Preparation method and application of porous membrane electrode of proton exchange membrane fuel cell
By using pore-forming agent in the catalytic layer of the proton exchange membrane fuel cell and combining the treatment of acid and hydrogen peroxide, the problem of insufficient porosity and pore size distribution of the catalytic layer is solved, the oxygen mass transfer efficiency and battery performance are improved, and the cost is achieved , efficient preparation of membrane electrodes.
Patent Information
- Application Number
- CN202411120415.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
The porosity and pore size distribution of the catalytic layer in the existing proton exchange membrane fuel cells is insufficient, resulting in high oxygen transmission resistance and affecting battery performance.
Pore-forming agent is used to introduce pores into the catalytic layer, and the pore size distribution of the catalytic layer is optimized through step-by-step impregnation and drying methods of acid and hydrogen peroxide to reduce oxygen mass transfer resistance.
It improves the utilization rate of the catalyst, reduces the oxygen mass transfer resistance, optimizes the material transfer of the membrane electrode, improves the battery performance, and simplifies the preparation process, reducing costs and energy consumption.
Smart Images

Figure CN119008981A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a method for preparing a porous membrane electrode of a proton exchange membrane fuel cell and application thereof. Background Art
[0002] In the quest to reduce air pollution and greenhouse gas emissions, green hydrogen is an important energy carrier with no carbon emissions; hydrogen, non-fossil and renewable energy need to play a vital role in future energy transformation and storage; proton exchange membrane fuel cells (PEMFCs), as an electrochemical energy conversion tool that converts oxygen and hydrogen into electricity with pure water as the only product, are seen as a highly promising solution. Fuel cells can play an important role in both energy storage and power generation, and demand is increasing; the high energy density characteristics of fuel cells are suitable for a wide range of industries such as transportation, where they can work in conjunction with other electrochemical power sources such as batteries and supercapacitors, so achieving high-performance and cost-effective fuel cells can provide a major way to build a low-carbon and sustainable future for the earth; the basic components of PEMFCs are a seven-in-one "sandwich" structure. The proton exchange membrane is in contact with the cathode and cathode catalyst layers CL, and then with the two gas diffusion layers GDL. The typical CL is composed of Pt nanoparticles, carbon carriers and resin ionomers to form a proton conduction network; the catalyst used in PEMFC is carbon-supported platinum nanoparticles, which are used to accelerate the slow oxygen reduction reaction (ORR) and promote the hydrogen oxidation reaction (HOR). The perfluorosulfonic acid membrane is used for cathode and cathode electron and proton conduction. Its structure involves a wide range of various particles and pores, including Pt nanoparticles on carbon carriers and 3-10nm primary pores on a microscopic scale. The reactions in the catalytic layer include electrochemical reactions, diffusion of hydrogen or hydrocarbon fuel anode and oxygen cathode, migration and diffusion of protons, migration of electrons, and water transport by diffusion, permeation, electroosmotic drag and water evaporation / condensation. The current is generated / consumed at the Pt nanoparticles randomly dispersed on the high specific surface carbon carrier.
[0003] The ideal CL structure can achieve the best balance between electronic conductivity, proton conductivity, gaseous reactant transport and catalyst utilization. Achieving and optimizing this balance is the key to high-performance CLs, which requires the catalyst particles to be in close contact with the ionomer. At the same time, in order to facilitate gas transport and water management, the catalytic layer needs to have high porosity and suitable pore size distribution (PSD).
[0004] Pores are the spaces between the solid components of fuel cells. They are a key requirement for efficient CL because it is through these channels that the reactant gases reach the catalyst surface. They also play an important role in water management, both by removing excess water in the ORR reaction and by maintaining the integrity of the hydrated membrane and ionomers. Traditional support particles are spherical, agglomerated into clusters (aggregates), separated by cavities or ionomers.
