Optical fiber SPR trace Cr < 3 + > sensor based on TiO2-MoS2-AuNPs heterojunction, manufacturing method and Cr < 3 + > concentration detection method
By using TiO2-MoS2-AuNPs heterojunction and SPR effect on optical fiber SPR sensors, the cost and time-consuming problems of Cr3+ detection methods in the prior art are solved, and Cr3+ detection with high sensitivity and strong stability is achieved. Excellent selectivity and environmental adaptability of Cr3+.
Patent Information
- Application Number
- CN202410818690.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-22
AI Technical Summary
It is difficult to develop a detection method with good specific identification, selectivity and stability for Cr3+. The traditional method requires huge equipment, is costly and takes a long time.
Using an optical fiber SPR sensor based on TiO2-MoS2-AuNPs heterojunction, the thin-core optical fiber and multi-mode optical fiber are melted, the silver film is plated and the TiO2-MoS2-AuNPs sensitive film is coated, and the Cr3+ concentration is monitored using the SPR effect and the wavelength modulation is carried out. and formant movements realize detection.
It realizes high sensitivity detection of Cr3+, with better selectivity than other heavy metal ions, and has excellent temperature, pH and time stability, with lower detection limits than international standards, and is cost-effective.
Smart Images

Figure CN119000618A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sensor technology, and in particular to an optical fiber SPR trace C based on TiO2-MoS2-AuNPs heterojunction. r3+ Sensor, manufacturing method and Cr 3+ Concentration detection method. Background Art
[0002] Chromium is widely used in various industrial processes such as electroplating, alloying, fixing pigments and anti-corrosion films, and the release of chromium during the production process has led to the pollution of rivers, lakes and seawater. Generally, there are two oxidation states in aqueous solution, chromium III (Cr 3+ ) and chromium VI (Cr2O 7- Although chromium (III) is less harmful than chromium (VI), chromium (VI) in aqueous solution can be easily chemically reduced to chromium (III). Due to the increasing threat of chromium exposure in the environment, it is crucial to develop highly sensitive and selective analytical methods for chromium detection.
[0003] In recent years, many methods have been developed to detect Cr 3+ , such as inductively coupled plasma mass spectrometry (ICP-MS) and atomic absorption spectroscopy. These methods usually require large, special instruments, are costly, time-consuming, and require tedious sample preparation. Therefore, it is necessary to develop a cost-effective, sensitive, and stable method to detect Cr in water environments. 3+ concentration.
[0004] Surface plasmon resonance (SPR) uses the collective oscillation of electrons at the interface between metal and dielectric to detect changes in the refractive index near the sensing surface. It is an ideal method for real-time measurement of heavy metal ions. In the SPR heavy metal ion detection sensor, groups with special specific recognition functions are on the surface of the metal film (Au or Ag, etc.), and heavy metal ions in the liquid solution can interact with the groups with specific recognition functions, causing changes in the refractive index near the sensing surface. Compared with lens-based SPR sensors, fiber-optic SPR sensors are more flexible, simpler and faster, lower cost, and smaller in size. Therefore, fiber-optic SPR sensors have great application potential in heavy metal ion monitoring. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the technical problem to be solved by the present invention is: how to provide a method for 3+ Fiber-optic SPR trace C based on TiO2-MoS2-AuNPs heterojunction with good specific recognition, high selectivity and strong stability r3+ sensor.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A fiber-optic SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction 3+ The sensor includes two thin-core optical fibers connected by fusion into a tapered structure, and the ends of the two thin-core optical fibers away from the tapered structure are respectively fused with multi-mode optical fibers. The cladding surfaces of the two thin-core optical fibers are coated with a layer of silver film, and the surface of the silver film is coated with a TiO2-MoS2-AuNPs sensitive film treated by carboxylation with MSA solution.
[0008] The fiber SPR sensor uses the evanescent wave generated by the total reflection of the incident light at the interface between the fiber core and the metal with different dielectric properties to excite the free electrons on the metal surface and generate surface plasma waves (SPW) on the metal and medium surfaces. If the SPW wave vector is equal to the wave vector of the incident light in the horizontal direction, the SPR effect is generated, causing the corresponding wave vector intensity in the total reflected light to drop significantly, and an absorption peak appears. The position of this peak is related to the external refractive index (RI).
