placed in an oven at 45 to 55°C for 1.5 to 3.0 hours to obtain a BWCP composite nanofiber membrane, that is, the flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding described in the present invention.
[0011] The advantage of the present invention is that the BWCP composite nanofiber membrane for X-ray shielding is prepared by combining electrospinning technology with two post-treatment methods: solvent thermal reaction and continuous ion layer adsorption reduction reaction. The method is simple to operate, safe to use, and low in cost. The metal elements W and Bi used are much cheaper than elements such as silver. At the same time, the method has great flexibility and can achieve different composition structures and properties by changing the reaction conditions, which is conducive to meeting different usage requirements. The metal-metal oxide / conductive layer confined composite nanofiber membrane prepared by the present invention has a multi-layer inorganic nanostructure and is well dispersed. Interface constraints are formed between layers, resulting in an interface confinement effect. MWCNT and W18 O 49 The heterojunction between Bi and W 18 O 49 The Schottky contact between the two effectively enhances the photoelectric effect of the composite film and improves the shielding effect of the material against X-rays. When accumulated to a certain thickness, it can achieve a shielding effect similar to that of traditional X-ray shielding materials. Test data show that the mass attenuation coefficient of the BWCP composite nanofiber membrane containing 12% MWCNT prepared by the above method (corresponding to Example 3) can reach 15.85cm at an X-ray photon energy of 33keV. 2 / g; when the composite film is increased to 4.24mm thick by simply stacking multiple films, the X-ray shielding rate at 33keV energy can reach more than 85%. At the same time, the composite film is lightweight, with a density of only 0.36g / cm 3 It is flexible and can be folded and bent repeatedly without being damaged, and avoids the use of traditional X-ray shielding materials such as lead, which is highly toxic. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 This is the mass attenuation coefficient curve of the BWCP-3 composite nanofiber membrane prepared in Example 1 of the present invention for X-ray photon energies of 33keV, 48keV, 65keV, 83keV, and 100keV.
[0013] Figure 2 This is the X-ray shielding rate curve of the BWCP-3 composite nanofiber membrane prepared in Example 1 of the present invention for X-ray photon energies of 33keV, 48keV, 65keV, 83keV, and 100keV.
[0014] Figure 3 This is the mass attenuation coefficient curve of the BWCP-6 composite nanofiber membrane prepared in Example 2 of the present invention for X-ray photon energies of 33keV, 48keV, 65keV, 83keV, and 100keV.
[0015] Figure 4 This is the X-ray shielding rate curve of the BWCP-6 composite nanofiber membrane prepared in Example 2 of the present invention for X-ray photon energies of 33keV, 48keV, 65keV, 83keV, and 100keV.
[0016] Figure 5 This is the mass attenuation coefficient curve of the BWCP-12 composite nanofiber membrane prepared in Example 3 of the present invention for X-ray photon energies of 33keV, 48keV, 65keV, 83keV, and 100keV.
[0017] Figure 6These are the X-ray shielding rate curves of the BWCP-12 composite nanofiber membrane prepared in Example 3 of the present invention for X-ray photon energies of 33keV, 48keV, 65keV, 83keV, and 100keV at thicknesses of 0.51mm, 1.04mm, 2.15mm, 3.16mm, and 4.24mm, respectively.
[0018] Figure 7 This is a scanning electron microscope image of the BWCP-12 composite nanofiber membrane prepared in Example 3 of the present invention;
[0019] Figure 8 These are flexible optical photographs of the folding, restoration, and refolding of the BWCP-12 composite nanofiber membrane prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0020] The following examples will further illustrate the present invention. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of protection of the present invention.
[0021] Example 1
[0022] (1) Take 0.027g of MWCNT and add it to a beaker containing 7.12g of N,N-dimethylformamide (DMF). After ultrasonic dispersion for 1h, dissolve 0.88g of polyacrylonitrile (PAN) in the dispersion and stir magnetically for 10h to obtain a spinning precursor solution. Use a 10mL syringe to extract the spinning solution and fix the syringe on a propulsion pump with a 1mm diameter stainless steel needle. Connect the positive electrode of the high-voltage power supply to the needle and the negative electrode to a roller covered with silicone oil paper. The positive electrode voltage is set to 6kV, the negative electrode voltage is set to -10kV, the receiving distance is fixed to 10cm, the propulsion speed of the propulsion pump stepper motor is set to 0.6mL / h, the roller speed is 400r / min, the ambient temperature is 20℃, the ambient humidity is 40%, and after spinning for 12h, the fiber membrane is collected and placed in a 60℃ oven for drying for 5h to obtain a MWCNT-filled polymer nanofiber membrane, which is recorded as a MWCNT / PAN-3 composite nanofiber membrane.