[0005] Pores are the void spaces within each particle, between each particle in a cluster, and between each cluster. The pore size is the distance between two opposing walls of a pore. Porosity is the ratio of total pore volume to apparent total volume, usually expressed as a percentage or fraction. Micropores are pores with a pore size less than 2 nm, which are usually caused by channels inside the particles. Mesopores are pores with a pore size between 2 and 50 nm, which may be caused by larger channels inside the particles or voids between particles. Macropores are pores with a pore size greater than 50 nm, which are usually between different particles or clusters. Macropores are called O2 diffusion channels because they are generally considered to be key to gas diffusion, especially in thicker locations in CLs. Pores are defined as primary or secondary pores, with primary pores ranging from 6 to 20 nm and secondary pores ranging from 20 to 100 nm. Researchers generally believe that the interior of pores smaller than 20 nm is not coated by ionomers. Closed or isolated pores are pores that are completely closed and therefore cannot be entered by fluids or gases. Catalysts in closed pores are not electrochemically active, and the pores themselves affect the overall CL structure / density. An ideal catalyst layer structure does not contain closed pores, as these pores only serve to increase electrode thickness and reduce catalyst utilization; the morphology, porosity, and PSD of the entire CL depend on the fabrication, ionomer content / distribution, size / structure, and initial porosity / PSD of the support material; porosity and PSD have been reported to play an important role in catalyst durability. Depending on the pore size, localized water can increase O2 transport resistance by forcing gas to diffuse through water-flooded pores to the catalyst surface, which, combined with a more tortuous gas diffusion path and the possibility that ionomers may partially block the pore entrance, further limits gas diffusion O2 transport. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a porous membrane electrode for a proton exchange membrane fuel cell and its application, using a pore-forming agent and introducing pores into the catalyst layer by washing with acid and hydrogen peroxide, thereby reducing the oxygen transmission resistance during battery operation and improving battery performance.
[0007] The technical solution adopted by the present invention is:
[0008] A method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, comprising the following steps:
[0009] Step S1. mixing a catalyst, water, an organic alcohol and a perfluorosulfonic acid resin solution to obtain a catalyst mixture;
[0010] Step S2. adding a pore-forming agent to the catalyst mixture, and placing the mixture in an ultrasonic disperser for ultrasonication to obtain a uniformly dispersed catalyst slurry;
[0011] Step S3. coating the catalyst slurry on the substrate, and obtaining a catalyst layer containing a pore-forming agent after drying;
[0012] Step S4. The catalyst layer prepared in step S3 is immersed in an acid solution, then washed and dried, and then immersed in hydrogen peroxide, and finally the catalyst layer is washed and dried to obtain a cathode catalyst layer and / or an anode catalyst layer;
[0013] Step S5. Stack the cathode catalyst layer, the proton exchange membrane, and the anode catalyst layer in sequence from top to bottom and bond them together by thermal transfer to obtain a proton exchange membrane fuel cell porous membrane electrode.
[0014] Preferably, the method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, wherein: the solid content of the catalyst mixture in step S1 is 3-15%, the catalyst is a platinum-based catalyst, and the platinum-based catalyst is selected from one of Pt / C, PtCo, PtPd, and PtRu; the mass ratio of the resin in the perfluorosulfonic acid resin solution to the mass ratio of the carbon in the platinum-based catalyst is 0.5-1.2, and the volume ratio of water to the organic alcohol is 3-1:1.
[0015] Preferably, in the method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, the pore-forming agent in step S2 is selected from one of nano-nickel, nano-zinc, nano-aluminum and nano-cobalt, and the molar ratio of platinum to the pore-forming agent in the platinum-based catalyst is 0.2-5:1.
[0016] Preferably, in the method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, the ultrasonic time in step S2 is 20-120 min, and the ultrasonic temperature is 20° C.-25° C.
[0017] Preferably, in the method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, the process for coating the catalyst slurry on the substrate in step S3 is selected from one of Meyer rod coating, spray coating, slit coating and screen printing.
[0018] Preferably, in the method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, the acid in the acid solution in step S4 is selected from one of sulfuric acid, hydrochloric acid and nitric acid, the concentration of the acid solution is 0.1-1M, and the immersion time is 2-10h.
[0019] Preferably, in the method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, the concentration of the hydrogen peroxide in step S4 is 3-30%, and the immersion time is 2-10 hours.