[0009] The fiber-optic SPR sensor uses wavelength modulation. Through Maxwell's equations and related boundary conditions, the propagation constant k of the SPW along the metal-dielectric interface is sp You can get:
[0010]
[0011] where ε m and ε e The dielectric constants of metal and dielectric are respectively, ω and c are the frequency of electromagnetic waves and the speed of light in vacuum, respectively. When light is incident from the dielectric at an angle of θ, the electric field component perpendicular to the interface can excite the surface charge and produce oscillatory motion. The propagation constant k e The parallel component of can be expressed as:
[0012]
[0013] The incident light and the resonance condition of the SPW have the same propagation constant, i.e., k e =k sp Since ε m <0,ε e >0 and |ε m |>ε e , regardless of the angle of incident light from the dielectric to the metal surface, k sp Always greater than k e Therefore, in order to obtain SPR, the propagation constant of the incident light along the metal-dielectric interface must be increased, and the evanescent wave formed in the optical fiber meets the requirements. The propagation constant of the evanescent wave (k ev ) is expressed as:
[0014]
[0015] Where k0 is the propagation constant of the incident light, ε0 is the dielectric constant of the fiber core, and θ0 is the angle of incidence. When the dielectric constant of the sensing film changes and the angle of incidence is fixed, k ev =k sp , and the resonance wavelength shifts as the refractive index of the monitored environment changes. 3+ When adsorbed by the sensing film, the effective refractive index of the sensing film will change, resulting in the movement of the resonance peak. Therefore, in the present invention, the multimode fiber-thin core fiber-multimode fiber SPR sensing structure is used to obtain the evanescent wave in the metal-dielectric interface, and the Cr is measured by monitoring the movement of the tilted wavelength. 3+ concentration.
[0016] like Figure 1 As shown in the figure, the surface of the optical fiber is hydroxylated by dopamine hydrochloride, so that a large number of hydroxyl groups are exposed on the side of the optical fiber. Then, the surface of the optical fiber is hydroxylated by APTES, and the hydroxyl groups on the surface of the optical fiber are removed. + The amino group can be replaced by the amino group, which can bind to gold nanoparticles. There are thiol groups (-SH) and -COOH in the MSA structure, and -COOH can bind to Cr. 3+ Specific sensitivity. Disulfide bonds are relatively stable covalent bonds. TiO2-MoS2-AuNPs are functionalized by MSA. The thiol groups of MSA couple with MoS2 to form disulfide bonds, exposing free carboxyl groups on the surface of the optical fiber. This allows the specific adsorption of Cr with different concentrations in the solution. 3+ , optical fiber surface -COOH adsorbs different concentrations of Cr 3+ After that, the effective refractive index of the sensor surface will change, causing the SPR resonance peak to shift.
[0017] As an optimization, the thickness of the silver film is (67-73) nm, and the thickness of the TiO2-MoS2-AuNPs sensitive film is (1-1.2) um.
[0018] A method for preparing the above-mentioned optical fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction 3+The method for producing a sensor comprises the following steps: obtaining two thin-core optical fibers and two multimode optical fibers and fusing them together respectively, wherein the two thin-core optical fibers are connected together to form a tapered structure, and the two multimode optical fibers are fusing at two ends of the two thin-core optical fibers respectively; a layer of silver film is deposited on the surface of the two thin-core optical fibers, and the surfaces of the two thin-core optical fibers coated with the silver film are hydroxylated, and after drying to a constant weight, the surfaces of the two thin-core optical fibers are amino treated, and after drying to a constant weight, a layer of TiO2-MoS2-AuNPs sensitive film is coated on the surfaces of the two thin-core optical fibers coated with the silver film, and the surfaces of the two thin-core optical fibers are carboxylated using an MSA solution, and the production is completed after drying to a constant weight.
[0019] As an optimization, when the hydroxylation treatment is performed, the two thin-core optical fibers are immersed in a DA solution, and when the amination treatment is performed, the two thin-core optical fibers are immersed in an APTES solution.
[0020] The invention also discloses a method for detecting Cr in liquid 3+ The concentration method uses the fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction described above. 3+ Sensor, connect the multimode optical fiber at one end of the sensor to the light source, connect the multimode optical end at the other end to the spectrometer, immerse the two thin-core optical fibers in the sensor into the liquid, obtain the wavelength of the resonance peak in the detection spectrum, and determine Cr 3+ The linear relationship between the concentration value and the wavelength value of the resonance peak is established based on the linear relationship. 3+ The database of concentration values and wavelength values of resonance peaks in the detection spectrum has Cr 3+ The concentration value and the corresponding wavelength value of the resonance peak are measured by using the sensor to detect the sample to be tested, and the detection spectrum is obtained. The wavelength of the resonance peak in the detection spectrum is obtained, and the Cr corresponding to the wavelength value of the corresponding resonance peak in the database is calculated. 3+ Concentration value, get the Cr in the sample to be tested 3+ Concentration value.
