Zirconium oxide medium, bearing ball, and method for producing same

By adjusting the chemical composition and microstructure of the zirconia sintered body, the problems of cracking and defects of the zirconia medium under high load conditions are solved, and its wear resistance and durability are improved, ensuring the high purity of the powder and Uniformity of mechanical properties.

CN119013101AActive Publication Date: 2024-11-22NIKKATO CORPORATION
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202380033115.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-25
Filing Date
2023-04-03
Publication Date
2024-11-22
Estimated Expiration
2043-04-03

AI Technical Summary

Technical Problem

The existing zirconia medium is prone to cracking and defects under high load conditions, resulting in a decrease in strength deviation and wear resistance of the medium during crushing and dispersion treatment, and it is difficult to suppress foreign matter mixing, affecting the high purity of the powder.

Method used

By adjusting the chemical composition and microstructure of ZrO2-Y2O3-type zirconia sintered bodies, we ensure that the molar ratio of Y2O3/ZrO2 is within the range of 2.5/97.5 to 3.2/96.8, the Al2O3 content is within the range of 0.1% to 30.0%, and the relative density is 95 Above % and the average grain diameter is between 0.25μm and 0.50μm, the crushing load value and Weibull coefficient meet specific standards, and the coefficient of variation of the media diameter is confirmed by scanning electron microscopy to improve the wear resistance of the media and durability.

Benefits of technology

Effectively inhibits cracking and defects of zirconia medium under high load conditions, improves its wear resistance and durability, ensures the high purity of the powder and the uniformity of mechanical properties, and meets the mechanics of zirconia bearing balls Require.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013101A_ABST
    Figure CN119013101A_ABST
Patent Text Reader

Abstract

Provided are: a zirconia medium having improved wear resistance and durability; a zirconia bearing ball; and a method for producing the zirconia bearing ball. A zirconia medium which comprises (a) a ZrO2-Y2O3-based zirconia sintered body having a Y2O3 / ZrO2 molar ratio in the range of 2.5 / 97.5 to 3.2 / 96.8 inclusive, (b) an Al2O3 content in the range of 0.1% by mass to 30.0% by mass inclusive, (c) a tetragonal zirconia content in the range of 90% by volume or more, (d) a relative density of 95% or more, (e) an average crystal grain diameter in the range of 0.25 [mu] m to 0.50 [mu] m inclusive, and (e) an average crystal grain diameter in the range of 0.25 [mu] m to 0.50 [mu] m inclusive. (f) the minimum value of the crush load value satisfies Pmin (N) > 600 * D2.0 (D is the average value of the medium diameter), (g) the Weibull coefficient of the crush load value is 10 or more, and (h) the coefficient of variation of the medium diameter is less than 6%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to zirconium oxide media, bearing balls and methods for making the same. Background Art

[0002] In recent years, electronic component materials such as multilayer ceramic capacitors are being miniaturized and improved in performance. In the manufacture of inorganic powders used as raw materials, emphasis is placed on micronization, high dispersion, and high purity. In the micronization process of such powders, a bead mill containing a medium containing a smaller inorganic sintered body is used as a medium for pulverization and dispersion. In the mill, the micro-medium is processed by high-speed stirring for efficient pulverization and dispersion. Therefore, a large load is applied to the medium used, and Y2O3-reinforced zirconia micro-medium with excellent impact resistance and wear resistance is used.

[0003] Since the micro-media is small in size, a large amount of it needs to be put into the mill. If there is even a small amount of low-strength media among the media put in, the high-speed rotation in the mill will bring a high load to the media, which can easily cause the media to break. If the damage to the media causes fragments to be generated, there is a risk that the fragments will be crushed and mixed into the processed powder as foreign matter. In addition, depending on the crushing and dispersion conditions, the slurry temperature in the mill may rise, and foreign matter may be mixed in due to the deterioration of the strength of the media and the reduction of wear resistance.

[0004] Patent Document 1 discloses a method for dispersing a pigment in a solution, wherein a pigment having an average particle size of 40 to 192 μm and a density of 5.9 g / cm 3 Zirconia sintered beads with a sphericity of 1.07 or less.

[0005] However, when a bead mill is used to grind and disperse powder, it only suppresses the deviation of the average particle size, density, and sphericity, but cannot suppress the occurrence of cracks and defects caused by the strength of the medium and the stress concentration on the defects existing inside the medium. In other words, Patent Document 1 does not mention the deviation of the bead strength. Even if the deviation of the average particle size, density, and sphericity is suppressed, the deviation of the strength will not be suppressed.

[0006] Patent document 2 discloses a ZrO2-Y2O3-based zirconia sintered body, which obtains wear resistance by controlling the chemical composition and microstructure of the medium used for crushing and dispersion. Patent document 2 discloses that the ZrO2-Y2O3-based zirconia sintered body has excellent wear resistance in crushing and dispersing hard powder.

[0007] However, there is no record of suppressing the deviation of the characteristics of all micro-mediums even if the chemical composition of the ZrO2-Y2O3-based zirconia sintered body is adjusted. When used as micro-mediums subjected to high loads, if not all micro-mediums meet the specified strength, there is a risk of cracking and defecting due to stress concentration on micro-mediums with low strength.

[0008] In patent document 3, it is recorded that due to the different granulation methods of the formed sphere before sintering, there is a situation where the size of the average crystal grain size near the center and near the surface of the sintered sphere is different. And it is recorded that if the average crystal grain size of the sphere is larger than that near the surface near the center, then wear is significantly carried out in the initial stage, and the amount of impurities mixed surges. And it is recorded that if the average crystal grain size of the sphere is smaller than that near the surface near the center, then the internal void becomes more, because the void becomes the starting point of destruction, so the strength is greatly reduced. Therefore, it is disclosed that the specific surface area and the average secondary particle size of the ZrO2 powder formed by the formed sphere before sintering are adjusted to a specific range, and the chemical composition of the content of Y2O3, Al2O3, Fe, Ti, etc. is in a specific range, so as to adjust the uniformity of the average crystal grain size near the center and near the surface of each sphere.

[0009] However, even if the uniformity of the average crystal grain size inside the sphere and near the surface is adjusted, if the deviation in the strength of all the micro-mediums is not suppressed, there is a risk of cracking and defects when the processed powder is crushed and dispersed due to stress concentration on the micro-mediums with slightly lower strength.

[0010] Patent document 4 discloses a zirconia sintered body which, by controlling the molar ratio of Y2O3 to ZrO2, the content of Al2O3, the combined content of SiO2 and TiO2, and the average grain size, exhibits excellent wear resistance and durability over a long period of time in warm water or a high-humidity atmosphere at around 100°C or below 100°C.

[0011] However, there is no record of suppressing the deviation of the characteristics of all micro-mediums even if the chemical composition of the ZrO2-Y2O3-based zirconia sintered body is adjusted. When used as micro-mediums that bear high loads, if not all micro-mediums meet the specified strength, there is a risk of cracking and defecting due to the slight concentration of stress on micro-mediums with low strength, which may lead to reduced durability, as in Patent Document 2.

[0012] Prior art literature

[0013] Patent Literature

[0014] Patent Document 1: Japanese Patent Application Laid-Open No. 7-155577

[0015] Patent Document 2: Japanese Patent Application Publication No. 2014-205586

[0016] Patent Document 3: Japanese Patent Application Publication No. 2004-315246

[0017] Patent Document 4: Japanese Patent Application Publication No. 2004-307339 Summary of the invention

[0018] Problems to be solved by the invention

[0019] The present invention aims to provide a zirconia medium, a bearing ball and a method for producing the same, which suppresses the variation in the medium shape and the variation in the mechanical characteristics and improves the wear resistance and durability.

[0020] Means of solving the problem

[0021] A first aspect of the present invention is a zirconia medium that satisfies the following requirements (a) to (h):

[0022] (a) a sintered body comprising ZrO2-Y2O3-based zirconia, wherein the molar ratio of Y2O3 / ZrO2 is within the range of 2.5 / 97.5 or more and 3.2 / 96.8 or less,

[0023] (b) the content of Al2O3 is in the range of 0.1 mass % or more and 30.0 mass % or less,

[0024] (c) containing 90% by volume or more of tetragonal zirconium oxide,

[0025] (d) relative density is above 95%,

[0026] (e) the average grain size is within the range of 0.25 μm or more and 0.50 μm or less,

[0027] (f) The minimum value of the crushing load measured at a crosshead speed of 0.5 mm / min satisfies Pmin (N) > 600 × D 2.0 (D is the average value of the medium diameter),

[0028] (g) The Weibull coefficient of the crushing load value is greater than 10,

[0029] (h) The maximum diameter of the medium that can be confirmed in the SEM image confirmed by using a scanning electron microscope is defined as the medium diameter, and the coefficient of variation of the medium diameter derived from the average value and standard deviation of the medium diameters of 200 media is less than 6%.

[0030] A second aspect of the present invention is a zirconia bearing ball, wherein the following requirements are satisfied:

[0031] (a) a sintered body comprising ZrO2-Y2O3-based zirconia, wherein the molar ratio of Y2O3 / ZrO2 is within the range of 2.5 / 97.5 or more and 3.2 / 96.8 or less,

[0032] (b) the content of Al2O3 is in the range of 0.1 mass % or more and 30.0 mass % or less,

[0033] (c) containing 90% by volume or more of tetragonal zirconium oxide,

[0034] (d) relative density is above 95%,

[0035] (e) the average grain size is within the range of 0.25 μm or more and 0.50 μm or less,

[0036] (f) The minimum value of the crushing load measured at a crosshead speed of 0.5 mm / min satisfies Pmin (N) > 600 × D 2.0 (D is the average value of the medium diameter),

[0037] (g) The Weibull coefficient of the crushing load value is greater than 10,

[0038] (h) the maximum diameter of the medium that can be confirmed in the SEM image confirmed by using a scanning electron microscope is taken as the medium diameter, and the coefficient of variation of the medium diameter derived from the average value and standard deviation of the medium diameters of 200 media is less than 6%,

[0039] (x) Fracture toughness higher than 5.0 MPa·m 1 / 2 ,

[0040] (y) The flexural strength is higher than 1100MPa and the Weibull modulus of flexural strength is higher than 7.