[0023] (2) 1.5 g of WCl6 was added to a 300 mL polytetrafluoroethylene liner containing 200 mL of anhydrous ethanol. The MWCNT / PAN-3 composite nanofiber membrane obtained in step (1) was cut into a size of 9×9 cm and completely immersed in the above solution. The liner was then placed in a reactor and sealed and heated in an oven at 170°C for 11 h. After the reactor was naturally cooled to room temperature, the fiber membrane was taken out and cleaned with anhydrous ethanol and deionized water in ultrasound in turn, and then dried in an oven at 50°C for 2 h to obtain W 18 O 49 / MWCNT / PAN-3 composite nanofiber membrane;
[0024] (3) Prepare 100 mL of 40 mmol / L potassium bismuth citrate aqueous solution, which is referred to as solution A; and then prepare 100 mL of 40 mmol / L potassium borohydride aqueous solution, which is referred to as solution B. 18 O 49 The / MWCNT / PAN-3 composite nanofiber membrane was immersed in solution A for 2 min and then rinsed with deionized water to remove excess Bi 3+ The nanofiber membrane was then immersed in solution B and reacted for 2 minutes to generate Bi nanostructures on the surface of the nanofibers. After being taken out, it was rinsed with deionized water to remove excess BH4 - Ions, the above "immersion in solution A-extraction-immersion in solution B-extraction" process is a continuous ion layer adsorption reaction (SILAR) cycle, and the loading amount of Bi nanoparticles is adjusted by the number of cycles, and the number of cycles is 14. Then it is cleaned in ultrasound with anhydrous ethanol and deionized water in turn, and dried in an oven at 50℃ for 2h to obtain a Bi / W film with a thickness of 437μm. 18 O 49 / MWCNT / PAN-3 composite nanofiber membrane, referred to as BWCP-3 composite nanofiber membrane.
[0025] The composite nanofiber membrane obtained by using this ratio is light and has an average density of 0.44 g / cm 3 , and maintains good flexibility. Its X-ray shielding efficiency and mass attenuation coefficient gradually decrease with the enhancement of X-rays. At a photon energy of 33keV, the mass attenuation coefficient is 13.63g / cm 3 , X-ray shielding efficiency is 23.06% (see Figure 1 and Figure 2 ).
[0026] Example 2
[0027] (1) Take 0.056g of MWCNT and add it to a beaker containing 7.12g of DMF. After ultrasonic dispersion for 1h, dissolve 0.88g of PAN in the dispersion and stir magnetically for 10h to obtain a spinning precursor solution. Use a 10mL syringe to extract the spinning solution and fix the syringe on the propulsion pump. The syringe has a 1mm diameter stainless steel needle. Connect the positive electrode of the high-voltage power supply to the needle and the negative electrode to the roller covered with silicone oil paper. The positive electrode voltage is set to 6kV, the negative electrode voltage is set to 10kV, the receiving distance is fixed to 10cm, the propulsion speed of the propulsion pump stepper motor is set to 0.6mL / h, the roller speed is 400r / min, the ambient temperature is 25℃, the ambient humidity is 40%, and after spinning for 12h, the fiber membrane is collected and placed in a 60℃ oven for drying for 5h to obtain a MWCNT-filled polymer nanofiber membrane, which is recorded as MWCNT / PAN-6 composite nanofiber membrane;
[0028] (2) 1.5 g of WCl6 was added to a 300 mL polytetrafluoroethylene liner containing 200 mL of anhydrous ethanol. The MWCNT / PAN-6 composite nanofiber membrane obtained in step (1) was cut into a size of 9×9 cm and completely immersed in the above solution. The liner was then placed in a reactor, sealed, and heated in an oven at 170°C for 11 h. After the reactor was naturally cooled to room temperature, the fiber membrane was taken out and cleaned with anhydrous ethanol and deionized water in ultrasound in turn, and then dried in an oven at 50°C for 2 h to obtain WCl6. 18 O 49 / MWCNT / PAN-6 composite nanofiber membrane;
[0029] (3) Prepare 100 mL of a 40 mmol / L aqueous solution of potassium bismuth citrate, referred to as solution A; and then prepare 100 mL of a 40 mmol / L aqueous solution of potassium borohydride, referred to as solution B. 18 O 49 The / MWCNT / PAN-6 composite nanofiber membrane was immersed in solution A for 2 min and then rinsed with deionized water to remove excess Bi 3+ The nanofiber membrane was then immersed in solution B and reacted for 2 minutes to generate Bi nanostructures on the surface of the nanofibers. After being taken out, it was rinsed with deionized water to remove excess BH4 - Ions, the above "immersion in solution A-extraction-immersion in solution B-extraction" process is a continuous ion layer adsorption reaction (SILAR) cycle, and the loading amount of Bi nanoparticles is adjusted by the number of cycles, and the number of cycles is 14. Then it is cleaned in ultrasound with anhydrous ethanol and deionized water in turn, and dried in a 50℃ oven for 2h to obtain a Bi / W film with a thickness of 382μm. 18 O 49 / MWCNT / PAN-6 composite nanofiber membrane, referred to as BWCP-6 composite nanofiber membrane.
