Processing method for reducing reverse transmission capacitance of silicon carbide MOSFET

By depositing and etching silicon nitride on the wafer surface before the silicon carbide MOSFET gate oxide process to form a non-uniform gate oxide layer, the on-resistance and reliability problems caused by increasing the gate oxide layer thickness or changing the drive circuit in the prior art are solved, and the reverse transfer capacitance is reduced and the switching characteristics are improved.

CN119008412APending Publication Date: 2024-11-22TIANJIN HUANXIN TECH DEV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411096130.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing technologies that reduce the reverse transfer capacitance of silicon carbide MOSFETs by increasing the gate oxide layer thickness or changing the drive circuit can easily lead to increased on-resistance or gate oxide layer stress, affecting device reliability.

Method used

Before the gate oxidation process of silicon carbide MOSFET, a layer of silicon nitride is deposited on the wafer surface. The silicon nitride on the JFET region is etched away by photolithography and dry etching to expose the silicon carbide surface. Then the gate oxidation process is performed. The shielding effect of silicon nitride makes the oxide layer in the JFET region grow faster and the oxide layer in other regions grow slower, forming an uneven gate oxide film layer.

Benefits of technology

Without increasing the gate oxide thickness or changing the drive circuit, the reverse transfer capacitance was reduced, the switching characteristics of the MOSFET were improved, the switching time and the probability of false turn-on were reduced, and the breakdown resistance of the gate oxide was improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008412A_ABST
    Figure CN119008412A_ABST
Patent Text Reader

Abstract

The invention provides a processing method for reducing reverse transmission capacitance of a silicon carbide MOSFET (Metal-Oxide-Semiconductor Field Effect Transistor), which comprises the following steps of: before forming a gate oxide layer on the front surface of a silicon carbide epitaxial substrate with an MOSFET structure, forming a barrier layer with the same structure as a gate oxide layer mask pattern, so that gate oxide layers with different thicknesses can be formed during gate oxidation. According to the processing method for reducing the reverse transmission capacitance of the silicon carbide MOSFET, the thickness of the oxide layer above the JFET region can be increased under the conditions that the thickness of the gate oxide layer is not increased and a driving circuit is not changed, and the purpose of reducing the reverse transmission capacitance is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of semiconductor chip manufacturing, and in particular, relates to a processing method for reducing the reverse transfer capacitance of a silicon carbide MOSFET. Background Art

[0002] Silicon carbide material is one of the ideal materials for making high-temperature, high-frequency, high-power, and high-voltage devices. Compared with traditional silicon materials, the bandgap width of silicon carbide is 3 times that of silicon, and the thermal conductivity is 4-5 times that of silicon; the breakdown voltage is 8-10 times that of silicon; the electron saturation drift rate is 2-3 times that of silicon, which meets the needs of modern industry for high power, high voltage, and high frequency. It is mainly used to make high-speed, high-frequency, high-power and light-emitting electronic components;

[0003] Because of the above advantages, silicon carbide MOSFET usually works in high-frequency switching situations, so the impact of parasitic parameters on it is more significant, usually called the Miller effect. The Miller effect not only increases switching delay, but may also cause parasitic conduction and increase device loss. The root cause of the Miller effect is the parasitic capacitance Cgd between the gate and the drain. Due to the structure of the semiconductor design, there are various types of parasitic capacitance inside the MOSFET, which can be divided into gate-source capacitance, gate-drain capacitance and gate-source capacitance. The capacitance between the gate and the drain is the Miller capacitance, also called the reverse transfer capacitance.

[0004] The reverse transfer capacitance of Cgd cannot be eliminated, so it can only be reduced by optimizing the device design. The methods used in the prior art and their problems are as follows:

[0005] 1. Increasing the thickness of the gate oxide layer can reduce Cgd, but it will also increase the threshold voltage, which cannot meet the driving application. In addition, increasing the thickness will reduce the channel mobility and increase the on-resistance at the same driving voltage.

[0006] 2. Change the driving circuit and actually use negative voltage shutdown. In order to offset the voltage generated by Cgd and prevent false turn-on, negative gate voltage shutdown is required. However, this will increase the stress of the gate oxide layer and have a negative impact on the long-term reliability of the device.