[0041] A third aspect of the present invention is a method for producing a zirconia medium including the following sintered body, comprising:

[0042] (p) mixing a zirconium raw material and a yttrium raw material so that the Y2O3 / ZrO2 molar ratio is within the range of 2.5 / 97.5 or more and 3.2 / 96.8 or less, hydrolyzing the mixture, and pre-calcining the resulting hydrate of zirconium and yttrium at a temperature within the range of 600°C or more and 1200°C or less to obtain a synthetic powder,

[0043] (q) mixing the obtained synthetic powder with Al2O3 powder to obtain a mixed powder in such a manner that the content of Al2O3 is within the range of 0.1 mass % to 30.0 mass % with respect to the total amount,

[0044] (r) drying the mixed powder slurry obtained by wet pulverizing and / or dispersing the mixed powder to obtain a powder having a specific surface area of ​​5 m 2 / g or more and 10m 2 / g or less,

[0045] (s) pulverizing and / or dispersing the mixed powder slurry by a wet method in such a manner that the average particle size having a cumulative frequency of 50% in the volume-based particle size distribution measured by a laser diffraction method in accordance with JIS Z8825 is within a range of 0.3 μm to 0.6 μm,

[0046] (t) preparing a molding powder obtained by drying and granulating powder in a slurry for measuring the average particle size of agglomerated powder obtained by mixing 1 part by mass of a powder obtained by drying the mixed powder slurry with 100 parts by mass of a molding solvent in such a manner that the average particle size of agglomerated powder having a cumulative frequency of 50% in a volume-based particle size distribution measured in accordance with JIS Z8825 is within a range of 1 μm or more and 5 μm or less,

[0047] (u) granulating the molding powder to obtain a molded body,

[0048] (v) The molded body is sintered at a temperature within a range of 1250° C. to 1600° C. to obtain a ZrO 2 —Y 2 O 3 -based zirconia sintered body.

[0049] A fourth aspect of the present invention is a method for producing a zirconia bearing ball including a sintered body, comprising:

[0050] (p) mixing a zirconium raw material and a yttrium raw material so that the Y2O3 / ZrO2 molar ratio is within the range of 2.5 / 97.5 or more and 3.2 / 96.8 or less, hydrolyzing the mixture, and pre-calcining the resulting hydrate of zirconium and yttrium at a temperature within the range of 600°C or more and 1200°C or less to obtain a synthetic powder,

[0051] (q) mixing the obtained synthetic powder with Al2O3 powder to obtain a mixed powder in such a manner that the content of Al2O3 is within the range of 0.1 mass % to 30.0 mass % with respect to the total amount,

[0052] (r) drying the mixed powder slurry obtained by wet pulverizing and / or dispersing the mixed powder to obtain a powder having a specific surface area of ​​5 m 2 / g or more and 10m 2 / g or less,

[0053] (s) pulverizing and / or dispersing the mixed powder slurry by a wet method in such a manner that the average particle size having a cumulative frequency of 50% in the volume-based particle size distribution measured by a laser diffraction method in accordance with JIS Z8825 is within a range of 0.3 μm to 0.6 μm,

[0054] (t) preparing a molding powder obtained by drying and granulating powder in a slurry for measuring the average particle size of agglomerated powder obtained by mixing 1 part by mass of a powder obtained by drying the mixed powder slurry with 100 parts by mass of a molding solvent in such a manner that the average particle size of agglomerated powder having a cumulative frequency of 50% in a volume-based particle size distribution measured in accordance with JIS Z8825 is within a range of 1 μm or more and 5 μm or less,

[0055] (u) granulating the molding powder to obtain a molded body,

[0056] (v) The molded body is sintered at a temperature within a range of 1250° C. to 1600° C. to obtain a ZrO 2 —Y 2 O 3 -based zirconia sintered body.

[0057] Effects of the Invention

[0058] The present invention can provide a zirconia medium and a zirconia bearing ball having improved wear resistance and durability, and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 This is a photograph of the medium of Example 1 taken with a scanning electron microscope (SEM).

[0060] Figure 2 This is a photograph of the medium of Comparative Example 7 taken with a scanning electron microscope (SEM).

[0061] Figure 3A This is a photograph of the medium of Comparative Example 8 before being subjected to a pulverization and / or dispersion treatment, taken with a scanning electron microscope (SEM).

[0062] Figure 3B This is a photograph of the medium of Comparative Example 8 after the pulverization and / or dispersion treatment, taken with a scanning electron microscope (SEM).

[0063] Figure 4 It is a schematic perspective view showing an example of a bearing. DETAILED DESCRIPTION

[0064] Next, the present invention will be described based on examples of embodiments. However, the present invention is not limited to the embodiments described below.

[0065] The zirconia medium of the present invention satisfies the following requirements (a) to (h), preferably satisfies the following requirement (k), and may also satisfy the following requirement (j), (n) or (o).

[0066] The zirconia bearing ball of the present invention satisfies the following requirements (a) to (h), further satisfies the following requirements (x) and (y), preferably satisfies the following requirement (k), and may also satisfy the following requirements (j), (n) or (o).

[0067] Zirconia medium or zirconia bearing ball, (a) comprising a sintered body of ZrO2-Y2O3 system zirconia, with a Y2O3 / ZrO2 molar ratio in the range of 2.5 / 97.5 or more and 3.2 / 96.8 or less, (b) an Al2O3 content in the range of 0.1 mass % or more and 30.0 mass % or less, (c) containing 90 volume % or more of tetragonal zirconia, (d) a relative density of 95% or more, (e) an average grain size in the range of 0.25 μm or more and 0.50 μm or less, (f) a minimum value of a crushing load value measured at a crosshead speed of 0.5 mm / min satisfies Pmin(N)>600×D 2.0 (D is the average value of the medium diameter), (g) the Weibull coefficient of the crushing load value is greater than 10, and (h) the maximum diameter of the medium that can be confirmed in the SEM image confirmed by using a scanning electron microscope is taken as the medium diameter, and the coefficient of variation of the medium diameter derived from the average value and standard deviation of the medium diameter of 200 media is less than 6%. In this specification, if it is a zirconia bearing ball, "medium" can also be replaced by "bearing ball".

[0068] Zirconia media or zirconia bearing balls include a sintered body of ZrO2-Y2O3-based zirconia, and the chemical composition, crystal phase, relative density, average grain size, minimum value of crushing load value, Weibull coefficient of crushing load value, and coefficient of variation of media diameter of the sintered body are within specific ranges, thereby suppressing the shape deviation of the media and the deviation of mechanical properties such as wear resistance and crushing load value of the media. Zirconia media will not crack or break even when used as a micro-media in a bead mill that rotates at high speed, and can improve durability and wear resistance. Because cracking and breaking of zirconia media are suppressed, the processed powder can be crushed and dispersed while maintaining the high purity of the processed powder. In the case of zirconia bearing balls, because cracking and breaking of the bearing balls are suppressed, bearing balls that meet the specified values ​​described below can be provided.

[0069] A zirconia medium or a zirconia bearing ball, (a) comprising a sintered body of ZrO2-Y2O3-based zirconia, wherein the Y2O3 / ZrO2 molar ratio is within the range of 2.5 / 97.5 to 3.2 / 96.8, or may be within the range of 2.6 / 97.4 to 3.1 / 96.9. If the Y2O3 / ZrO2 molar ratio of the zirconia medium or the zirconia bearing ball is within the range, the monoclinic zirconia is less and the stability of the crystal structure of the tetragonal zirconia is good. If the Y2O3 / ZrO2 molar ratio of the zirconia medium or the zirconia bearing ball is within the range, cracking and defects can be suppressed, and wear resistance and durability can be improved. If the Y2O3 / ZrO2 molar ratio of the zirconia medium or the zirconia bearing ball is lower than 2.5 / 97.5, the content of monoclinic zirconia increases and the stability of the tetragonal zirconia decreases. In addition, if the Y2O3 / ZrO2 molar ratio of the zirconia medium or the zirconia bearing ball is lower than 2.5 / 97.5, fine cracks occur due to stress, which causes cracking and defects, and the wear resistance or durability is reduced. If the Y2O3 / ZrO2 molar ratio of the zirconia medium or the zirconia bearing ball is higher than 3.2 / 96.8, the amount of tetragonal zirconium oxide is reduced and the mechanical strength is reduced. If the mechanical strength is reduced, the medium will crack and be damaged in the bead mill with a high load, and the wear resistance will be reduced. If the mechanical strength is reduced, the wear resistance and durability of the zirconia bearing ball will be reduced. Since HfO2 is usually contained in a small amount in the ZrO2 raw material, the total amount of ZrO2 and HfO2 is taken as the amount of ZrO2. The ZrO2 powder may also contain at least one selected from the group consisting of TiO2, FeO2, MgO, Na2O and K2O. The content of components other than ZrO 2 contained in the ZrO 2 powder can be 0.3 mass % or less relative to the total amount of ZrO 2.

[0070] The content of (b) Al2O3 in the zirconia medium or zirconia bearing ball is within the range of 0.1 mass % to 30.0 mass %. If the content of (b) Al2O3 in the zirconia medium or zirconia bearing ball is within the range, the sinterability of ZrO2 is improved. If the content of (b) Al2O3 in the zirconia medium or zirconia bearing ball is within the range, Al2O3 segregates at the grain boundaries of ZrO2 or also exists as grains of Al2O3, so that the grain boundaries of ZrO2 are strengthened and mechanical properties such as impact resistance are improved. If the content of Al2O3 in the zirconia medium or zirconia bearing ball is less than 0.1 mass %, the effect of improving sinterability and mechanical properties by adding Al2O3 cannot be obtained. If the content of Al2O3 in the zirconia medium or zirconia bearing ball is higher than 30.0 mass %, the content of Al2O3 increases too much, and the sinterability and mechanical properties are reduced instead. The Al2O3 content of the zirconia medium or zirconia bearing ball is preferably in the range of 0.2 mass % to 25 mass %.

[0071] The zirconia medium or zirconia bearing ball preferably (k) contains SiO2 in a range of 0.2 mass % to 1.0 mass %. If a sintered body of ZrO2-Y2O3-based zirconia is used in warm water above 40°C, the grain boundaries are easily eroded by water, and the wear resistance may be greatly reduced. If SiO2 is contained in the zirconia medium or the zirconia bearing ball, the wear resistance can be maintained even when the medium is used in warm water above 40°C. If SiO2 is contained in the zirconia medium or the zirconia bearing ball in a range of 0.2 mass % to 1.0 mass %, the erosion of the grain boundaries of ZrO2 in the sintered body constituting the medium by water can be suppressed, and the wear resistance can be maintained even when the medium is used in warm water above 40°C. If the content of SiO2 in the zirconia medium or the zirconia bearing ball is higher than 1.0 mass %, SiO2 phases may be formed at the grain boundaries of ZrO2, resulting in a reduction in strength. The content of SiO2 in the zirconia medium or the zirconia bearing ball may be in the range of 0.3 mass % to 0.9 mass %, or in the range of 0.4 mass % to 0.7 mass %. When used under conditions where degradation does not occur, such as when not used in warm water at 40°C or above, the content of SiO2 in the zirconia medium or the zirconia bearing ball may be less than 0.2 mass %.