[0021] As an optimization, Cr 3+ The linear relationship between the concentration value and the wavelength value of the resonance peak is determined by taking a number of known Cr 3+ The samples with different concentration values are measured by sensors to obtain corresponding detection spectra. The Cr 3+ There is a linear relationship between the concentration value and the wavelength value of the resonance peak.
[0022] Compared with the prior art, the present invention has the following beneficial effects: the present invention uses TiO2-MoS2-AuNPs as the sensitive material of the sensor and develops a Cr 3+The sensor has a better response by coating the TiO2-MoS2-AuNPs sensitive film, and the sensor is sensitive to Cr 3+ The selectivity is better than other common heavy metal ions in water; and the sensor in the present invention also has excellent temperature, pH value and time stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The sensor of the present invention adsorbs Cr 3+ Mechanism diagram of
[0024] Figure 2 FTIR spectra of TiO2-MoS2-AuNPs and TiO2-MoS2-AuNPs-MSA composite materials in the present invention;
[0025] Figure 3 The sensor coated with MoS2 sensitive film in the present invention is sensitive to different concentrations of Cr 3+ The corresponding spectrum of
[0026] Figure 4 The sensor coated with TiO2 sensitive film in the present invention is sensitive to different concentrations of Cr 3+ The corresponding spectrum of
[0027] Figure 5 The sensor coated with TiO2-MoS2 sensitive film in the present invention is sensitive to different concentrations of Cr 3+ The corresponding spectrum of
[0028] Figure 6 The sensor of the present invention is used to detect different concentrations of Cr 3+ The corresponding spectrum of
[0029] Figure 7 The wavelength drift of the sensor in the present invention and Cr 3+ Linear fitting curve diagram of ;
[0030] Figure 8 The sensor coated with different materials of sensitive film in the present invention is Cr 3+ Comparison chart of wavelength variation of concentration;
[0031] Fig. 9 is a diagram showing the selectivity of the sensor of the present invention to different metal ions;
[0032] Fig.10 It is a diagram showing the influence of different pH values on the sensor of the present invention;
[0033] Fig.11 It is a diagram showing the influence of different temperatures on the sensor of the present invention;
[0034] Fig.12is a time stability diagram of the sensor in the present invention;
[0035] Fig.13 The sensor of the present invention was tested three times for different concentrations of Cr 3+ The corresponding spectrum of . DETAILED DESCRIPTION
[0036] The optical fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction in this specific embodiment 3+ The sensor includes two thin-core optical fibers connected by fusion into a tapered structure, and the ends of the two thin-core optical fibers away from the tapered structure are respectively fused with multi-mode optical fibers. The cladding surfaces of the two thin-core optical fibers are coated with a layer of silver film, and the surface of the silver film is coated with a TiO2-MoS2-AuNPs sensitive film treated by carboxylation with MSA solution.
[0037] A method for preparing the above-mentioned optical fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction 3+ The method for producing a sensor comprises the following steps: obtaining two thin-core optical fibers and two multimode optical fibers and fusing them together respectively, wherein the two thin-core optical fibers are connected together to form a tapered structure, and the two multimode optical fibers are fusing at two ends of the two thin-core optical fibers respectively; a layer of silver film is deposited on the surface of the two thin-core optical fibers, and the surfaces of the two thin-core optical fibers coated with the silver film are hydroxylated, and after drying to a constant weight, the surfaces of the two thin-core optical fibers are amino treated, and after drying to a constant weight, a layer of TiO2-MoS2-AuNPs sensitive film is coated on the surfaces of the two thin-core optical fibers coated with the silver film, and the surfaces of the two thin-core optical fibers are carboxylated using an MSA solution, and the production is completed after drying to a constant weight.
[0038] According to the prior art, heterojunction sensitive material TiO2-MoS2-AuNPs was prepared. In order to synthesize TiO2-MoS2 heterostructure, 0.08g of nano-TiO2 was dispersed in a mixture of 10mL EtOH and 20mL ultrapure water (DI), 0.35g of sodium molybdate dihydrate and 0.52g of thiourea were dissolved in the solution, and the solution was subjected to solvothermal reaction at 220°C for 20h, cooled to room temperature, rinsed with ultrapure water, and dried at 60°C. MoS2 nanosheets were synthesized by the same method without adding nano-TiO2.