[0007] Therefore, how to make a special MOSFET gate structure that can reduce the reverse transfer capacitance and thus improve the switching characteristics of the device without increasing the thickness of the gate oxide layer or changing the driving circuit is the focus of the invention in this case. Summary of the invention

[0008] The present application provides a method for reducing the reverse transfer capacitance of a silicon carbide MOSFET, which solves the technical problem that the method of reducing the reverse transfer capacitance by increasing the thickness of the gate oxide layer or changing the drive circuit in the prior art easily causes an increase in on-resistance or gate oxide layer stress, thereby affecting device reliability.

[0009] In order to solve at least one of the above technical problems, the technical solution adopted in this application is:

[0010] A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET, the steps comprising:

[0011] Before forming a gate oxide layer on the front side of a silicon carbide epitaxial substrate having a MOSFET structure, a barrier layer having the same structure as the gate oxide layer mask pattern is first formed so that gate oxide layers of different thicknesses can be formed during gate oxidation.

[0012] Furthermore, before forming the barrier layer, it also includes activating all ions inside the epitaxial substrate, and then performing a sacrificial oxidation operation on the front side of the epitaxial substrate, specifically:

[0013] First, put the epitaxial substrate as a whole into a high-temperature annealing furnace with a temperature of 1600-1900°C and an activation time of 10-40 minutes to activate all ions inside the epitaxial substrate;

[0014] Placing the epitaxial substrate in an oxidation furnace, oxidizing the front and back surfaces of the epitaxial substrate in a wet oxygen atmosphere to form a silicon dioxide oxide layer respectively;

[0015] The epitaxial substrate is taken out, and the silicon dioxide oxide layer is etched away using hydrofluoric acid to expose the surface of a new silicon carbide epitaxial substrate.

[0016] Furthermore, the oxidation temperature during sacrificial oxidation is 1000-1100° C., the oxidation time is 30-60 min, and the thickness of the silicon dioxide oxide layer on a single side surface is 10-50 nm.

[0017] Furthermore, deposition is performed on the epitaxial substrate after sacrificial oxidation, and a barrier layer is formed on the front side by LPCVD, the temperature during deposition is 600-900°C, and the time is 30-60min; and the thickness of the barrier layer is 100nm-1um.

[0018] Further, preparing the barrier layer includes:

[0019] Coating a layer of photoresist on the barrier layer, and photolithographically fabricating a structure pattern above the JFET region;

[0020] Then, a dry etching process is used to etch away the barrier layer above the JFET region, exposing the surface of a new silicon carbide epitaxial substrate, and retaining the barrier layer covering the non-JFET region;

[0021] Then, an organic stripping solution is used to remove the photoresist to obtain a barrier layer with the same pattern as the gate oxide layer.

[0022] Furthermore, a gate oxide layer is prepared on the epitaxial substrate having the barrier layer, specifically:

[0023] Cleaning epitaxial substrates;

[0024] Gate oxidation is performed in a high-temperature oxidation furnace. The oxidation speed of the area blocked by the barrier layer is slow, while the oxidation speed of the area not blocked by the barrier layer is fast, so that a patterned gate oxide layer with uneven thickness can be formed on the surface of the epitaxial substrate;

[0025] The silicon nitride layer on the front side of the epitaxial substrate is then removed using a phosphoric acid solution.

[0026] Furthermore, when cleaning the epitaxial substrate, the epitaxial substrate is controlled to be cleaned in ammonia water, hydrochloric acid and sulfuric acid solutions in sequence;

[0027] The temperature during gate oxidation is 1200-1400° C., and the time is 30-120 min; the thickness of the obtained gate oxide layer is 30-70 nm.

[0028] Furthermore, after the gate oxide layer is formed, a front electrode is formed on the front side, specifically:

[0029] depositing a layer of polysilicon on the gate oxide layer;

[0030] A gate is formed by etching using photolithography and dry etching;

[0031] Deposit a silicon dioxide insulating layer on the epitaxial substrate to wrap the gate, and make the insulating layer 1um thick;

[0032] The insulating layer is subjected to photolithography and dry etching to obtain an insulating layer that only exposes the P+ and N+ source regions.