[0072] The zirconia medium or zirconia bearing ball, (c) contains more than 90 volume % of tetragonal zirconia, preferably more than 95 volume %. If the zirconia medium or zirconia bearing ball contains more than 90 volume % of tetragonal zirconia, it is possible to improve mechanical strength such as wear resistance, durability, and impact resistance. The zirconia medium or zirconia bearing ball may also contain 100 volume % of tetragonal zirconia. If the content of tetragonal zirconia in the zirconia medium or zirconia bearing ball is less than 90 volume %, a large amount of monoclinic zirconia is contained. Fine cracks occur around the monoclinic zirconia contained in the zirconia medium or zirconia bearing ball, and the wear resistance, durability, and impact resistance are reduced. The content of monoclinic zirconia in the zirconia medium or zirconia bearing ball is allowed to be up to 5 volume %, preferably less than 5 volume %. In addition, if the zirconia media or zirconia bearing balls contain a large amount of cubic zirconia, the effect of stress-induced phase transformation is reduced, the toughness is reduced, and micro cracks are easily generated when used in a bead mill under high load. The content of cubic zirconia in the zirconia media or zirconia bearing balls is allowed to be up to 5% by volume, preferably 5% by volume or less.

[0073] The presence and content of monoclinic zirconia (M), the content of tetragonal zirconia (T), and the presence and content of cubic zirconia (C) in the zirconia crystal phase of the sintered body can be determined by X-ray diffraction.

[0074] The medium is arranged in a curable embedding resin in such a manner that the medium has an area of ​​a circle with a diameter of 10 mm or more, and the curable embedding resin is cured. The medium is ground to about one third of the diameter of the cross section of the medium embedded in the cured curable embedding resin. The ground surface is ground with diamond abrasive grains of 4 to 8 μm, and then with diamond abrasive grains of 3 μm or less to a depth of 5 μm or more, and finally polished with diamond abrasive grains of 1 μm or less, and mirror polished in such a manner that the surface roughness Rz according to JIS B0601:2001 reaches less than 0.050 μm (surface roughness Rz < 0.05 μm), and measured by X-ray diffraction method in the range of diffraction angles of 27 degrees to 34 degrees. Based on the results obtained by the measurement, the content (volume %) of monoclinic zirconium oxide (M) can be obtained by the following formula (1). In the present specification, the curable embedding resin can be, for example, a polyester resin, an acrylic resin or an epoxy resin.

[0075] [Formula 1]

[0076]

[0077] The presence or absence of cubic zirconia (C) and its content (volume %) can be measured by X-ray diffraction within a diffraction angle range of 70 to 77 degrees, similar to the content of monoclinic zirconia (M), and can be determined from the results obtained by the following formula (2).

[0078] Furthermore, based on the above results, the content of tetragonal zirconium oxide (T) can be calculated from the following formula (3).

[0079] [Formula 2]

[0080]

[0081] The relative density (d) of the zirconia medium or zirconia bearing ball is preferably 95% or more, and more preferably 97% or more. If the relative density (d) of the zirconia medium or zirconia bearing ball is 95% or more, the relative density of the zirconia medium or zirconia bearing ball becomes higher. The relative density of the zirconia medium or zirconia bearing ball may be 100% or 99.9% or less. The zirconia medium or zirconia bearing ball with a high relative density has fewer pores (holes) contained in the sintered body, which can suppress cracking and defects. If the relative density (d) of the zirconia medium or zirconia bearing ball is lower than 95%, the interior of the sintered body contains a large number of pores (holes). The zirconia medium containing a large number of pores becomes a cause of cracking and defects in a bead mill subjected to high loads, and the wear resistance and durability are reduced. The zirconia bearing ball containing a large number of pores has reduced wear resistance and durability. The relative density of the zirconia medium or zirconia bearing ball can be obtained by the following formula (4). The apparent density is measured by the gas replacement method specified in JIS R1620. The theoretical density can be based on the theoretical density of ZrO2 in which Y2O3 is dissolved (6.1 g / cm 3 ) and the theoretical density of Al2O3 (3.98 g / m 3 ), calculated based on the composition ratio of ZrO2 and Al2O3 in which Y2O3 is solid dissolved in the sintered body.

[0082] [Formula 3]

[0083] Relative density (%) = apparent density / theoretical density × 100 (4)

[0084] Average grain diameter

[0085] The average grain diameter (e) of the zirconia medium or zirconia bearing ball is within the range of 0.25 μm to 0.50 μm. The average grain diameter (e) of the zirconia medium or zirconia bearing ball may also be within the range of 0.26 μm to 0.48 μm, or within the range of 0.3 μm to 0.45 μm. If the average grain diameter (e) of the zirconia medium or zirconia bearing ball is less than 0.25 μm, the toughness is reduced, and chipping and cracking are likely to occur in the mill under high load, making it difficult to ensure the high purity of the processed powder. If the average grain diameter (e) of the zirconia medium or zirconia bearing ball is higher than 0.5 μm, the wear resistance and durability are reduced. The wear resistance of the zirconia medium or zirconia bearing ball is affected by the fine structure of the crystals near the surface of the sintered body constituting the zirconia medium or zirconia bearing ball. Therefore, the average grain size of the zirconia medium or zirconia bearing ball is preferably measured within 10% of the medium diameter in the direction from the surface toward the center of the medium. The average grain size of the zirconia medium or zirconia bearing ball can be measured as follows.

[0086] The sintered body constituting the medium is embedded in a curable embedding resin, and the curable embedding resin is cured. The surface of the sintered body embedded in the cured curable embedding resin is ground toward the center in a manner less than 10% of the medium diameter, and the ground surface is mirror-polished in the same manner as the measurement surface for crystal phase measurement to achieve a surface roughness Rz < 0.05 μm in accordance with JIS B0601: 2001. After thermal etching or chemical etching, the surface is observed using a scanning electron microscope (SEM) at a magnification that allows more than 100 grains to be observed in one field of view, and the average grain diameter is obtained by the intercept method. Specifically, a straight line of length L is drawn on the surface where the target grain is visible, and the number of grains passed by the straight line is obtained. The grain whose top end is inside the straight line is counted as 1 / 2. The average grain diameter can be obtained according to the following formula (5). It is preferred to draw 2 to 5 straight lines of length L to obtain the average grain diameter.

[0087] [Formula 4]

[0088] Average grain diameter (μm) = 1.5 × L / n (5)

[0089] [In the formula, L: represents the measurement length (μm) n: represents the number of grains per measurement length.]

[0090] Zirconia media or zirconia bearing balls, (f) the minimum value of the crushing load measured at a crosshead speed of 0.5 mm / min satisfies Pmin (N) > 600 × D 2.0(D is the average value of the medium diameter). If the minimum crushing load value Pmin is not greater than the product of the average value of the medium diameter D to the power of 2.0 times 600 (Pmin(N)>600×D 2.0 ), it becomes a factor that easily causes cracks and defects in the mill under high load. The minimum value of the crushing load value Pmin is a value less than the product of the average medium diameter D to the power of 2.0 multiplied by 600 (Pmin(N)≤600×D 2.0 ), it means that low-strength media with low crushing load values ​​are mixed. If low-strength media with low crushing load values ​​are mixed, the probability of cracking and defecting of the media with low crushing load values ​​due to impact in the mill under high load is high. If the zirconia media is cracked or defective, it is difficult to ensure the high purity of the processed powder. The maximum diameter measured based on the image of one medium observed using a scanning electron microscope is taken as the medium diameter, and the average value D of the medium diameter is the average value of the medium diameters of 200 media.

[0091] The crushing load value refers to the load value when a medium is sandwiched between two diamond sintered bodies or boron nitride (BN) sintered bodies using a material testing machine and a load is applied to the medium at a crosshead speed of 0.5 mm / min (the speed at which the distance between the plates is shortened) until it breaks. The crushing load values ​​of 50 media are measured, and the lowest crushing load value is taken as the minimum value Pmin (N).

[0092] The Weibull coefficient of the (g) crushing load value of the zirconia medium or zirconia bearing ball is 10 or more, preferably 12 or more. If the Weibull coefficient of the (g) crushing load value of the zirconia medium or zirconia bearing ball is 10 or more, the deviation of the strength is small, and the wear resistance and durability can be improved. If the Weibull coefficient of the crushing load value of the zirconia medium or zirconia bearing ball is less than 10, the deviation of the strength becomes large, and the medium with low strength in the mill under high load will crack and be damaged, and the wear resistance and durability will be reduced. The Weibull coefficient of the crushing load value can also be 25 or less.

[0093] In this specification, the Weibull coefficient is the Weibull coefficient when the crushing load values ​​or bending strengths of 50 media are plotted on a Weibull diagram. The Weibull coefficient can be calculated as follows. For the crushing load value or bending strength σ of each level i (i=1~n), the cumulative failure probability is calculated according to the following formula (6) using the average rank method. In the following formula (6), when calculating the Weibull coefficient of the bending strength, the crushing load value is replaced by the bending strength. According to the level i of the crushing load value or bending strength, a group of σi and Fi is established, and the Y-axis lnln(1-F) is plotted. -1 , X-axis lnσ. In this Weibull plot (lnln(1-F) -1The least square method was applied to the data points of -lnσ to obtain the linear regression line, and its slope was calculated as the Weibull coefficient m.