[0039] When preparing the TiO2-MoS2-AuNPs composite material, 2mL of 0.01M chloroauric acid and 2mL of 0.01M sodium citrate were added to a uniform suspension of 40mg TiO2-MoS2 heterostructure and stirred continuously in 40mL of ultrapure water; then, 2mL of fresh NaBH4 solution (0.1M, 0-4℃) was added to the suspension and stirred vigorously for 30 minutes; then stirred for another 30min at room temperature and then left undisturbed overnight; the composite material was centrifuged, washed with DI and EtOH in sequence, and then dried in a vacuum at 60℃ overnight.
[0040] Take a thin core (TCF) fiber and a multimode (MMF) fiber, strip the coating of two sections of about 10mm TCF fiber and 15mmMMF fiber respectively, rinse with anhydrous ethanol to remove the residual coating, and then use a fiber fusion splicer to pull the two sections of TCF fiber into a cone, and then fusion splice with the 15mmMMF fiber. Put the treated MMF-TCF fiber into a high vacuum resistance evaporation coating machine, and deposit a silver film on the surface of the two TCF fibers by evaporation; then immerse the silver-coated TCF fiber in DA solution to hydroxylate the surface of the silver-coated fiber; secondly, use APTES solution to amino-dip the surface of the silver-coated TCF fiber; then, use a dip-pull coating machine to coat a uniform layer of TiO2-MoS2-AuNPs sensitive film on the surface of the silver-coated TCF fiber; finally, use MSA solution to carboxylate the surface of the TCF fiber and dry it in a vacuum drying oven at 60℃ for 6h. The morphology of the silver film and TiO2-MoS2-AuNPs sensitive film coated on the surface of the thin-core optical fiber was characterized by scanning electron microscopy (SEM). The thickness of the silver film was about 72.57nm, while the thickness of the TiO2-MoS2-AuNPs film was about 1.13μm.
[0041] Fourier transform infrared (FTIR) spectroscopy was used to confirm that the TiO2-MoS2-AuNPs composites were successfully functionalized by mercaptosuccinic acid (MSA) and exposed to Cr. 3+ Specific sensitive carboxyl group (-COOH). Figure 2 As shown, in the TiO2-MoS2-AuNPs spectrum, 3440.65 cm -1 and 1638.40cm -1 Corresponding to the stretching vibration of hydroxyl -OH, the spectrum line of functionalized TiO2-MoS2-AuNPs-MSA is located at 3432.33 cm -1 Wider belt and 1644.72cm -1 The stretching vibration of hydroxyl-OH and the bending mode of Ti-OH are at 1388.23 cm -1The peak at 1113.78cm is attributed to the stretching vibration of Ti-O mode. -1 and 617.91cm -1 The vibration peak corresponding to MoS2 is 1110.82 cm in the spectrum of TiO2-MoS2-AuNPs-MSA after functionalization. -1 and 617.91cm -1 The vibration peak of MoS2 appears. 2922.11cm -1 and 2851.72cm -1 Corresponding to the methylene CH stretching. At the same time, after the TiO2-MoS2-AuNPs composite material was successfully functionalized by MSA, the FTIR spectrum was located at 1720.80 cm -1 The results attributed to the stretching mode of COOH groups indicated that the composite successfully exposed COOH groups. This indicated that TiO2-MoS2-AuNPs could be functionalized by MSA and exposed to Cr 3+ Specific sensitivity to carboxyl groups.
[0042] A method for detecting Cr in liquid 3+ The concentration method uses the fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction described above. 3+ Sensor, connect the multimode optical fiber at one end of the sensor to the light source, connect the multimode optical end at the other end to the spectrometer, immerse the two thin-core optical fibers in the sensor into the liquid, obtain the wavelength of the resonance peak in the detection spectrum, and determine Cr 3+ The linear relationship between the concentration value and the wavelength value of the resonance peak is established based on the linear relationship. 3+ The database of concentration values and wavelength values of resonance peaks in the detection spectrum has Cr 3+ The concentration value and the corresponding wavelength value of the resonance peak are measured by using the sensor to detect the sample to be tested, and the detection spectrum is obtained. The wavelength of the resonance peak in the detection spectrum is obtained, and the Cr corresponding to the wavelength value of the corresponding resonance peak in the database is calculated. 3+ Concentration value, get the Cr in the sample to be tested 3+ Concentration value.