[0033] Furthermore, it also includes:

[0034] Depositing a source metal layer on the front side of the epitaxial substrate by evaporation or sputtering, wherein the corresponding metals in the metal layer are Ni, Ti, and Al from bottom to top, respectively, with a thickness of 10nm-4um, and forming a front source metal pattern by photolithography and etching to obtain a front electrode to form a source;

[0035] Then, four metal layers of Ni, Ti, Ni, and Ag are deposited in sequence on the back of the epitaxial substrate by sputtering or evaporation, with a thickness ranging from 50nm to 2um, to obtain a back electrode to form a drain.

[0036] Furthermore, before preparing the barrier layer, it also includes preparing a silicon carbide epitaxial substrate having a MOSFET structure, specifically:

[0037] The P-well region structure is obtained by first implanting Al ions into the epitaxial layer of the epitaxial wafer;

[0038] Then, N ions are implanted on the front side of the epitaxial wafer having the P-well region structure to obtain an N+ source region structure stacked on the P-well region;

[0039] Then, Al ions are implanted on the P-well layer on the front side of the epitaxial wafer to obtain a P+ source region structure stacked on the P-well region, and to make the P+ and N+ source regions adjacent to each other;

[0040] The silicon carbide epitaxial substrate having P-well, N+ and P+ source region structures is obtained.

[0041] A method for reducing the reverse transfer capacitance of silicon carbide MOSFET designed by the present application is adopted. Before the gate oxidation process of silicon carbide MOSFET, a layer of silicon nitride is first deposited on the surface of the wafer, and then the silicon nitride above the JFET area is etched away by photolithography and dry etching to expose the silicon carbide surface, and then the gate oxidation process is performed. Due to the shielding effect of the silicon nitride film, the oxide layer grows faster in the exposed area of ​​silicon carbide, while other areas grow slower due to the shielding of silicon nitride, resulting in an uneven gate oxide film layer. This method can increase the oxide layer thickness above the JFET area without increasing the gate oxide layer thickness or changing the drive circuit, thereby achieving the purpose of reducing the reverse transfer capacitance. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 It is a schematic diagram of a reverse transfer capacitor in a chip having a MOSFET structure in the prior art;

[0043] Figure 2 It is a flow chart of a method for reducing the reverse transfer capacitance of a silicon carbide MOSFET in the present application;

[0044] Figure 3 It is a schematic structural diagram of the front side of the silicon carbide epitaxial substrate having a MOSFET structure in the present application;

[0045] Figure 4 It is a schematic diagram of the structure of depositing a barrier layer on the front side of an epitaxial substrate in the present application;

[0046] Figure 5is a schematic diagram of the structure of the blocking layer after patterning in the present application;

[0047] Figure 6 It is a schematic structural diagram of the front side of the epitaxial substrate after gate oxidation in the present application;

[0048] Figure 7 It is a schematic diagram of the structure of the gate oxide layer with different thicknesses in this application;

[0049] Figure 8 It is a schematic structural diagram of the front side of a MOSFET chip having a gate oxide layer structure with uneven thickness in the present application;

[0050] Fig. 9 It is a schematic diagram of the reverse transfer capacitor in the MOSFET chip with a gate oxide layer structure of uneven thickness in the present application.

[0051] In the figure:

[0052] 10. Epitaxial layer 11. P-well region 12. P+ source region

[0053] 13. N+ source region 14. JFET region 20. Substrate layer

[0054] 30, barrier layer 40, gate oxide layer 41, gate

[0055] 50, polysilicon electrode 60, insulating layer 70, source

[0056] 80. Drain DETAILED DESCRIPTION

[0057] The present application is described in detail below with reference to the accompanying drawings and specific embodiments.

[0058] This embodiment provides a method for reducing the reverse transfer capacitance of a silicon carbide MOSFET. Figure 2 As shown, the steps include:

[0059] S1. Obtain a silicon carbide epitaxial substrate having a MOSFET structure.

[0060] like Figure 3 As shown, Al ions are first injected into the epitaxial layer 10 in the epitaxial wafer to obtain the structure of the P-well region 11; then N ions are injected into the front side of the epitaxial wafer having the P-well region 11 structure to obtain the N+ source region 13 structure superimposed on the P-well region 11; finally, Al ions are injected into the P-well layer 11 on the front side of the epitaxial wafer to obtain the P+ source region 12 structure superimposed on the P-well region 11, and the P+ and N+ source regions are adjacent to each other, and finally a silicon carbide epitaxial substrate having P-well, N+ and P+ source region structures is obtained.