[0020] The present invention also provides an application of a proton exchange membrane fuel cell porous membrane electrode prepared by the proton exchange membrane fuel cell porous membrane electrode preparation method. The proton exchange membrane fuel cell porous membrane electrode is used in a fuel cell.
[0021] Advantages of the present invention:
[0022] (1) Compared with the conventional membrane electrode preparation method, the preparation method of the proton exchange membrane fuel cell porous membrane electrode of the present invention has a simple and easy preparation process, low cost, low energy consumption, and is easy to achieve large-scale production.
[0023] (2) The preparation method of the porous membrane electrode for a proton exchange membrane fuel cell of the present invention introduces a pore-forming agent during the preparation process, which can independently design the porosity and pore size distribution of the catalyst layer. The pore-forming agent is cheap and easily available on the market, which provides the possibility for subsequent large-scale production. The pore-forming agent is removed by a step-by-step impregnation method using a low-concentration acid and a hydrogen peroxide solution. Not only is the removal effect more thorough, but the process is also gentle and safe, the integrity of the catalyst layer structure is maintained, and the stable operation of the subsequent membrane electrode is guaranteed. The pores introduced in the catalyst layer not only allow the catalyst to be better exposed and participate in the reaction, increase the three-phase interface of the reaction, thereby improving the catalyst utilization rate, but also reduce the oxygen mass transfer resistance, thereby optimizing the material transport in the membrane electrode and improving the battery performance.
[0024] (3) The preparation method of the porous membrane electrode for proton exchange membrane fuel cells of the present invention and its application. The porous catalyst layer preparation method involved can not only be applied to proton exchange membrane fuel cells, but also has great application potential in the fields of water electrolysis and energy storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the SEM image of Example 1 of the present invention.
[0026] Figure 2 This is the SEM image of Example 2 of the present invention.
[0027] Figure 3 This is the SEM image of Example 3 of the present invention.
[0028] Figure 4 This is the SEM image of Example 4 of the present invention.
[0029] Figure 5 This is the SEM image of Comparative Example 1 of the present invention.
[0030] Figure 6This is the SEM image of Comparative Example 2 of the present invention.
[0031] Figure 7 The polarization curves and surface resistance diagrams of Example 1 of the present invention and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with specific drawings and embodiments.
[0033] Example 1
[0034] A method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, comprising the following steps:
[0035] Step S1. 32 mg of Pt / C catalyst was completely wetted with 600 μl of deionized water, and then 275 μl of n-propanol was added to obtain a catalyst slurry, 160 μg of DuPont D2020 solution was weighed and added to the catalyst slurry, and stirred at a speed of 600 rpm for 10 min to obtain a catalyst mixture; the solid content of the catalyst mixture was 6%, and the mass ratio of the resin in the perfluorosulfonic acid resin solution to the carbon in the platinum-based catalyst was 1.0;
[0036] Step S2. Add 3.5 mg of nano nickel powder to the catalyst mixture, and place the mixture in an ultrasonic disperser for 60 min at an ultrasonic temperature of 20° C. to obtain a uniformly dispersed catalyst slurry; the molar ratio of Pt to pore-forming agent in the Pt / C catalyst is 3:1;
[0037] Step S3. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 3 μm, the coating temperature is 100° C., and the first catalyst layer is obtained after drying. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 12 μm, the coating temperature is 100° C., and the second catalyst layer is obtained after drying.
[0038] Step S4. The first catalytic layer and the second catalytic layer prepared in step S3 are immersed in a 0.5M sulfuric acid solution for 3 hours, then washed with deionized water and dried at 100°C for 30 minutes, and then the first catalytic layer and the second catalytic layer are immersed in 7.5% hydrogen peroxide for 3 hours, and finally the first catalytic layer and the second catalytic layer are washed and dried at 100°C for 30 minutes to obtain an anode catalytic layer and a cathode catalytic layer. The Pt loading of the anode catalytic layer is 0.102 mg / cm 2 The Pt loading of the cathode catalyst layer is 0.314 mg / cm 2 ;
[0039] Step S5. Stack the cathode catalyst layer, the proton exchange membrane, and the anode catalyst layer from top to bottom and adhere them by thermal transfer to obtain a proton exchange membrane fuel cell porous membrane electrode; combine the proton exchange membrane fuel cell porous membrane electrode and GDL into a single cell and test it, wherein the transfer pressure is 1300kg, the transfer temperature is 140°C, the proton exchange membrane is Gore PEM, and the GDL uses Toray GDL.