[0094] [Formula 5]

[0095] Fi=i / (n+1) (6)

[0096] [Where n: total number of tests of crushing load value, i: levels arranged from small to large, Fi: cumulative failure probability of level i]

[0097] The zirconia medium or zirconia bearing ball preferably has a maximum diameter of the medium that can be confirmed in the SEM image confirmed by using a scanning electron microscope (h) as the medium diameter, and the coefficient of variation of the medium diameter derived from the average value of the medium diameter of 200 media and the standard deviation is less than 6%. The coefficient of variation of the medium diameter of the zirconia medium or zirconia bearing ball is preferably 5.9% or less, and may be 5.8% or less, and more preferably 4% or less. The coefficient of variation of the medium diameter is preferably 0%, and may be 0.1% or more. If the coefficient of variation of the medium diameter (h) of the zirconia medium or zirconia bearing ball is less than 6%, the size deviation of the medium is small, the crushing characteristics of the medium in the bead mill are uniform, and the processed powder can be uniformly crushed and dispersed. If the coefficient of variation of the medium diameter (h) of the zirconia medium or zirconia bearing ball is 6% or more, large-sized media and small-sized media are mixed, and the movement of media of different sizes is different in the bead mill, resulting in deviations in the crushing and dispersion characteristics of the media, resulting in deviations in the particle size distribution of the processed powder, and poor reproducibility in the crushing and dispersion process. In addition, since the crushing load value of the medium is small, it becomes a cause of cracking and defect of the medium. In addition, since the medium with small size is worn first, the uneven wear is promoted due to the size of the medium, resulting in reduced wear resistance and durability, so it is not preferred. The coefficient of variation of the medium diameter can be obtained according to the following formula (7).

[0098] [Formula 6]

[0099] Coefficient of variation of medium diameter (%) = standard deviation of medium diameter / mean value of medium diameter × 100 (7)

[0100] The zirconia medium or zirconia bearing ball satisfies the requirements (a) to (h) above, and preferably also satisfies the requirement (k) above. The zirconia medium or zirconia bearing ball satisfies the requirements (a) to (h) above, and preferably also satisfies at least one of the following requirements (j), (k), (n) and (o). The zirconia medium or zirconia bearing ball satisfies the requirements (a) to (h) and (k) above, and preferably also satisfies at least one of the following requirements (j), (n) and (o).

[0101] A zirconia medium or a zirconia bearing ball, preferably (j) according to ISO 14577, one medium is embedded in a curable embedding resin, the curable embedding resin is cured, and the medium is ground to 40% to 50% of its diameter. The ground surface is mirror-polished in the same manner as the surface measured for crystal phase measurement in accordance with JIS B0601:2001 so that the surface roughness reaches Rz < 0.05 μm, and then the micro-indentation hardness of 10 places of the ground medium cross section is measured at equal intervals using an ultra-micro-indentation hardness tester, and the coefficient of variation of the micro-indentation hardness derived from the average value and standard deviation of the micro-indentation hardness measured for the 10 media is 5% or less.

[0102] The zirconia medium or zirconia bearing ball preferably has a (k) SiO2 content in the range of 0.2 mass % to 1.0 mass %.

[0103] The zirconia medium or zirconia bearing ball preferably has a crushing load ratio A (Pmin(N) / Pave(N)) of the minimum crushing load value Pmin(N) measured at a crosshead speed of 0.5 mm / min relative to the average crushing load value Pave(N) of 0.8 or more.

[0104] The zirconia medium or zirconia bearing ball preferably has a crushing load ratio B (Pave0.1(N) / Pave(N)) of 0.95 or more, wherein (o) the average crushing load value Pave0.1(N) measured at a crosshead speed of 0.1 mm / min relative to the average crushing load value Pave(N) measured at a crosshead speed of 0.5 mm / min.

[0105] A zirconia medium or a zirconia bearing ball, (j) according to ISO 14577, one medium is embedded in a curable embedding resin, the curable embedding resin is cured, and the medium is ground to 40% to 50% of its diameter, and the cross section is mirror-polished according to the above method in a manner to achieve a surface roughness of Rz < 0.05 μm in accordance with JIS B0601:2001, and then the micro-indentation hardness of the ground medium cross section is measured at equal intervals at 10 locations using an ultra-micro-indentation hardness tester, and the coefficient of variation of the micro-indentation hardness can be derived from the average value and standard deviation of the micro-indentation hardness measured in the 10 media. The zirconia medium or the zirconia bearing ball preferably has a coefficient of variation of the micro-indentation hardness of (j) 5% or less. The coefficient of variation of the micro-indentation hardness of the zirconia medium or zirconia bearing ball is preferably 4.8% or less, or 4.5% or less, or 4.0% or less, or 3.5% or less, preferably 0%, but it may be 0.1% or more, 0.2% or more, or 0.5% or more. If the density of the molded body formed by granulating the molding powder used to form the zirconia medium or zirconia bearing ball is uneven, a difference in the amount of shrinkage will occur in one sintered body in the subsequent sintering process, so the inhomogeneity of the structure becomes larger. The sintered body with large inhomogeneity of the structure also has uneven ultra-micro indentation hardness. If the structure is uneven, the residual stress also increases, so the resistance to impact is reduced, which becomes a cause of cracking and defect when used in a bead mill under high load. If the coefficient of variation of the micro-indentation hardness of the zirconia medium or zirconia bearing ball is 5% or less, the structure in the sintered body constituting the medium is uniform, and cracking and defect can be suppressed. If the coefficient of variation of the micro-indentation hardness of zirconia media or zirconia bearing balls is higher than 5%, the structure of the sintered body constituting the media is uneven. Zirconia media with an uneven sintered structure are prone to cracking and defects due to collisions between media in a bead mill under high load, and wear resistance is reduced. Zirconia bearing balls with an uneven sintered structure, for example, are prone to cracking and defects if subjected to high loads in bearings, and wear resistance and durability are reduced. Even if the distribution of the media diameter is a sharpened spherical shape, if there is a deviation in the micro-indentation hardness inside the media, it will also lead to a reduction in impact resistance, wear resistance and durability. The micro-indentation hardness of zirconia media or zirconia bearing balls can be measured with a test load of 50mN, a load application speed of 5mN / second, a test load holding time of 1 second, and an unloading speed of 5mN / second. The coefficient of variation of the micro-indentation hardness of the media measured with an ultra-micro indentation hardness tester can be obtained by the following formula (8).

[0106] [Formula 7]

[0107] Coefficient of variation of micro-indentation hardness (%) =

[0108] Standard deviation of micro-indentation hardness / average value of micro-indentation hardness × 100 (8)

[0109] The zirconia medium or zirconia bearing ball preferably has a medium diameter (m) of 0.5 mm or less. The zirconia medium or zirconia bearing ball more preferably has a medium diameter of 0.2 mm or less. The medium diameter may also be greater than 0.01 mm, or greater than 0.015 mm. The method for measuring the medium diameter is the same as the method for measuring by confirming an image using a scanning electron microscope. If the medium diameter of the zirconia medium is less than 0.5 mm, it can be used as a medium for crushing and dispersing fine powders. The crushing and dispersing of fine powders also requires a tiny medium. In order to crush and disperse fine powders of 1 nm to 100 nm in size, which are called nanopowders, it is preferred to use a medium with a diameter of less than 0.5 mm, and more preferably a tiny medium with a diameter of less than 0.2 mm. If the size of the medium is too large relative to the size of the processed powder, the processed powder cannot be crushed and dispersed into a microscopic size. In addition, if the size of the medium is too large relative to the size of the processed powder, the mass of the medium also increases, which will damage the surface of the processed powder, activating the surface of the powder and making it easy to re-agglomerate. If the (m) medium diameter of the zirconia bearing ball is small, it can also be used for small bearings.

[0110] The zirconia medium or zirconia bearing ball preferably has a crushing load ratio A (Pmin(N) / Pave(N)) of the minimum crushing load value Pmin(N) measured at a crosshead speed of 0.5 mm / min relative to the average crushing load value Pave(N) of 0.8 or more, or 0.81 or more. The crushing load ratio A is 1 or less.

[0111] The crushing load value is affected by the grain boundary strength of the sintered body constituting the medium, and the size and number of internal defects. Therefore, the medium is not only the coefficient of variation that indicates the uniformity of the medium diameter distribution, but also can be said to have uniform strength if the crushing load ratio A is 0.8 or more. In zirconia media or zirconia bearing balls, if the crushing load ratio A is 0.8 or more, it can be said that they have uniform strength that maintains impact resistance, wear resistance and durability.

[0112] The average value of the crushing load value is measured in the same way as the measurement of the minimum crushing load value Pmin(N), and the average value of the crushing load values ​​of 50 media is taken as Pave(N). The crushing load ratio A can be obtained by the following formula (9).

[0113] [Formula 8]

[0114] Crushing load ratio A: Pmin(N) / Pave(N)≥0.8 (9)

[0115] [Wherein, Pmin(N): minimum value of crushing load value Pave(N): average value of crushing load value]

[0116] The zirconia medium or zirconia bearing ball preferably has a crushing load ratio B (Pave0.1(N) / Pave(N)) of the average crushing load value Pave0.1(N) measured at a crosshead speed of 0.1 mm / min relative to the average crushing load value Pave(N) measured at a crosshead speed of 0.5 mm / min of 0.950 or more, more preferably 0.955 or more, further preferably 0.960 or more, and further preferably 0.965 or more. The closer the average crushing load value Pave and the average crushing load value Pave0.1 are to the same value (Pave0.1(N) / Pave(N)=1), the fewer internal defects the zirconia medium or zirconia bearing ball has.

[0117] In the case of slow loading speed, stress is easily concentrated on low-strength structures such as unevenness and defects in the medium, and the crushing load value tends to decrease. If the crushing load ratio B of the average value of the crushing load value Pave0.1 (N) measured at a crosshead speed of 0.1 mm / min to the average value of the crushing load value Pave (N) measured at a crosshead speed of 0.5 mm / min is 0.95 or more, it means that the medium has more uniform strength, indicating excellent impact resistance, wear resistance and durability.

[0118] The average value of the crushing load values ​​Pave0.1 (N) measured at a crosshead speed of 0.1 mm / min is the average value of the crushing load values ​​of 50 media as Pave0.1 (N). The crushing load ratio B can be calculated by the following formula (10).

[0119] [Formula 9]

[0120] Crushing load ratio B: Pave0.1(N) / Pave(N)≥0.95 (10)

[0121] [Wherein, Pave (N): the average value of the crushing load value measured at a crosshead speed of 0.5 mm / min; Pave0.1 (N): the average value of the crushing load value measured at a crosshead speed of 0.1 mm / min]

[0122] Zirconia bearing ball, (x) fracture toughness 5.0MPa·m 1 / 2 Above, preferably 5.2 MPa·m 1 / 2 More preferably, 5.4 MPa·m 1 / 2 More preferably, 5.5 MPa·m 1 / 2Above, particularly preferably 5.6 MPa·m 1 / 2 Above, it can also be 8.0MPa·m 1 / 2 Below, it can also be 7.0MPa·m 1 / 2 Below, it can also be 6.5MPa·m 1 / 2 Below. Zirconia bearing ball, (x) fracture toughness can also be 7.0MPa·m 1 / 2 Below, it can also be 6.8MPa·m 1 / 2 If the (x) fracture toughness of the zirconia bearing ball is 5.0 MPa·m 1 / 2 The above can satisfy the fracture toughness of grade III of silicon nitride (Si3N4) bearing balls specified in F2094 of ASTM International (formerly American Society for Testing and Materials), and can be used as bearing balls that meet the standard values ​​of ASTM International. In addition, the fracture toughness of grade 3 of silicon nitride (Si3N4) materials for rolling bearing balls specified in JIS R1669 can be satisfied, and can be used as bearing balls that meet the standard values ​​of JIS R1669. The fracture toughness of zirconia bearing balls can be measured according to JIS R1669.