[0061] Specifically, a layer of silicon dioxide is first deposited on the front side of the epitaxial wafer, and then the silicon dioxide layer is etched to form a P-well mask pattern, wherein the epitaxial wafer includes an epitaxial layer 10 and a substrate layer 20. At this time, the epitaxial layer 10 and the substrate layer 20 are both epitaxial wafers made of N-type SiC material, and because the initial thickness of the substrate layer 20 is relatively thick, about 300-500um, its base structure strength is high, and etching can be performed directly on the front side.

[0062] The silicon dioxide layer is a common deposition layer, which is convenient for photolithography masking on the front side. Then a layer of photoresist with a P-well mask pattern is coated on the surface of the silicon dioxide layer, the purpose of which is to perform photolithography on this silicon dioxide layer to form a P-well mask pattern. After the P-well mask pattern is formed on the silicon dioxide layer, the photoresist is removed. At this time, there are three layers on the epitaxial wafer, the epitaxial layer 10 located on the front side, the silicon dioxide layer with a P-well mask pattern located on the front side (omitted in the figure), and the substrate layer 20 located on the back side.

[0063] Based on the P-well mask pattern on the silicon dioxide layer, Al ions are first implanted into the epitaxial layer 10 on the front side of the epitaxial wafer to obtain the P-well region 11 structure on the front side of the epitaxial layer 10. The temperature when Al ions are implanted is 500-600°C, the energy is 500-10keV, and the dose is 1E11-1E13, thereby obtaining an epitaxial wafer having the P-well region 11 structure on the front side of the epitaxial layer 10.

[0064] Hydrofluoric acid is used to remove the silicon dioxide P-well mask layer deposited for the first time on the front side of the epitaxial wafer.

[0065] A silicon dioxide layer is deposited on the front of the epitaxial wafer for the second time, and a photoresist having a mask pattern of the N+ source region 13 is coated on the surface of the silicon dioxide layer. Based on the photoresist, the mask pattern of the N+ source region 13 is etched on the silicon dioxide layer. After the mask pattern of the N+ source region 13 is formed on the silicon dioxide layer, the photoresist is removed.

[0066] Based on the mask pattern of the N+ source region 13 of the silicon dioxide layer, N ions are implanted on the P-well region 11 in the epitaxial layer 10 on the front side of the epitaxial wafer to obtain an N+ source region 13 structure stacked on the P-well region 11. The temperature when the N ions are implanted is 500-600°C, the energy is 200-10keV, and the dose is 1E12-1E14, thereby obtaining an epitaxial wafer having an N+ source region 13 structure stacked on the P-well region 11 in the epitaxial layer 10.

[0067] The mask layer of silicon dioxide N+ source region 13 deposited for the second time on the front side of the epitaxial wafer is removed by using hydrofluoric acid.

[0068] A silicon dioxide layer is deposited on the front of the epitaxial wafer for the third time, and a photoresist having a mask pattern of the P+ source region 12 is coated on the surface of the silicon dioxide layer. Based on the photoresist, the mask pattern of the P+ source region 12 is etched on the silicon dioxide layer. After the mask pattern of the P+ source region 12 is formed on the silicon dioxide layer, the photoresist is removed.

[0069] Based on the mask pattern of the P+ source region 12 of the silicon dioxide layer, Al ions are implanted on the P-well region 11 in the epitaxial layer 10 on the front side of the epitaxial wafer to obtain a P+ source region 12 structure stacked on the P-well region 11, and the P+ and N+ source regions 13 are adjacent. The temperature when Al ions are implanted to obtain the P+ source region 12 is 500-600°C, the energy is 30-500keV, and the dose is 1E12-1E15, thereby obtaining an epitaxial wafer having a P+ source region 12 structure stacked on the P-well region 11 in the epitaxial layer 10, and the P+ and N+ source regions 13 are adjacent, for ohmic contact.

[0070] Hydrofluoric acid is used to remove the third deposited silicon dioxide P+ source region 12 mask layer on the front side of the epitaxial wafer, and then the following is obtained: Figure 3 The substrate shown has a structure of a P-well region 11, an N+ source region 13 and a P+ source region 12; at the same time, on the substrate, the area between adjacent P-well regions 11 is a junction field effect transistor JFET region 14.