[0040] Example 2
[0041] A method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, comprising the following steps:
[0042] Step S1. 32 mg of Pt / C catalyst was completely wetted with 600 μl of deionized water, and then 275 μl of n-propanol was added to obtain a catalyst slurry, 160 μg of DuPont D2020 solution was weighed and added to the catalyst slurry, and stirred at a speed of 600 rpm for 10 min to obtain a catalyst mixture; the solid content of the catalyst mixture was 6%, and the mass ratio of the resin in the perfluorosulfonic acid resin solution to the carbon in the platinum-based catalyst was 1.0;
[0043] Step S2. Add 3.5 mg of nano nickel powder to the catalyst mixture, and place the mixture in an ultrasonic disperser for 60 min at an ultrasonic temperature of 20° C. to obtain a uniformly dispersed catalyst slurry; the molar ratio of Pt to pore-forming agent in the Pt / C catalyst is 3:1;
[0044] Step S3. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 3 μm, the coating temperature is 100°C, and the first catalyst layer is obtained after drying. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 12 μm, the coating temperature is 100°C, and the second catalyst layer is obtained after drying.
[0045] Step S4. The first catalytic layer and the second catalytic layer prepared in step S3 are immersed in a 0.5M sulfuric acid solution for 3 hours, then washed with deionized water and dried at 100°C for 30 minutes, and then the first catalytic layer and the second catalytic layer are immersed in 3% hydrogen peroxide for 3 hours, and finally the first catalytic layer and the second catalytic layer are washed and dried at 100°C for 30 minutes to obtain an anode catalytic layer and a cathode catalytic layer, and the Pt loading of the anode catalytic layer and the cathode catalytic layer is 0.098 mg / cm 2 and 0.305mg / cm 2 ;
[0046] Step S5. Stack the cathode catalyst layer, the proton exchange membrane, and the anode catalyst layer from top to bottom in sequence and bond them together by thermal transfer to obtain a proton exchange membrane fuel cell porous membrane electrode; combine the proton exchange membrane fuel cell porous membrane electrode and GDL into a single cell and test it, wherein the transfer pressure is 1300kg, the transfer temperature is 140°C, the proton exchange membrane is Gore PEM, and the GDL uses Toray GDL.
[0047] Example 3
[0048] A method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, comprising the following steps:
[0049] Step S1. 32 mg of Pt / C catalyst was completely wetted with 600 μl of deionized water, and then 275 μl of n-propanol was added to obtain a catalyst slurry, 160 μg of DuPont D2020 solution was weighed and added to the catalyst slurry, and stirred at a speed of 600 rpm for 10 min to obtain a catalyst mixture; the solid content of the catalyst mixture was 6%, and the mass ratio of the resin in the perfluorosulfonic acid resin solution to the carbon in the platinum-based catalyst was 1.0;
[0050] Step S2. Add 3.5 mg of nano nickel powder to the catalyst mixture, and place the mixture in an ultrasonic disperser for 60 min at an ultrasonic temperature of 20° C. to obtain a uniformly dispersed catalyst slurry; the molar ratio of Pt to pore-forming agent in the Pt / C catalyst is 3:1;
[0051] Step S3. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 3 μm, the coating temperature is 100°C, and the first catalyst layer is obtained after drying. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 12 μm, the coating temperature is 100°C, and the second catalyst layer is obtained after drying.