[0030] The composite nanofiber membrane obtained by using this ratio is lightweight and has an average density of 0.32 g / cm 3 , and maintains good flexibility. Its X-ray shielding efficiency and mass attenuation coefficient gradually decrease with the enhancement of X-rays. The mass attenuation coefficient is 14.17g / cm at a photon energy of 33keV. 3 , X-ray shielding efficiency is 24.40% (see Figure 3 and Figure 4 ).
[0031] Example 3
[0032] (1) Take 0.12g MWCNT and add it to a beaker containing 7.12g DMF. After ultrasonic dispersion for 1h, dissolve 0.88g PAN in the dispersion and stir magnetically for 10h to obtain a spinning precursor solution. Use a 10mL syringe to extract the spinning solution and fix the syringe on a propulsion pump with a 1mm diameter stainless steel needle. Connect the positive electrode of the high-voltage power supply to the needle and the negative electrode to a roller covered with silicone oil paper. Set the positive voltage to 6kV and the negative voltage to 10kV. Set the receiving distance to 10cm. Set the propulsion speed of the propulsion pump stepper motor to 0.6mL / h, the roller speed to 400r / min, the ambient temperature to 20℃, the ambient humidity to 40%, collect the fiber membrane after spinning for 12h and place it in a 60℃ oven for 5h to obtain a MWCNT-filled polymer nanofiber membrane, recorded as MWCNT / PAN-12 composite nanofiber membrane.
[0033] (2) 1.5 g of WCl6 was added to a 300 mL polytetrafluoroethylene liner containing 200 mL of anhydrous ethanol. The MWCNT / PAN-12 composite nanofiber membrane obtained in step (1) was cut into a size of 9×9 cm and completely immersed in the above solution. The liner was then placed in a reactor and sealed and heated in an oven at 170°C for 11 hours. After the reactor was naturally cooled to room temperature, the fiber membrane was taken out and cleaned with anhydrous ethanol and deionized water in ultrasound in turn, and then placed in an oven at 50°C for 2 hours to obtain W 18 O 49 / MWCNT / PAN-12 composite nanofiber membrane;
[0034] (3) Prepare 100 mL of a 40 mmol / L aqueous solution of potassium bismuth citrate, referred to as solution A; and then prepare 100 mL of a 40 mmol / L aqueous solution of potassium borohydride, referred to as solution B. 18 O 49The / MWCNT / PAN-12 composite nanofiber membrane was immersed in solution A for 2 min and then rinsed with deionized water to remove excess Bi 3+ ions. The nanofiber membrane was then immersed in solution B, and the reduction reaction lasted for 2 minutes to chemically deposit Bi nanostructures on the surface of the nanofibers. After being taken out, it was rinsed with deionized water to remove excess BH4 - Ions, the above "immersion in solution A-extraction-immersion in solution B-extraction" process is a continuous ion layer adsorption reaction (SILAR) cycle, and the loading amount of Bi nanoparticles is adjusted by the number of cycles, and the number of cycles is 14. Then it is cleaned in ultrasound with anhydrous ethanol and deionized water in turn, and dried in a 50℃ oven for 2h to obtain a Bi / W film with a thickness of 505μm. 18 O 49 / MWCNT / PAN-12 composite nanofiber membrane, referred to as BWCP-12 composite nanofiber membrane.