[0043] In this specific embodiment, Cr 3+ The linear relationship between the concentration value and the wavelength value of the resonance peak is determined by taking a number of known Cr 3+ The samples with different concentration values are measured by sensors to obtain corresponding detection spectra. The Cr 3+ There is a linear relationship between the concentration value and the wavelength value of the resonance peak.
[0044] The performance of different sensors made by coating the surface of TCF optical fiber with silver film with MoS2, TiO2 and TiO2-MoS2 was tested and compared with the sensor of the present invention. Each sensor was connected to a halogen light source and a spectrometer, and the performance of each sensor was tested for 0-1.3μMCr. 3+ Concentration response. Figures 3 to 6 The sensors coated with different materials are sensitive to Cr in the concentration range of 0-1.3μM. 3+ The SPR spectrum response of the solution increases with the Cr 3+ With the increase of concentration, the resonance wavelength of the SPR spectra of Ag-MoS2, Ag-TiO2, Ag-TiO2-MoS2, and Ag-TiO2-MoS2-AuNPs coated materials all showed red shift, and the resonance peak intensity gradually became shallower with the increase of concentration. The maximum wavelength drift of the sensor of Ag-TiO2, Ag-MoS2, Ag-TiO2-MoS2, and Ag-TiO2-MoS2-AuNPs sensitive film was 0.59nm, 10.43nm, 3.92nm, and 63.44nm, respectively. The wavelength drift of the sensor coated with Ag-TiO2-MoS2-AuNPs sensitive film was about 107.52 times, 6.08 times, and 16.18 times that of Ag-MoS2, Ag-TiO2, and Ag-TiO2-MoS2 thin films. It was proved that the composite of semiconductor materials TiO2 and MoS2 coated on the surface of TCF optical fiber effectively improved the sensitivity of the sensor. like Figure 7 As shown, the linear fit is R 2 =0.99, the sensor has good linearity. The maximum sensitivity of the sensor is 49.89nm / μΜ, for Cr 3+ The detection limit (LOD) was calculated to be 0.03 μM, which is much lower than the international standard (50 ppb), and the sensor has good sensitivity. Figure 8 It shows that different coating materials have different 3+ The wavelength shift of the sensor coated with TiO2-MoS2-AuNPs sensitive film is compared with the wavelength shift of Cr in the range of 0-1.3μΜ. 3+ The response of is better than the other two materials, and its wavelength drift is the largest.
[0045] In order to further study the sensitivity of the sensor of the present invention to common heavy metal ions, 1 μM concentration of Zn 2+ NH 4+ , Mn 2+ , Fe 3+ , Cu 2+ 、Co 2+ 、Al 3+ 、Cd 2+ , Ca2+ and Ba 2+ Heavy metal ion solution. Fig. 9 As shown, the sensor of the present invention is Cr 3+ The response drift is more obvious. After adding other heavy metal ions, the SPR resonance wavelength drift is about 1.362nm, which is less than 10% of the sensor drift, indicating that the sensor is only sensitive to Cr. 3+ The sensor is sensitive and shows high selectivity.
[0046] In addition, acidic and alkaline solutions with pH values of 8-11 and 2-6 were prepared respectively, and the above solutions were dripped into the sensor liquid chamber to monitor the sensor wavelength drift. The performance of the sensor was evaluated in an environment with a pH value of 2-11. Fig.10 The effect of different pH environments on the sensor is shown. The degree of wavelength shift increases with the increase of acidity or alkalinity. When the pH value is 2-11, the wavelength shift is below 1.3nm, and when the pH value is 4-9, the wavelength shift is less than 1nm. This shows that the effect of different pH environments on the performance of the sensor can be ignored. Therefore, when the pH value is 4-9, it is a suitable sensing condition.
[0047] The present invention also studies the influence of temperature on the sensor, such as Fig.11 As shown in Figure 2, within the temperature range of 25-50°C, the resonance wavelength shift increases with increasing temperature. At 50°C, the maximum shift of the resonance wavelength is about 6.14nm, which is lower than the sensor's response to Cr. 3+ The response displacement is 10%. When the temperature is below 50℃, the maximum displacement of the resonance wavelength is about 2.97nm, which is much lower than the sensor's response to Cr. 3+ In response to displacement, the sensor has good thermal stability.
[0048] In addition, the time stability is determined by monitoring the sensor in ultrapure water for 180 minutes. Fig.12 As shown, within the detection time range, the resonance wavelength shift of the sensor is between 677.43-678.99 nm, and the resonance wavelength shift is very small, about 1.56 nm, indicating that the sensor has good time stability.