[0052] Step S4. The first catalytic layer and the second catalytic layer prepared in step S3 are immersed in a 0.5M sulfuric acid solution for 3 hours, then washed with deionized water and dried at 100°C for 30 minutes, and then immersed in 5% hydrogen peroxide for 3 hours. Finally, the first catalytic layer and the second catalytic layer are washed and dried at 100°C for 30 minutes to obtain an anode catalytic layer and a cathode catalytic layer. The Pt loading of the anode catalytic layer and the cathode catalytic layer is 0.108 mg / cm 2 and 0.307mg / cm 2 ;
[0053] Step S5. Stack the cathode catalyst layer, the proton exchange membrane, and the anode catalyst layer from top to bottom in sequence and bond them together by thermal transfer to obtain a proton exchange membrane fuel cell porous membrane electrode; combine the proton exchange membrane fuel cell porous membrane electrode and GDL into a single cell and test it, wherein the transfer pressure is 1300kg, the transfer temperature is 140°C, the proton exchange membrane is Gore PEM, and the GDL uses Toray GDL.
[0054] Example 4
[0055] A method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, comprising the following steps:
[0056] Step S1. 32 mg of Pt / C catalyst was completely wetted with 600 μl of deionized water, and then 275 μl of n-propanol was added to obtain a catalyst slurry, 160 μg of DuPont D2020 solution was weighed and added to the catalyst slurry, and stirred at a speed of 600 rpm for 10 min to obtain a catalyst mixture; the solid content of the catalyst mixture was 6%, and the mass ratio of the resin in the perfluorosulfonic acid resin solution to the carbon in the platinum-based catalyst was 1.0;
[0057] Step S2. Add 3.5 mg of nano nickel powder to the catalyst mixture, and place the mixture in an ultrasonic disperser for 60 min at an ultrasonic temperature of 20° C. to obtain a uniformly dispersed catalyst slurry; the molar ratio of Pt to pore-forming agent in the Pt / C catalyst is 3:1;
[0058] Step S3. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 3 μm, the coating temperature is 100°C, and the first catalyst layer is obtained after drying. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 12 μm, the coating temperature is 100°C, and the second catalyst layer is obtained after drying.
[0059] Step S4. The first catalytic layer and the second catalytic layer prepared in step S3 are immersed in a 0.5M sulfuric acid solution for 3 hours, then washed with deionized water and dried at 100°C for 30 minutes, and then the first catalytic layer and the second catalytic layer are immersed in 30% hydrogen peroxide for 3 hours, and finally the first catalytic layer and the second catalytic layer are washed and dried at 100°C for 30 minutes to obtain an anode catalytic layer and a cathode catalytic layer, and the Pt loading of the anode catalytic layer and the cathode catalytic layer is 0.099 mg / cm 2 and 0.312mg / cm 2 ;
[0060] Step S5. Stack the cathode catalyst layer, the proton exchange membrane, and the anode catalyst layer from top to bottom in sequence and bond them together by thermal transfer to obtain a proton exchange membrane fuel cell porous membrane electrode; combine the proton exchange membrane fuel cell porous membrane electrode and GDL into a single cell and test it, wherein the transfer pressure is 1300kg, the transfer temperature is 140°C, the proton exchange membrane is Gore PEM, and the GDL uses Toray GDL.
[0061] Comparative Example 1
[0062] A method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, comprising the following steps:
[0063] Step S1. 32 mg of Pt / C catalyst was completely wetted with 600 μl of deionized water, and then 275 μl of n-propanol was added to obtain a catalyst slurry, 160 μg of DuPont D2020 solution was weighed and added to the catalyst slurry, and stirred at a speed of 600 rpm for 10 min to obtain a catalyst mixture; the solid content of the catalyst mixture was 6%, and the mass ratio of the resin in the perfluorosulfonic acid resin solution to the carbon in the platinum-based catalyst was 1.0;
[0064] Step S2. placing the catalyst mixture in an ultrasonic disperser and ultrasonicating for 60 min at a temperature of 20° C. to obtain a uniformly dispersed catalyst slurry;
[0065] Step S3. The catalyst slurry is applied on the substrate by scraping with a Meyer rod to form a catalyst slurry layer with a thickness of 3 μm, the scraping temperature is 100°C, and the anode catalyst layer is obtained after drying. The catalyst slurry is applied on the substrate by scraping with a Meyer rod to form a catalyst slurry layer with a thickness of 12 μm, the scraping temperature is 100°C, and the cathode catalyst layer is obtained after drying. The Pt loadings of the anode catalyst layer and the cathode catalyst layer are 0.103 mg / cm 2 and 0.311mg / cm 2 ;
[0066] Step S4. Stack the cathode catalyst layer, the proton exchange membrane, and the anode catalyst layer and bond them together by thermal transfer to obtain a proton exchange membrane fuel cell porous membrane electrode; combine the proton exchange membrane fuel cell porous membrane electrode and GDL into a single cell and test it, wherein the transfer pressure is 1300kg, the transfer temperature is 140°C, the proton exchange membrane is Gore PEM, and the GDL uses Toray GDL.