[0035] The BWCP-12 composite nanofiber membrane obtained using this ratio is lightweight and has an average density of 0.36 g / cm 3 ; has good flexibility (see Figure 8 Photo); the microstructure shows a multi-level structure (see Figure 7 SEM morphology), first the carbon nanotubes are evenly distributed inside and outside the PAN nanofibers, and then 18 O 49 The Bi layer covers the entire surface of MWCNT / PAN nanofibers, and finally the Bi layer is covered on the W 18 O 49 The surface of the layer; its mass attenuation coefficient and X-ray shielding efficiency gradually decrease with the enhancement of X-rays. The shielding efficiency of 33keV X-rays is 25.26%, and the mass attenuation coefficient is 15.84g / cm 3 The X-ray shielding rate of the composite film increases with the thickness. When the composite film is stacked to a thickness of 4.24 mm by simply stacking multiple films, the X-ray shielding rate for 33 keV can reach 85.74% (see Figure 5 and Figure 6 ). Compared with Example 1 and Example 2, the X-ray shielding rate and mass attenuation coefficient of the composite film obtained by this ratio are the highest, indicating that MWCNT plays a great role in strengthening the confinement effect of electrons and improving the shielding efficiency of X-rays.
Claims
1. A method for preparing a flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding, the steps of which are as follows: (1) Preparation of MWCNT-filled polymer nanofiber membrane by high-voltage electrospinning: 0.027-0.12 g MWCNT was ultrasonically dispersed in 6-8 g N,N-dimethylformamide to obtain a dispersion; 0.8-0.9 g polyacrylonitrile was then dissolved in the dispersion and stirred to obtain a spinning precursor solution; after spinning for 4-15 h, the fiber membrane was collected and placed in an oven at 45-65 °C for 5-10 h to obtain a MWCNT-filled polymer nanofiber membrane, which was recorded as a MWCNT / PAN composite nanofiber membrane; (2) Solvothermal reaction: 1-2 g of tungsten chloride is dissolved in 150-300 mL of anhydrous ethanol and transferred to a polytetrafluoroethylene liner. The MWCNT / PAN composite nanofiber membrane obtained in step (1) is cut and completely immersed in the above solution. The polytetrafluoroethylene liner is then sealed in a reactor and heated at 160-200° C. for 4-15 h. After the reactor is naturally cooled to room temperature, the nanofiber membrane is taken out and washed and dried to obtain W 18 O 49 / MWCNT / PAN composite nanofiber membrane; (3) Continuous ion layer adsorption reduction reaction: prepare 60-200 mL of 10-50 mmol / L potassium bismuth citrate aqueous solution, referred to as solution A; then prepare 60-200 mL of 10-50 mmol / L KBH4 solution, referred to as solution B; 18 O 49 The / MWCNT / PAN composite nanofiber membrane was immersed in solution A for 1 to 3 minutes and then rinsed with deionized water to remove excess Bi. 3+ ions; then the nanofiber membrane is immersed in solution B for 1 to 3 minutes to react, thereby generating Bi nanostructures on the surface of the nanofibers, and then removed and rinsed with deionized water to remove excess BH4 - ions; the above "immersing in solution A-taking out-immersing in solution B-taking out" process is a continuous ion layer adsorption reaction cycle, and the loading amount of Bi nanoparticles is adjusted by the number of cycles, and the number of cycles is set to 8 to 16 times. Finally, the obtained nanofiber membrane is washed and dried to obtain a BWCP composite nanofiber membrane, that is, the flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding.
2. The method for preparing a flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding according to claim 1, characterized in that: In step (1), a spinning solution is extracted with a syringe, and the syringe is fixed on a propulsion pump, wherein the syringe is provided with a stainless steel needle with a diameter of 0.8 to 1.2 mm; the positive electrode of a high-voltage power supply is connected to the needle, and the negative electrode is connected to a roller covered with silicone oil paper, the positive electrode voltage is set to 7 to 14 kV, the negative electrode voltage is set to -4 to -10 kV, the receiving distance is set to 10 to 15 cm, the propulsion speed of the propulsion pump stepper motor is set to 0.5 to 1.0 mL / h, the roller speed is 300 to 1000 r / min, the ambient temperature is 20 to 25° C., the ambient humidity is 30% to 50%, and the fiber membrane is collected after spinning for 4 to 15 hours.
3. The method for preparing a flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding according to claim 1, characterized in that: In step (2), the MWCNT / PAN composite nanofiber membrane is cut into a size of (8-10) cm×(8-10) cm and then immersed in the above solution.
4. The method for preparing a flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding according to claim 1, characterized in that: The cleaning and drying in step (2) and step (3) is to clean the nanofiber membrane with anhydrous ethanol and deionized water in ultrasound in sequence, and then place it in an oven at 45 to 55° C. to dry it for 1.5 to 3.0 hours.
5. A flexible metal-metal oxide / conductive layer confined composite nanofiber membrane for X-ray shielding, characterized in that: The method is prepared by any one of claims 1 to 4.