[0123] The fracture toughness of zirconia bearing balls can be measured using the SENB method, using a test molded body formed by pressure molding the molding powder used to form the zirconia bearing balls, sintered under the same conditions as the medium, and cut using a #140 diamond wheel into a 3mm×4mm×45mm (vertical×lateral×thick) test piece. The test piece can be evaluated by 3-point bending with a span of 30mm and a crosshead speed of 0.5mm / min. A notch is machined in the center of the tensile surface of the test piece with a radius of curvature of 10μm and a depth of 1.5mm at the front end of the notch and the measurement is performed. Fracture toughness K IC It can be obtained from the following equations (11) and (12).

[0124] [Formula 10]

[0125]

[0126] Zirconia bearing balls, (y) have a flexural strength higher than 1100 MPa, and a Weibull modulus of flexural strength higher than 7. The flexural strength may be higher than 1110 MPa, higher than 1120 MPa, higher than 1150 MPa, lower than 1600 MPa, lower than 1500 MPa, or lower than 1450 MPa. The Weibull modulus of flexural strength may be higher than 7.1, higher than 7.5, higher than 8, lower than 30, or lower than 25. Zirconia bearing balls, (y) if the flexural strength is higher than 1100 MPa and the Weibull modulus of flexural strength is higher than 7, can meet the flexural strength of material grade III of silicon nitride (Si3N4) bearing balls specified in F2094 of ASTM International, can meet the Weibull modulus of flexural strength, and can be used as bearing balls that meet the standard values ​​of ASTM International. In addition, the flexural strength and Weibull coefficient of flexural strength of grade 3 silicon nitride (Si3N4) material for rolling bearing balls specified in JIS R1669 can be used as bearing balls that meet the standard values ​​of JIS R1669. The flexural strength of zirconia bearing balls can be measured in accordance with JIS R1669 by measuring the flexural strength of 10 samples at three points with a span of 30 mm and a crosshead speed of 0.5 mm / min, and the arithmetic mean of the measured values ​​of the 10 samples is taken as the (y) flexural strength. In addition, the Weibull coefficient of flexural strength can be obtained by replacing the crushing load value with the flexural strength in the above formula (6).

[0127] Figure 4 This is a schematic stereogram showing an example of a bearing using a zirconia bearing ball. The bearing 1 has a bearing ball 4 held in a retainer (not shown) between an inner ring 2 and an outer ring 3. The bearing can be used in wind turbines, airplanes, cars, bicycles, trams, refrigerators, air conditioners, vacuum cleaners, copiers, washing machines, massage chairs, cameras, electric screwdrivers, personal computers, automatic ticket gates, sidewalks, elevators, conveyors, etc. In addition, it can also be used in medical devices such as computed tomography (CT), magnetic resonance imaging (MRI), and dental handpieces. In cars, bearings are used in wheels, suspension systems, steering systems, etc. In bicycles, bearings are used in transmissions, wheels, etc. In automatic ticket gates, bearings are used in roller parts that convey tickets, etc. In dental handpieces, bearings are used in drills that rotate at high speeds, for example.

[0128] Method for manufacturing zirconium oxide medium or zirconium oxide bearing ball

[0129] The method for manufacturing the zirconium oxide medium or the zirconium oxide bearing ball of the present invention comprises:

[0130] (p) mixing a zirconium raw material and a yttrium raw material so that the Y2O3 / ZrO2 molar ratio is within the range of 2.5 / 97.5 or more and 3.2 / 96.8 or less, hydrolyzing the mixture, and pre-calcining the resulting hydrate of zirconium and yttrium at a temperature within the range of 600°C or more and 1200°C or less to obtain a synthetic powder,

[0131] (q) mixing the obtained synthetic powder with Al2O3 powder to obtain a mixed powder in such a manner that the content of Al2O3 is within the range of 0.1 mass % to 30.0 mass % with respect to the total amount,

[0132] (r) drying the mixed powder slurry obtained by wet pulverizing and / or dispersing the mixed powder to obtain a powder having a specific surface area of ​​5 m 2 / g or more and 10m 2 Within the range below / g,

[0133] (s) pulverizing and / or dispersing the mixed powder slurry by a wet method in such a manner that the average particle size having a cumulative frequency of 50% in the volume-based particle size distribution measured by a laser diffraction method in accordance with JIS Z8825 is within a range of 0.3 μm to 0.6 μm,

[0134] (t) preparing a molding powder obtained by drying and granulating powder in a slurry for measuring the average particle size of agglomerated powder obtained by mixing 1 part by mass of a powder obtained by drying the mixed powder slurry with 100 parts by mass of a molding solvent in such a manner that the average particle size of agglomerated powder having a cumulative frequency of 50% in a volume-based particle size distribution measured in accordance with JIS Z8825 is within a range of 1 μm or more and 5 μm or less,

[0135] (u) granulating the molding powder to obtain a molded body,

[0136] (v) The molded body is sintered at a temperature within a range of 1250° C. to 1600° C. to obtain a ZrO 2 —Y 2 O 3 -based zirconia sintered body.

[0137] (p) A zirconium raw material and a yttrium raw material are mixed so that the Y2O3 / ZrO2 molar ratio is within the range of 2.5 / 97.5 or more and 3.2 / 96.8 or less, and the mixture is hydrolyzed. The resulting hydrate of zirconium and yttrium is pre-calcined within the range of 600°C or more and 1200°C or less to obtain a synthetic powder. If the Y2O3 / ZrO2 molar ratio of the synthetic powder is within the range of 2.5 / 97.5 or more and 3.2 / 96.8 or less, a ZrO2-Y2O3 system zirconia sintered body containing less monoclinic zirconia and more than 95% by volume of tetragonal zirconia can be obtained. If the Y2O3 / ZrO2 molar ratio of the synthetic powder is within the aforementioned range, the tetragonal zirconia contained in the obtained sintered body is well stabilized, cracking and defect of the sintered body can be suppressed, and a sintered body with improved wear resistance and durability can be obtained.

[0138] The zirconium raw material and the yttrium raw material are mixed in such a manner that the Y2O3 / ZrO2 molar ratio is within the range of 2.5 / 97.5 or more and 3.2 / 96.8 or less, and water is added to form an aqueous solution. After the aqueous solution is hydrolyzed by heating and refluxing at a temperature of 100°C, the obtained zirconium and yttrium hydrates are dehydrated and dried, and pre-fired within the range of 600°C or more and 1200°C or less to obtain a synthetic powder. The pre-fired temperature may also be within the range of 800°C or more and 1000°C or less. If the pre-fired temperature is within the range of 600°C or more and 1200°C or less, the composition in the synthetic powder becomes uniform, and the composition is uniform during firing, and a sintered body with uniform strength is easily obtained. The pre-fired time is 30 minutes or more and within 2 hours, and may also be within 1 hour. The pre-fired is preferably carried out in an atmospheric atmosphere (oxygen is 20 volume %) and under standard atmospheric pressure (0.101MPa).

[0139] In order to prepare synthetic powder, a zirconium compound is used as a zirconium raw material. Zirconium oxychloride, zirconium acetate, zirconium nitrate, zirconium sulfate, etc. can be used as the zirconium compound. The zirconium compound preferably has a purity of 99.9% by mass or more. If the impurity amount of the zirconium compound used as the zirconium raw material is large, the impurity phase is easily generated at the grain boundary of the obtained sintered body. If a high load is applied to the sintered body, stress is concentrated on the impurity phase, which becomes the cause of cracking and defect of the zirconium oxide medium formed by the sintered body, so it is not preferred. In this specification, the purity of the zirconium compound can refer to the value recorded in the catalog of each compound.

[0140] Y2O3 solid-dissolved in ZrO2 uses yttrium compounds as yttrium raw materials. Yttrium compounds can use yttrium nitrate, yttrium oxide, etc. The yttrium compound preferably has a purity of 99.9% by mass or more. If the yttrium compound has a large amount of impurities, as mentioned above, it is easy to generate impurity phases at the grain boundaries of the obtained sintered body, so it is not preferred.

[0141] (q) Al2O3 powder is mixed with synthetic powder in such a manner that the content of Al2O3 is within a range of 0.1 mass % to 30.0 mass % relative to the total amount to obtain a mixed powder. If the mixed powder contains Al2O3 powder, the sinterability of a formed body made using a forming powder made from the mixed powder is improved. In addition, since Al2O3 segregates to the grain boundaries of ZrO2 and also exists as crystal particles of Al2O3, the grain boundaries of ZrO2 are strengthened, and a sintered body with improved mechanical properties such as impact resistance can be obtained.

[0142] The Al2O3 powder preferably has an aluminum oxide purity of 99.9% by mass or more, and an average particle size with a cumulative frequency of 50% in the volume-based particle size distribution measured by laser diffraction method in accordance with JISZ8825 is within the range of 0.1 μm to 0.3 μm. If the amount of impurities in the Al2O3 powder is large, as mentioned above, impurity phases are easily generated at the grain boundaries of the resulting sintered body. In addition, if the average particle size of the Al2O3 powder is within the range of 0.1 μm to 0.3 μm, an amount of Al2O3 powder that meets the requirement (q) is uniformly dispersed in the mixed powder containing the synthetic powder and the Al2O3 powder. In the resulting sintered body, Al2O3 segregates at the grain boundaries of ZrO2, and also exists as crystal particles of Al2O3, the grain boundaries of ZrO2 are strengthened, and a sintered body with improved mechanical properties such as impact resistance can be obtained. If the Al2O3 powder is larger than 0.3 μm, the size of the Al2O3 crystal particles is too large relative to the ZrO2 crystal particles, so the sintered body cannot be uniformly structured. In addition, if the Al2O3 powder is smaller than 0.1 μm, it is easy to aggregate and cannot be evenly dispersed.