[0067] Comparative Example 2
[0068] A method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, comprising the following steps:
[0069] Step S1. 32 mg of Pt / C catalyst was completely wetted with 600 μl of deionized water, and then 275 μl of n-propanol was added to obtain a catalyst slurry, 160 μg of DuPont D2020 solution was weighed and added to the catalyst slurry, and stirred at a speed of 600 rpm for 10 min to obtain a catalyst mixture; the solid content of the catalyst mixture was 6%, and the mass ratio of the resin in the perfluorosulfonic acid resin solution to the carbon in the platinum-based catalyst was 1.0;
[0070] Step S2. Add 3.5 mg of nano nickel powder to the catalyst mixture, and place the mixture in an ultrasonic disperser for 60 min at an ultrasonic temperature of 20° C. to obtain a uniformly dispersed catalyst slurry; the molar ratio of Pt to pore-forming agent in the Pt / C catalyst is 3:1;
[0071] Step S3. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 3 μm, the coating temperature is 100°C, and the first catalyst layer is obtained after drying. The catalyst slurry is applied on the substrate by a Meyer rod to form a catalyst slurry layer with a thickness of 12 μm, the coating temperature is 100°C, and the second catalyst layer is obtained after drying.
[0072] Step S4. The first catalyst layer and the second catalyst layer prepared in step S3 were immersed in a 0.5M sulfuric acid solution for 3 h, then washed with deionized water and dried at 100°C for 30 min to obtain an anode catalyst layer and a cathode catalyst layer. The Pt loading of the anode catalyst layer and the cathode catalyst layer was 0.11 mg / cm 2 and 0.304mg / cm 2 ;
[0073] Step S5. Stack the cathode catalyst layer, the proton exchange membrane, and the anode catalyst layer from top to bottom in sequence and bond them together by thermal transfer to obtain a proton exchange membrane fuel cell porous membrane electrode; combine the proton exchange membrane fuel cell porous membrane electrode and GDL into a single cell and test it, wherein the transfer pressure is 1300kg, the transfer temperature is 140°C, the proton exchange membrane is Gore PEM, and the GDL uses Toray GDL.
[0074] The cathode catalyst layers prepared in Examples 1-4 and Comparative Examples 1-2 were characterized by EDS. The results are shown in Table 1.
[0075] Table 1
[0076]
[0077] The present invention introduces a pore-forming agent into the catalyst layer, immerses it in hydrogen peroxide with different concentrations after dilute acid immersion, and then dries and takes it out, thereby successfully preparing a membrane electrode with obvious pores.
[0078] according to Figure 1According to SEM and Table 1, the residual amount of pore-forming agent in the catalyst layer of Example 1 is 0, which indicates that the method of first acid washing with 0.5MH2SO4 solution for 3 hours and then soaking in 7.5% H2O2 solution for 3 hours is very thorough in removing the pore-forming agent on the surface of the catalyst layer. 7.5% is the optimal H2O2 solution concentration explored by the present invention. Figure 1 and Figure 5 By comparison, the pores of 50-200 nm are increased on the surface of the catalyst layer, achieving the purpose of forming pores in the catalyst layer of the present invention. Figure 1-4 As shown in Table 1, the surface of the porous membrane electrode prepared by the present invention is covered with uniform pores. Figure 5 The traditional membrane electrode has significantly fewer and more uneven pores on its surface, which is very unfavorable for the internal material transport during battery operation.
[0079] according to Figure 6 It can be seen that the method of impregnation with only 0.5M H2SO4 is not ideal for removing the pore-forming agent. The residual pore-forming agent particles are clearly visible on the catalyst surface. The residual pore-forming agent will reduce the advantage of the porous electrode in material transfer and even affect the proton exchange membrane, thereby causing the stability of the single cell operation to decrease.