[0049] The present invention also repeatedly tests the sensor and compares the drift of the sensor after three repeated tests to evaluate the repeatability of the sensor. Fig.13 As shown in the figure, (a), (b) and (c) are the spectra of the sensor tested three times. 3+ With the increase of concentration, the red shift of the resonance wavelength in the spectra of (a), (b) and (c) is 71.44nm, 60.83nm and 59.86nm respectively. The drift of the sensor is repeatedly measured. Figure 6The measured drift of the sensor is compared with an error of less than 10 nm, indicating that the sensing structure has good repeatability.
[0050] In this specific embodiment, by comparing the spectral response curves of TiO2, MoS2, TiO2-MoS2, and TiO2-MoS2-AuNPs sensitive films, it is concluded that the sensor coated with the TiO2-MoS2-AuNPs sensitive film has a better response. In the detection concentration range of 0-1.3 μM, as the detection concentration increases, the resonance wavelength also red-shifts, and the offset is about 63.44 nm; in the range of 0-1 μM, the linearity is 0.99, the sensitivity is 49.89 nm / μM, the detection limit is 0.03 μΜ, and the optical fiber SPR sensor is sensitive to Cr 3+ The sensor has superior selectivity to other common heavy metal ions in water and has excellent temperature, pH and time stability.
[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction 3+ The sensor is characterized by: The method comprises two thin-core optical fibers connected by fusion into a tapered structure, wherein a multimode optical fiber is fused to one end of each of the two thin-core optical fibers away from the tapered structure, and a layer of silver film is coated on the cladding surface of the two thin-core optical fibers, and a layer of TiO2-MoS2-AuNPs sensitive film carboxylated by MSA solution is coated on the surface of the silver film.
2. The optical fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction according to claim 1 3+ The sensor is characterized by: The thickness of the silver film is (67-73) nm, and the thickness of the TiO2-MoS2-AuNPs sensitive film is (1-1.2) um.
3. A method for preparing a fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction as claimed in any one of claims 1 or 2 3+ A sensor method, characterized in that: Two thin-core optical fibers and two multimode optical fibers are obtained and fused together respectively, wherein the two thin-core optical fibers are connected together to form a tapered structure, and the two multimode optical fibers are fused to the two ends of the two thin-core optical fibers respectively; a layer of silver film is deposited on the surface of the two thin-core optical fibers, and the surfaces of the two thin-core optical fibers coated with the silver film are hydroxylated, and after drying to constant weight, the surfaces of the two thin-core optical fibers are amino treated, and after drying to constant weight, a layer of TiO2-MoS2-AuNPs sensitive film is coated on the surfaces of the two thin-core optical fibers coated with the silver film, and then the surfaces of the two thin-core optical fibers are carboxylated using an MSA solution, and the production is completed after drying to constant weight.
4. The method for preparing a fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction according to claim 3 3+ A sensor method, characterized in that: When the hydroxylation treatment is performed, the two thin-core optical fibers are immersed in a DA solution, and when the amination treatment is performed, the two thin-core optical fibers are immersed in an APTES solution.
5. A method for detecting Cr in liquid 3+ The concentration method is characterized by: Optical fiber SPR trace Cr based on TiO2-MoS2-AuNPs heterojunction according to any one of claims 1 or 2 3+ Sensor, connect the multimode optical fiber at one end of the sensor to the light source, connect the multimode optical end at the other end to the spectrometer, immerse the two thin-core optical fibers in the sensor into the liquid, obtain the wavelength of the resonance peak in the detection spectrum, and determine Cr 3+ The linear relationship between the concentration value and the wavelength value of the resonance peak is established based on the linear relationship. 3+ The database of concentration values and wavelength values of resonance peaks in the detection spectrum has Cr 3+ The concentration value and the corresponding wavelength value of the resonance peak are measured by using the sensor to detect the sample to be tested, and the detection spectrum is obtained. The wavelength of the resonance peak in the detection spectrum is obtained, and the Cr corresponding to the wavelength value of the corresponding resonance peak in the database is calculated. 3+ Concentration value, get the Cr in the sample to be tested 3+ Concentration value.
6. The method for detecting Cr in liquid according to claim 5 3+ The concentration method is characterized by: Cr 3+ The linear relationship between the concentration value and the wavelength value of the resonance peak is determined by taking a number of known Cr 3+ The samples with different concentration values are measured by sensors to obtain corresponding detection spectra. The Cr 3+ There is a linear relationship between the concentration value and the wavelength value of the resonance peak.