[0143] In the mixed powder, it is preferred that (w) the SiO2 raw material is contained in a range of 0.2 mass % to 1.0 mass % relative to the total amount of SiO2, and it may be contained in a range of 0.3 mass % to 0.9 mass % or in a range of 0.5 mass % to 0.7 mass %. If (w) the SiO2 raw material is contained in the mixed powder in a range of 0.2 mass % to 1.0 mass % relative to the total amount, even when the medium is used in warm water at 40°C or above, it is possible to suppress the erosion of the grain boundaries of ZrO2 in the sintered body constituting the medium by water, thereby maintaining the wear resistance.

[0144] As the SiO 2 raw material, SiO 2 powder such as fumed silica, or silica sol such as ethyl silicate and colloidal silica can be used as a SiO 2 source.

[0145] The specific surface area of ​​the powder obtained by drying the mixed powder slurry obtained by wet pulverization and / or dispersion is 5 m 2 / g or more and 10m 2 / g or less, (s) the mixed powder slurry is crushed and / or dispersed in a manner such that the average particle size of the mixed powder slurry measured by the laser diffraction method is within the range of 0.3μm or more and 0.6μm or less. The obtained mixed powder slurry is dried and granulated in a manner such that the agglomerated powder particle size shown below is achieved to obtain a molding powder. The molding powder is used so that the specific surface area and the average particle shape are within the above ranges. When the molded body obtained by granulation molding is sintered, a sintered body with uniform strength and uniform sintering inside the molded body can be obtained. If the specific surface area of ​​the mixed powder is higher than 10m 2 / g, or the average particle size of the mixed powder is less than 0.3μm. When the granulated body is sintered, the sinterability is too large, the interior is sintered unevenly, and a sintered body with low strength parts is formed. The sintered body with low strength parts is prone to stress concentration at weak points, resulting in cracks and defects, and reduced wear resistance and durability. If the specific surface area of ​​the mixed powder is less than 5m 2 / g, or if the average particle size of the mixed powder exceeds 0.6 μm, the sinterability is reduced, defects are likely to remain, the strength of the sintered body is reduced, cracks and defects occur, and the wear resistance and durability are reduced.

[0146] The mixed powder can be made to have a specific surface area of ​​5.2 m 2 / g or above and 9.5m 2 / g or less by wet grinding and / or dispersion. In addition, the mixed powder can be pulverized and / or dispersed by wet grinding in a manner such that the average particle size measured by laser diffraction method is within the range of 0.32 μm or more and 0.59 μm or less, or can be pulverized and / or dispersed by wet grinding in a manner such that the average particle size is within the range of 0.35 μm or more and 0.50 μm or less.

[0147] (t) A molding powder is prepared by drying and granulating the powder agglomerated in a slurry for measuring the average particle size of the agglomerated powder obtained by mixing 1 part by mass of the powder obtained by drying the mixed powder slurry with 100 parts by mass of the molding solvent so that the average particle size of the agglomerated powder is within the range of 1 μm to 5 μm at a cumulative frequency of 50% in the volume-based particle size distribution measured in accordance with JIS Z8825. The average particle size of the agglomerated powder may be within the range of 1.2 μm to 4.9 μm or within the range of 1.5 μm to 4.0 μm.

[0148] The present inventors have newly found that not only the specific surface area and average particle size of the mixed powder but also the powder state of the mixed powder slurry after drying has a significant influence on the formability and sinterability.

[0149] The state of the powder of the mixed powder slurry after drying and agglomeration greatly affects the wettability with the molding solvent when the molding powder is granulated and formed. If the agglomerated powder average particle size of the mixed powder after drying and agglomeration is adjusted in a range of 1 μm or more and 5 μm or less, the conditions of wet pulverization, dispersion and addition, drying and granulation of a suitable surfactant are adjusted to prepare the molding powder, the wettability of the molding powder during granulation is suitable, and a molding with uniform organization and molding density can be formed during granulation. The obtained molding can be uniformly sintered, and the density of the obtained sintered body can be uniform. The surfactant added when the mixed powder is wet pulverized and dispersed can use polycarboxylic acid sodium salt, polycarboxylic acid ammonium salt, etc. The surfactant can be used in the range of 0.1% by mass and 5% by mass relative to 100% by mass of the mixed powder slurry as needed. The obtained molding is uniformly sintered, so that the shrinkage difference caused by sintering can be eliminated.

[0150] In this specification, the agglomerated powder refers to a powder in which secondary particles are more weakly agglomerated. The agglomerated powder maintains the agglomerated state even in the slurry.

[0151] The agglomerated powder can be measured by mixing 1 part by mass of the agglomerated powder with 100 parts by mass of the molding solvent in a test tube. Specifically, add 0.1 g of agglomerated powder and 10 g of molding solvent to a test tube, shake for 3 seconds, mix and shake to the maximum extent, pipette, add the slurry pipetted into the analysis container, irradiate the slurry in the analysis container with laser, and measure the average particle size of the agglomerated powder of the agglomerated powder in the slurry. The molding solvent needs to use the same solvent as the molding solvent used when the molding powder described later is granulated and molded to form a molded body. If the average particle size of the agglomerated powder of the agglomerated powder is within the range of 1.2 μm or more and 4.9 μm or less, it can be used as a molding powder.

[0152] The method for manufacturing a zirconium oxide medium or a zirconium oxide bearing ball comprises (u) granulating the obtained molding powder to obtain a molded body. A molding solvent is added to the molding powder to perform granulation molding to obtain a molded body. The molding solvent used during molding may include water, alcohols, paraffin hydrocarbons and mixtures thereof. Water may include, for example, ion exchange water. As alcohols, for example, alcohols having a linear or branched alkyl group with a carbon number of 1 to 4 may be included. The molded body is preferably formed by granulation molding in a manner such that the medium diameter is less than 0.5 mm after sintering.

[0153] A method for manufacturing a zirconia medium or a zirconia bearing ball, comprising (v) sintering the obtained molded body in the range of 1250°C to 1600°C to obtain a ZrO2-Y2O3 zirconia sintered body. The sintering temperature is more preferably in the range of 1300°C to 1550°C. If the sintering temperature is in the range of 1250°C to 1600°C, uniform sintering can be achieved, and a sintered body with high strength can be obtained. The medium formed by the sintered body obtained by the method for manufacturing a zirconia medium can meet the requirements of (a) to (h). If the sintering temperature is lower than 1250°C, the sintering is insufficient, pores as defects remain, the strength is reduced, and the wear resistance of the obtained sintered body is reduced. If the sintering temperature is higher than 1600°C, the grain diameter may be too large, and the content of cubic zirconia increases, the toughness is reduced, and the wear resistance is reduced. The shaped body is preferably fired using a gas furnace or the like in an air atmosphere (oxygen 20% by volume) and a standard atmospheric pressure (0.101 MPa).

[0154] The obtained sintered body is preferably ground using a barrel grinder until the surface roughness Rz (maximum height of the roughness curve of the surface roughness) according to JIS B0601:2001 reaches 0.3 μm or less (Rz≤0.3 μm). By grinding the surface of the obtained sintered body with a barrel grinder, the surface irregularities disappear, and the wear resistance can be improved. The obtained sintered body can be used as a medium.

[0155] Example

[0156] Hereinafter, the present invention will be described in further detail based on Examples and Comparative Examples. The present invention is not limited to these Examples.

[0157] Examples 1 to 8, Comparative Examples 1 to 11

[0158] Zirconium oxychloride with a purity of 99.9% by mass (catalog value) and yttrium nitrate with a purity of 99.9% by mass (catalog value) are added to water and mixed in such a manner that the Y2O3 / ZrO2 molar ratio in terms of oxides reaches the value shown in Table 2 to obtain an aqueous solution. Then, the aqueous solution is hydrolyzed under heating reflux at 100°C to obtain a precipitate of yttrium-containing zirconium hydrate. The yttrium-containing zirconium hydrate is dehydrated and dried at 100°C for 24 hours to obtain yttrium-containing zirconium hydrate. After reaching the pre-calcination temperature shown in Table 1, the yttrium-containing zirconium hydrate is pre-calcined in a gas furnace in an atmospheric atmosphere and standard atmospheric pressure for 1 hour to obtain a synthetic powder (the treatment of (p)).

[0159] The resulting synthetic powder contains Al2O3 powder having a purity of 99.9 mass % (catalog value) and, as required, fumed silica or silica sol having a purity of 99.9 mass % (catalog value) as a SiO2 source, which are wet dispersed in water in a manner to achieve a content shown in Table 2 relative to the total amount, thereby obtaining a mixed powder (the treatments of (q) and (w) described above).

[0160] The mixed powder obtained by wet grinding and / or dispersion using water as a medium has a specific surface area measured by the BET method described below as shown in Table 1, and an average particle size measured by the laser diffraction method described below as shown in Table 1, thereby obtaining a mixed powder slurry. (Processing of (r) and (s))

[0161] The mixed powder slurry is dried, and the agglomerated powder in the slurry for measuring the average particle size of the agglomerated powder obtained by mixing 1 part by mass of the dried powder with 100 parts by mass of the molding solvent is dried and sized in such a manner that the average particle size of the agglomerated powder measured by the laser diffraction method described later is the value shown in Table 1, thereby obtaining a molding powder. The sizing is performed by classification with a sieve (the treatment of (t)).

[0162] Water was added as a molding solvent to each molding powder of Examples and Comparative Examples, and the mixture was granulated to form a molded body, thereby obtaining each molded body of Examples and Comparative Examples (treatment (u)).

[0163] After reaching the firing temperature shown in Table 1, each of the molded bodies of the examples and comparative examples was fired for 1 hour in a gas furnace at an atmospheric atmosphere and standard atmospheric pressure to obtain sintered bodies of the examples and comparative examples. The surface of the sintered body was ground using a barrel grinding device until the surface roughness Rz (the maximum height of the roughness curve of the surface roughness) reached 0.3 μm or less (Rz ≤ 0.3 μm) according to JIS B0601:2001, and the ground sintered body was used as a medium for pulverization and dispersion (the treatment of (v)). The roughness curve of the surface roughness was measured using a laser microscope (manufactured by KEYENCE Co., Ltd.).

[0164] The specific surface area and average particle size of each mixed powder of the examples and comparative examples were measured as follows. In addition, the average particle size of the agglomerated powder of the molding powder was obtained as follows. These results are recorded in Table 1 together with the calcination temperature and firing temperature of each molded body.

[0165] Specific surface area of ​​mixed powder slurry

[0166] The specific surface area of ​​the mixed powder slurry was measured by the BET method using a specific surface area measuring device (Tristar II, manufactured by Shimadzu Corporation).