[0080] according to Figure 7 It can be seen that the introduction of pores in the catalyst layer by pore creation increases the three-phase interface of the reaction, reduces the material transfer resistance, and increases the membrane electrode from the traditional 0.65V@1.6A to 0.65V@2.17A. However, the performance of Comparative Example 2 is not significantly improved compared with the traditional membrane electrode, which is closely related to the fact that a large amount of the pore-forming agent introduced remains in the catalyst layer. Compared with the traditional membrane electrode, the membrane electrode of Example 1 has a higher porosity, better material transfer efficiency, and lower oxygen mass transfer resistance, thereby effectively improving the utilization rate of the precious metal Pt and enhancing the performance of the membrane electrode.
[0081] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a porous membrane electrode for a proton exchange membrane fuel cell, characterized in that: The following steps are involved: Step S1. mixing a catalyst, water, an organic alcohol and a perfluorosulfonic acid resin solution to obtain a catalyst mixture; Step S2. adding a pore-forming agent to the catalyst mixture, and placing the catalyst mixture in an ultrasonic disperser for ultrasonication to obtain a uniformly dispersed catalyst slurry; Step S3. coating the catalyst slurry on the substrate, and obtaining a catalyst layer containing a pore-forming agent after drying; Step S4. The catalyst layer prepared in step S3 is immersed in an acid solution, then washed and dried, and then immersed in hydrogen peroxide, and finally the catalyst layer is washed and dried to obtain a cathode catalyst layer and / or an anode catalyst layer; Step S5. Stack the cathode catalyst layer, the proton exchange membrane, and the anode catalyst layer in sequence from top to bottom and bond them together by thermal transfer to obtain a proton exchange membrane fuel cell porous membrane electrode.
2. The method for preparing a porous membrane electrode for a proton exchange membrane fuel cell according to claim 1, characterized in that: The solid content of the catalyst mixture in step S1 is 3-15%, the catalyst is a platinum-based catalyst, and the platinum-based catalyst is selected from one of Pt / C, PtCo, PtPd, and PtRu; the mass ratio of the resin in the perfluorosulfonic acid resin solution to the mass ratio of the carbon in the platinum-based catalyst is 0.5-1.2, and the volume ratio of the water to the organic alcohol is 3-1:
1.
3. The method for preparing a porous membrane electrode for a proton exchange membrane fuel cell according to claim 2, characterized in that: In step S2, the pore-forming agent is selected from one of nano-nickel, nano-zinc, nano-aluminum and nano-cobalt, and the molar ratio of platinum to the pore-forming agent in the platinum-based catalyst is 0.2-5:
1.
4. The method for preparing a porous membrane electrode for a proton exchange membrane fuel cell according to claim 1, characterized in that: In step S2, the ultrasonic time is 20-120 min, and the ultrasonic temperature is 20°C-25°C.
5. The method for preparing a porous membrane electrode for a proton exchange membrane fuel cell according to claim 1, characterized in that: In step S3, the process for coating the catalyst slurry on the substrate is selected from one of Meyer rod coating, spray coating, slit coating and screen printing.
6. The method for preparing a porous membrane electrode for a proton exchange membrane fuel cell according to claim 1, characterized in that: The acid in the acid solution in step S4 is selected from one of sulfuric acid, hydrochloric acid and nitric acid, the concentration of the acid solution is 0.1-1 M, and the immersion time is 2-10 h.
7. The method for preparing a porous membrane electrode for a proton exchange membrane fuel cell according to claim 1, characterized in that: In step S4, the concentration of hydrogen peroxide is 3-30%, and the immersion time is 2-10 h.
8. Use of the proton exchange membrane fuel cell porous membrane electrode prepared by the method for preparing a proton exchange membrane fuel cell porous membrane electrode according to any one of claims 1 to 7, characterized in that: The proton exchange membrane fuel cell porous membrane electrode is used in a fuel cell.
Citation Information
Cited By
Porous cathode electrode preparation method based on bubble precipitation pore forming
CN119252946A