[0071] S2. Activate all ions inside the epitaxial substrate, and then perform a sacrificial oxidation operation on the front side of the epitaxial substrate.

[0072] First, the epitaxial substrate is placed in a high-temperature annealing furnace with a temperature of 1600-1900°C and an activation time of 10-40 minutes to activate all ions inside the epitaxial substrate.

[0073] Then the epitaxial substrate is placed in an oxidation furnace, and the silicon carbide on the surface of the epitaxial substrate is oxidized in a wet oxygen atmosphere, including the front and back surfaces of the epitaxial substrate, so that a layer of silicon dioxide oxide layer is formed on the front and back surfaces of the epitaxial substrate. The temperature of oxygen in the oxidation furnace is 1000-1100°C, and the oxidation time is 30-60 minutes; finally, the thickness of the silicon dioxide oxide layer on a single side is 10-50nm.

[0074] The epitaxial substrate is taken out, and the silicon dioxide oxide layer on the surface of the epitaxial substrate is etched away using hydrofluoric acid to expose the surface of a new silicon carbide epitaxial substrate.

[0075] S3. Form a silicon nitride barrier layer on the epitaxial substrate.

[0076] like Figure 4As shown, deposition is performed on the new silicon carbide epitaxial substrate obtained after sacrificial oxidation, and a barrier layer 30 is formed on the front side by LPCVD. The temperature during deposition is 600-900°C, and the time is 30-60min; and the thickness of the barrier layer 30 is 100nm-1um.

[0077] like Figure 5 As shown, the silicon nitride layer is patterned to obtain a structure identical to the gate oxide layer mask pattern, and the silicon nitride layer is used as a barrier layer 30 for the gate oxide layer.

[0078] This operation is to form a silicon nitride layer with the same structure as the gate oxide mask pattern before forming a gate oxide layer on the front side of the silicon carbide epitaxial substrate with a MOSFET structure; due to the blocking effect of the silicon nitride layer, the blocked area oxidizes slowly, while the exposed area oxidizes quickly, so a patterned gate oxide layer 40 with uneven thickness is formed on the surface of the front side of the epitaxial substrate. Furthermore, without increasing the thickness of the gate oxide layer or changing the driving circuit, the oxide layer thickness above the JFET region is increased to achieve the purpose of reducing the reverse transfer capacitance.

[0079] Specifically, preparing the barrier layer 30 includes:

[0080] In such Figure 4 A layer of photoresist is coated on the barrier layer 30 shown, and a structure pattern above the JFET region 14 is formed on the photoresist through photolithography and etching processes.

[0081] Based on the pattern structure of the photoresist, a dry etching process is used to etch away the barrier layer above the JFET region 14 to expose a new silicon carbide epitaxial substrate surface, and retain the barrier layer 30 covering the non-JFET region 14 .

[0082] Then use organic stripping solution to remove the photoresist to obtain Figure 5 The barrier layer 30 shown and having the same pattern as the gate oxide layer, that is, the barrier layer 30 in the figure, is a schematic diagram of the structure of the patterned barrier layer 30, which is a silicon carbide epitaxial substrate surface protected by silicon nitride.

[0083] S4. Prepare a structure with a non-uniform gate oxide layer.

[0084] like Figure 6 As shown, a gate oxide layer 40 is prepared on an epitaxial substrate having a patterned barrier layer 30, specifically:

[0085] The epitaxial substrate is first cleaned, that is, the epitaxial substrate is first cleaned in ammonia water, hydrochloric acid and sulfuric acid solutions in sequence to remove surface organic matter, particles and metal ions.

[0086] Then, gate oxidation is performed in a high-temperature oxidation furnace, wherein the gate oxidation temperature is 1200-1400°C and the time is 30-120 minutes; the thickness of the obtained gate oxide layer 40 is 30-70nm. The oxidation speed of the area blocked by the barrier layer is slow, while the oxidation speed of the area not blocked by the barrier layer is fast, and a patterned gate oxide layer with uneven thickness can be formed on the surface of the epitaxial substrate. In order to increase the thickness of the oxide layer in the JFET region 14 and ensure the normal oxide layer required in the blocked area, the thickness of the gate oxide layer 40 is usually prepared to be 30-70nm, which can increase the oxidation speed and gate annealing time.