[0167] Average particle size of mixed powder slurry

[0168] The average particle size of the mixed powder is measured by laser diffraction method according to JIS Z8825 using a particle size distribution measuring device (MT3000, manufactured by MicrotracBEL Co., Ltd.) to obtain the average particle size of the mixed powder at a cumulative frequency of 50% in a volume-based particle size distribution.

[0169] Average particle size of agglomerated powder for molding

[0170] 1 part by mass of powder obtained by drying a mixed powder slurry is mixed with 100 parts by mass of ion exchange water as a molding solvent to obtain a slurry for measuring the average particle size of the agglomerated powder. For the agglomerated powder in this slurry, the average particle size of the agglomerated powder at a cumulative frequency of 50% in the volume-based particle size distribution is measured by laser diffraction method in accordance with JIS Z8825 using a particle size distribution measuring device (MT3000, manufactured by MicrotracBEL Co., Ltd.).

[0171] The following evaluations were performed on each medium of Examples and Comparative Examples, and the results are shown in Tables 2 to 5. In each evaluation, for conditions not shown below, the conditions of each evaluation described above can be referred to.

[0172] Average value of medium diameter, coefficient of variation of medium diameter

[0173] For each medium of the embodiment and the comparative example, 200 images of the medium were taken using a scanning electron microscope (SEM) (SU3500, manufactured by Hitachi High-Tech Co., Ltd.). For the taken images, the maximum diameter of the medium was used as the medium diameter using image analysis software (Image-Pro Plus, manufactured by Nippon Roper Co., Ltd.) to generate a particle size distribution of the medium diameters of the 200 media. The average value and standard deviation of the medium diameters of the 200 media were obtained, and the coefficient of variation of the medium diameter was obtained based on the above formula (7).

[0174] Content ratio of the crystal phase of the medium (volume %)

[0175] For each medium of the embodiment and the comparative example, the medium formed by the sintered body is arranged in a curable embedding resin in such a manner that the area of ​​the medium is greater than or equal to a circle having a diameter of 10 mm or greater. The curable embedding resin (epoxy resin) is cured and ground until the diameter of the cross section of the medium formed by the sintered body embedded in the curable embedding resin is about one-third, and mirror polishing is performed by the above-mentioned method so that the surface roughness of the ground surface reaches the surface roughness Rz < 0.05 μm in accordance with JIS B0601:2001. The X-ray diffraction method is used to measure the diffraction angle in the range of 27 to 34 degrees and in the range of 70 to 77 degrees. Based on the obtained results, the content (volume %) of monoclinic zirconium oxide (M), the content (volume %) of tetragonal zirconium oxide (T), and the content (volume %) of cubic zirconium oxide (C) are calculated based on the above-mentioned formulas (1) to (3).

[0176] The X-ray diffraction conditions were as follows: X-ray source: CuKα, output power: 40 kV / 40 mA, incident side divergence slit: 1 / 2°, incident side Soller slit: 4.1°, receiving side divergence slit: 5.2 mm, receiving side Soller slit: OPEN, scanning speed: 0.5° / min, scanning axis 2θ / θ.

[0177] Relative density

[0178] For each medium of the embodiment and comparative example, the apparent density was measured based on the gas replacement specified in JIS R1620. In addition, the theoretical density of each medium was calculated based on the Y2O3 / ZrO2 molar ratio and the Al2O3 content, and the relative density (%) was obtained based on the above formula (4). The theoretical density is based on the theoretical density of ZrO2 in which Y2O3 is dissolved (6.1 g / cm 3 ) and the theoretical density of Al2O3 (3.98 g / m 3 ), calculated based on the composition ratio of ZrO2 and Al2O3 in which Y2O3 is solid-dissolved in the sintered body.

[0179] Average grain diameter

[0180] For each medium of the embodiment and the comparative example, the medium is embedded in a curable embedding resin (epoxy resin), and the curable embedding resin is cured. From the surface of the medium embedded in the curable embedding resin toward the center, it is ground in a manner of less than 100 μm, and the ground surface is polished to a mirror surface by the aforementioned method, and then thermal etching or chemical etching is performed. Thereafter, a scanning electron microscope (SEM) (SU3500, manufactured by Hitachi High-Tech Co., Ltd.) is used to observe at a magnification that more than 100 grains can be observed in one field of view, and the average grain diameter is calculated by the intercept method. Specifically, 10 straight lines of length L are drawn on the surface where the target grains are visible, and the number of grains passed by the straight line is calculated. The grains inside the straight line at the top end are counted as 1 / 2, and the average grain diameter is calculated based on the above formula (5).

[0181] Minimum value of crushing load Pmin(N), 600×D 2.0

[0182] For each medium of the embodiment and comparative example, a universal material testing machine (5965, manufactured by INSTRON) was used. The pressure plate used a boron nitride (BN) sintered body. One medium was sandwiched between two pressure plates. The load was applied at a crosshead speed of 0.5 mm / min. The pressure at the time of destruction was measured as the crushing load value. The crushing load values ​​of 50 media were taken as the average value Pave (N), and the minimum value of the crushing load values ​​of 50 media was taken as Pmin (N). In addition, the average value of the diameter of the medium (D) was used to obtain the relationship between 600 and D 2.0 The product of 2.0 ).

[0183] Weibull coefficient for crushing load value

[0184] For each medium of the embodiment and the comparative example, similarly to the measurement of the lowest value of the crushing load value, the crushing load values ​​of 50 media are plotted on a Weibull plot, and for the crushing load value σ of each level i (i=1-n), the average rank method is used to obtain the cumulative failure probability by the above formula (6). According to the level i of the crushing load value, a group of σi and Fi is established, and the Y-axis lnln(1-F) is plotted. ―1 , X axis lnσ. In this Weibull plot (lnln(1-F) -1 The least square method is applied to the data points of -lnσ) to obtain the linear regression line, and its slope is calculated as the Weibull coefficient.

[0185] Crushing load ratio A

[0186] For each medium of the embodiment and the comparative example, in the same manner as the measurement of the minimum crushing load value, based on the formula (9), the crushing load ratio A (Pmin(N) / Pave(N)) of the minimum crushing load value Pmin(N) obtained by measuring the crushing load value of 50 media at a crosshead speed of 0.5 mm / min relative to the average crushing load value Pave(N) was calculated.

[0187] Crushing load ratio B

[0188] For each medium of the embodiment and the comparative example, in the same manner as the measurement of the lowest value of the crushing load value, based on the formula (10), the crushing load ratio B (Pave0.1(N) / Pave(N)) of the average value Pave0.1(N) of the crushing load values ​​measured at a crosshead speed of 0.1 mm / min relative to the average value Pave(N) of the crushing load values ​​of 50 media measured at a crosshead speed of 0.5 mm / min was calculated.

[0189] Coefficient of variation of hardness measured by ultra-micro indentation hardness tester

[0190] For each medium of the embodiment and comparative example, one medium was embedded in a curable embedding resin (epoxy resin) and the curable embedding resin was cured. The medium was ground to 40% to 50% of its diameter, and the cross section was mirror-polished by the aforementioned method to achieve a surface roughness Rz < 0.05 μm in accordance with JIS B0601:2001. Thereafter, an ultra-micro indentation hardness tester (ENT-1100a, manufactured by ELIONIX Co., Ltd.) was used with a Berkovich indenter, with a load of 50 mN, a load application speed of 5 mN / sec, a test load holding time of 1 sec, and an unloading speed of 5 mN / sec. The micro indentation hardness (N / mm) was measured at equal intervals in 10 locations in the diameter direction of the medium cross section. 2 ). Based on the average value and standard deviation of the micro-indentation hardness measured for 10 media, the coefficient of variation of the ultra-micro-indentation hardness was calculated based on the above formula (8).

[0191] Flexural Strength and Weibull Coefficient of Flexural Strength

[0192] Preparation of samples for processing

[0193] Sr.CIP-M manufactured by Kobe Steel, Ltd. was used at 1000 kgf / cm 2 The powders for forming the embodiments and comparative examples were formed by cold isostatic pressing (CIP), and then fired under the same conditions as the medium to produce processing samples. The processing samples were ground into a size of 3 mm in length × 4 mm in width × 45 mm in thickness using a #140 diamond grinding wheel to produce test pieces.

[0194] Flexural Strength and Weibull Coefficient of Flexural Strength

[0195] According to JIS R1601, 3-point bending strength was measured for 10 samples of the test piece at a span of 30 mm and a crosshead speed of 0.5 mm / min, and the arithmetic mean value was taken as the bending strength. In addition, based on the bending strength, the Weibull coefficient of bending strength was obtained for each medium of the aforementioned embodiment and comparative example based on the aforementioned formula (6).

[0196] Fracture toughness

[0197] The SENB method was used to evaluate the flexural strength by three-point bending with a span of 30 mm and a crosshead speed of 0.5 mm / min using the same test piece as the one used to measure the flexural strength. The notch was machined in the center of the tensile surface of the test piece, and the curvature radius of the notch tip was 10 μm and the depth was 1.5 mm. The fracture toughness (K) was calculated based on the above formulas (11) and (12). IC ).

[0198] Distributed processing

[0199] Using the media of the examples and comparative examples, a dual-shaft dispersion bead mill (Dual Apex Mill) (DAM-015, manufactured by Hiroshima Metal Machinery Co., Ltd.) was used, the mill component container was ZTA (alumina zirconium oxide composite material), the rotor was individual UHMV (made of polyethylene), the media filling amount was 60% by volume of the mill volume, the rotor speed was 8 m / s, and the dispersion treatment of the treated powder was carried out under the following conditions. The temperature of the first test slurry was a temperature below 40°C, or it was carried out at a temperature above 40°C. In Example 8, the temperature of the first test slurry was carried out at two temperatures: a temperature below 40°C and a temperature above 40°C.

[0200] Processed powder: Titanium oxide (primary particle size measured by transmission electron microscope (TEM) image is 35nm (catalog value), specific surface area measured by BET method is 37m 2 / g(directory value)

[0201] First test slurry concentration: 10 mass%

[0202] Slurry flow rate for the first test: 160 mL / min

[0203] Dispersion time: 3 hours

[0204] Crushing and dispersion of calcium carbonate (CaCO3)

[0205] The media of Examples 2 and 7 and the media of Comparative Examples 6 and 8 were used in a double-shaft dispersion bead mill (DAM-015, manufactured by Hiroshima Metal Machinery Co., Ltd.), the mill component container was ZTA (alumina zirconium oxide composite material), the rotor was UHMV (polyethylene), the media filling amount was 60% by volume of the mill volume, the rotor speed was 8 m / s, and the treated powder was mixed with water under the following conditions to prepare a second test slurry for dispersion treatment. The temperature of the dispersion treatment is recorded in Table 5.