[0087] Finally, phosphoric acid solution is used to remove the silicon nitride layer on the front side of the epitaxial substrate without damaging the gate oxide layer to obtain Figure 7 An epitaxial substrate with a non-uniform gate oxide structure is shown.

[0088] S5. Prepare the source and drain of a silicon carbide MOSFET chip with an uneven gate oxide layer structure.

[0089] like Figure 8 As shown, after the gate oxide layer, a layer of polysilicon is first deposited on the gate oxide layer 40 by LPCVD; and then photolithography and dry etching are used to etch and form the gate 41 and the polysilicon electrode 50.

[0090] Then, a silicon dioxide insulating layer 60 is deposited on the epitaxial substrate to wrap the gate 41, and the thickness of the insulating layer 60 is 1 um.

[0091] Then, the insulating layer is etched again by photolithography and dry etching, and the silicon dioxide insulating layer is etched away in the P+ and N+ source regions to obtain an insulating layer 60 that only exposes the P+ and N+ source regions.

[0092] Then, on the front side of the epitaxial substrate, a source metal layer is deposited by evaporation or sputtering. From bottom to top, the corresponding metals in the metal layer are Ni, Ti, and Al, respectively, with thicknesses ranging from 10nm to 4um. A front source metal pattern is formed by photolithography and etching to obtain a front electrode to form a source 70.

[0093] Then, four metal layers of Ni, Ti, Ni, and Ag are deposited in sequence on the back of the epitaxial substrate by sputtering or evaporation, with a thickness ranging from 50nm to 2um, to obtain a back electrode to form a drain 80.

[0094] like Fig. 9As shown, it is a schematic diagram of the reverse transfer capacitor in a MOSFET chip with a gate oxide layer structure of uneven thickness manufactured by the manufacturing method of the present application. It can be clearly seen from the figure that the silicon carbide MOSFET structure has a significantly thicker oxide layer in the JFET area 14, but the thickness of the gate oxide layer 40 in other areas is still a conventional thickness, which does not affect its threshold voltage and other parameters; at the same time, it also improves the anti-breakthrough ability of the gate oxide layer in the reverse withstand voltage state. Moreover, since the size of Cgd is inversely proportional to the oxide thickness of the JFET area below the gate, the addition of the oxide layer above the JFET area will significantly reduce Cgd, thereby improving the switching characteristics of the MOSFET, reducing the switching time, and reducing the probability of false opening.

[0095] A method for reducing the reverse transfer capacitance of silicon carbide MOSFET designed by the present application is adopted. Before the gate oxidation process of silicon carbide MOSFET, a layer of silicon nitride is first deposited on the surface of the wafer, and then the silicon nitride above the JFET area is etched away by photolithography and dry etching to expose the silicon carbide surface, and then the gate oxidation process is performed. Due to the shielding effect of the silicon nitride film, the oxide layer grows faster in the exposed area of ​​silicon carbide, while other areas grow slower due to the shielding of silicon nitride, resulting in an uneven gate oxide film layer. This method can increase the oxide layer thickness above the JFET area without increasing the gate oxide layer thickness or changing the drive circuit, thereby achieving the purpose of reducing the reverse transfer capacitance.

[0096] The above detailed description of the embodiments of the present application is only a preferred embodiment of the present application and cannot be considered to limit the scope of implementation of the present application. All equivalent changes and improvements made within the scope of the present application should still fall within the scope of the patent coverage of the present application.

Claims

1. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET, characterized in that the steps include: Before forming a gate oxide layer on the front side of a silicon carbide epitaxial substrate having a MOSFET structure, a barrier layer having the same structure as the gate oxide layer mask pattern is first formed so that gate oxide layers of different thicknesses can be formed during gate oxidation.

2. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET according to claim 1, characterized in that: Before forming the barrier layer, it also includes activating all ions inside the epitaxial substrate, and then performing a sacrificial oxidation operation on the front side of the epitaxial substrate, specifically: First, put the epitaxial substrate as a whole into a high-temperature annealing furnace with a temperature of 1600-1900°C and an activation time of 10-40 minutes to activate all ions inside the epitaxial substrate; Placing the epitaxial substrate in an oxidation furnace, oxidizing the front and back surfaces of the epitaxial substrate in a wet oxygen atmosphere to form a silicon dioxide oxide layer respectively; The epitaxial substrate is taken out, and the silicon dioxide oxide layer is etched away using hydrofluoric acid to expose the surface of a new silicon carbide epitaxial substrate.

3. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET according to claim 2, characterized in that: The oxidation temperature during sacrificial oxidation is 1000-1100° C., and the oxidation time is 30-60 min. The thickness of the silicon dioxide oxide layer on a single side surface is 10-50 nm.

4. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET according to claim 2 or 3, characterized in that: Deposition is performed on the epitaxial substrate after sacrificial oxidation, and a barrier layer is formed on the front side by LPCVD. The temperature during deposition is 600-900°C and the time is 30-60 minutes. The thickness of the barrier layer is 100nm-1um.

5. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET according to claim 4, characterized in that: The preparation of the barrier layer comprises: Coating a layer of photoresist on the barrier layer, and photolithographically fabricating a structure pattern above the JFET region; Then, a dry etching process is used to etch away the barrier layer above the JFET region, exposing the surface of a new silicon carbide epitaxial substrate, and retaining the barrier layer covering the non-JFET region; Then, an organic stripping solution is used to remove the photoresist to obtain a barrier layer with the same pattern as the gate oxide layer.

6. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET according to any one of claims 1 to 3 and 5, characterized in that: A gate oxide layer is prepared on an epitaxial substrate having a barrier layer, specifically: Cleaning epitaxial substrates; Gate oxidation is performed in a high-temperature oxidation furnace. The oxidation speed of the area blocked by the barrier layer is slow, while the oxidation speed of the area not blocked by the barrier layer is fast, so that a patterned gate oxide layer with uneven thickness can be formed on the surface of the epitaxial substrate; The silicon nitride layer on the front side of the epitaxial substrate is then removed using a phosphoric acid solution.

7. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET according to claim 6, characterized in that: When cleaning the epitaxial substrate, the epitaxial substrate is controlled to be cleaned in ammonia water, hydrochloric acid and sulfuric acid solutions in sequence; The temperature during gate oxidation is 1200-1400° C., and the time is 30-120 min; the thickness of the obtained gate oxide layer is 30-70 nm.

8. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET according to any one of claims 1-3, 5, and 7, characterized in that: After the gate oxide layer, the front electrode is prepared on the front side, specifically: depositing a layer of polysilicon on the gate oxide layer; A gate is formed by etching using photolithography and dry etching; Deposit a silicon dioxide insulating layer on the epitaxial substrate to wrap the gate, and make the insulating layer 1um thick; The insulating layer is subjected to photolithography and dry etching to obtain an insulating layer that only exposes the P+ and N+ source regions.

9. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET according to claim 8, characterized in that: Also includes: Depositing a source metal layer on the front side of the epitaxial substrate by evaporation or sputtering, wherein the corresponding metals in the metal layer are Ni, Ti, and Al from bottom to top, respectively, with a thickness of 10nm-4um, and forming a front source metal pattern by photolithography and etching to obtain a front electrode to form a source; Then, four metal layers of Ni, Ti, Ni, and Ag are deposited in sequence on the back of the epitaxial substrate by sputtering or evaporation, with a thickness ranging from 50nm to 2um, to obtain a back electrode to form a drain.

10. A method for reducing the reverse transfer capacitance of a silicon carbide MOSFET according to any one of claims 1-3, 5, 7, and 9, characterized in that: Before preparing the barrier layer, the method further includes preparing a silicon carbide epitaxial substrate having a MOSFET structure, specifically: The P-well region structure is obtained by first implanting Al ions into the epitaxial layer of the epitaxial wafer; Then, N ions are implanted on the front side of the epitaxial wafer having the P-well region structure to obtain an N+ source region structure stacked on the P-well region; Then, Al ions are implanted on the P-well layer on the front side of the epitaxial wafer to obtain a P+ source region structure stacked on the P-well region, and to make the P+ and N+ source regions adjacent to each other; The silicon carbide epitaxial substrate having P-well, N+ and P+ source region structures is obtained.

Citation Information

Cited By

  • Metal-oxide-semiconductor field effect transistor (MOSFET) device and manufacturing method

    CN120187073A