[0206] Processed powder: calcium carbonate (average particle size 2.1 μm (catalog value) obtained by laser diffraction particle size distribution measurement, specific surface area 10 m 2 / g(directory value)

[0207] Second test slurry concentration: 10 mass%

[0208] Second test slurry flow rate: 160 mL / min

[0209] Dispersion time: 3 hours

[0210] Wear rate

[0211] After the dispersion treatment, the amount of ZrO2 contained in the first test slurry or the second test slurry is measured as medium wear powder from the treated powder (titanium oxide powder and calcium carbonate powder) after the dispersion treatment by high-frequency inductively coupled plasma emission spectrometry (ICP) using an ICP emission analyzer (ICPS-8100, manufactured by Shimadzu Corporation). The wear rate (mass ppm / hour) obtained by measuring the amount of ZrO2 in the treated powder (titanium oxide) after the dispersion treatment is recorded in Table 4. In addition, the wear rate (mass ppm / hour) obtained by measuring the amount of ZrO2 in the treated powder (calcium carbonate powder) after the dispersion treatment is recorded in Table 5. The wear rate is calculated according to the following formula (13).

[0212] [Formula 11]

[0213]

[0214] Whether the medium is cracked

[0215] 10% of the total media used was taken out of the media before and after the dispersion treatment, and the images were visually observed at 200 times using a digital microscope (VHX-6000, manufactured by KEYENCE Co., Ltd.). Whether the treated powder (titanium oxide powder) had cracks after the dispersion treatment was recorded in Table 4, and whether the treated powder (calcium carbonate powder) had cracks after the dispersion treatment was recorded in Table 5.

[0216]

Table 1

[0217]

[0218]

Table 2

[0219]

[0220]

Table 3

[0221]

[0222]

Table 4

[0223]

[0224]

Table 5

[0225]

[0226] The media of Examples 1 to 8 fully satisfy the aforementioned requirements (a) to (h), (j), (k), (n) and (o), and in the manufacturing method, also satisfy the aforementioned treatments (p) to (w). In addition, the media of Examples 1 to 8 satisfy the aforementioned requirements (x) and (y), and satisfy the fracture toughness, flexural strength and Weibull modulus of flexural strength required by, for example, material grade III of silicon nitride (Si3N4) bearing balls specified in ASTM International's F2094 or grade 3 of silicon nitride (Si3N4) materials for rolling bearings specified in JIS R1669. When the media of Examples 1 to 5 and Example 8 are used for the crushing and dispersion treatment of the first test slurry containing the treated powder using a medium (water) having a temperature of 40°C or less, the wear rate is less than 100 mass ppm / hour, and the wear resistance is excellent. In addition, when the media of Examples 6 and 7 were used for the pulverization and dispersion treatment of the first test slurry containing the treated powder (titanium oxide powder) with a small primary particle size using a medium (water) with a temperature higher than 40°C, the wear rate was 101 mass ppm / hour or less, and the wear resistance was excellent even when used in warm water. The media of Examples 1 to 7 had no cracks or defects after the pulverization and dispersion treatment, and had excellent durability.

[0227] The media of Examples 2 and 7 were used for the crushing and dispersion of the second test slurry containing the treated powder (calcium carbonate) with an average particle size of 1 μm or more and 10 μm, and the wear rate was also below 1.5 mass ppm / hour, and the wear resistance was excellent. According to this result, it can be confirmed that the aforementioned requirements (a) to (h), preferably the requirements of requirements (j), (k), (n) and (o) are met, and the media is excellent in wear resistance even in the crushing and dispersion of calcium carbonate used as a medicinal powder, without cracking and defect, and can be crushed and dispersed for the treated powder while maintaining the purity of the treated powder and ensuring high purity. Figure 1 This is a photograph taken with a scanning electron microscope (SEM) of the medium of Example 1. The medium of Example 1 has a shape close to a sphere and is excellent in wear resistance.

[0228] The medium of Comparative Example 1 has a Y2O3 / ZrO2 molar ratio of less than 2.5 / 97.5 and a tetragonal zirconium oxide content of less than 90% by volume, which does not meet the requirements of (a) and (c). In addition, the fracture toughness of the medium of Comparative Example 1 is 4.2 MPa·m 1 / 2 The bending strength is 770 MPa, which does not meet some of the requirements (x) and (y). The medium of Comparative Example 1 also does not meet the treatment of (p) in the manufacturing method. The medium of Comparative Example 1 has a high content of monoclinic zirconium oxide of 11 volume %, low mechanical properties, and reduced wear resistance. The crushing load ratio B of the medium of Comparative Example 1 also does not meet the requirement (o).

[0229] The dielectrics of Comparative Examples 2 and 3 do not contain Al2O3 in a range of 0.1 mass % or more and 30.0 mass % or less, and thus do not satisfy the requirement (b). The dielectric of Comparative Example 2 does not contain Al2O3, so the sinterability cannot be improved, and the relative density is less than 95%, and thus does not satisfy the requirement (d). Since the mechanical properties are not improved, the minimum value of the crushing load value Pmin (N) > 600 × D is not satisfied. 2.0 (Requirement (f)). The Weibull coefficient of the crushing load value of the medium of Comparative Example 2 is also lower than 10, which does not meet the requirement (g). The bending strength of the medium of Comparative Example 2 is 700 MPa, which does not meet a part of the requirement (y). Since the medium of Comparative Example 2 is also mixed with a medium of low strength, the stress is concentrated in the medium of low strength, which is prone to cracking and defects, and the wear resistance and durability are reduced. The relative density of the medium of Comparative Example 3 is lower than 95%, which does not meet the requirement (d), and a large number of internal defects remain. Since the mechanical properties of the medium of Comparative Example 3 have not been improved, the minimum value of the crushing load value Pmin (N) > 600×D is not met. 2.0(the requirement of (f) above), the wear resistance and durability are reduced. The coefficient of variation of the micro-indentation hardness measured by the ultra-micro-indentation hardness tester of the medium of Comparative Example 3 is also large, exceeding 5%. The fracture toughness of the medium of Comparative Example 3 is 4.8 MPa·m 1 / 2 The bending strength was 690 MPa, which did not satisfy some of the requirements (x) and (y). The wear resistance of the medium of Comparative Example 3 was further reduced when 40° C. warm water was used in the crushing and dispersion process.

[0230] The media of Comparative Examples 4 and 5 do not meet the requirement that the specific surface area of ​​the mixed powder is within 5m 2 / g or more and 10m 2 / g or less. In addition, the media of Comparative Examples 4 and 5 do not satisfy the treatment of (p) because the pre-sintering temperature when obtaining the synthetic powder is not within the range of 600°C or more and 1200°C or less. The media of Comparative Example 4, since it is a fine powder with a large specific surface area of ​​the mixed powder, has uneven sintering properties and a Weibull coefficient of the crushing load value of less than 10, which does not satisfy the requirement (g). As a low-strength medium, stress will be concentrated in the low-strength part inside the medium, and wear resistance and durability will be reduced.

[0231] The medium of Comparative Example 4 also has a large coefficient of variation of hardness measured by an ultra-micro indentation hardness tester, exceeding 5%, and a crushing load ratio A lower than 0.8, which does not satisfy the requirements (j) and (n).

[0232] The medium of Comparative Example 5 has a small specific surface area and low sinterability, so defects remain inside the sintered body and the relative density is less than 95%, which does not meet the requirement (d). The medium of Comparative Example 5 does not meet the minimum value of the crushing load value Pmin (N) > 600 × D 2.0 (Requirement (f)) The medium of Comparative Example 5 had a flexural strength of 750 MPa and a Weibull modulus of flexural strength of 5.6, which did not satisfy the requirement (y).

[0233] The media of Comparative Examples 4 and 5 further deteriorated in abrasion resistance when warm water higher than 40° C. was used in the pulverization and dispersion process.

[0234] The media of Comparative Examples 6 and 7 do not satisfy the treatment (t) of making the average particle size of the agglomerated powder formed by drying the mixed powder slurry within the range of 1 μm to 5 μm. The media of Comparative Example 6 has an average particle size of the mixed powder of less than 0.3 μm, which does not satisfy the treatment (s). The media of Comparative Example 7 has an SiO2 content of more than 1.0 mass%, which does not satisfy the requirements of (k) or (w). The media of Comparative Examples 6 and 7 have poor formability because the average particle size of the agglomerated powder is not within the range of 1 μm to 5 μm, and the coefficient of variation of the media diameter is more than 6%, which does not satisfy the requirement of (h). The particle size distribution of the media diameter is uneven, and stress is concentrated on the low-strength media, causing cracks and defects, and reducing wear resistance and durability.

[0235] The medium of Comparative Example 6 does not meet the minimum value of the crushing load value Pmin (N)> 600×D 2.0 (Requirement (f) above), the Weibull coefficient of the crushing load value and the crushing load ratio A also do not satisfy the requirements (g) and (n) above. The medium of Comparative Example 6 has a bending strength of 1080 MPa, which does not satisfy part of the requirement (y) above.

[0236] The medium of Comparative Example 7 has a SiO2 content of more than 1.0 mass %, and a second phase formed by SiO2 phase is formed at the grain boundary of ZrO2, which does not meet the minimum value of the crushing load value Pmin (N)> 600×D 2.0 (Requirement (f) above), the crushing load ratio A and the crushing load ratio B also do not satisfy the requirements (n) and (o) above. The medium of Comparative Example 7 has a Weibull modulus of flexural strength of 6.2, which does not satisfy part of the requirement (y) above.

[0237] The medium of Comparative Example 7 has uneven internal shape, so the shrinkage during firing is uneven. Figure 2 Such a shaped sintered body is shown to exist. Figure 2 This is a photograph taken with a scanning electron microscope (SEM) of the medium of Comparative Example 7. The medium containing such a shaped sintered body is subjected to uneven load during dispersion treatment, and is prone to cracking and chipping, which reduces wear resistance and durability. Cracks and chips can be confirmed in the medium after use.

[0238] The medium of Comparative Example 8 has a Y2O3 / ZrO2 molar ratio higher than 3.2 / 96.8, which does not meet the requirement (a). In the medium of Comparative Example 8, the content of cubic zirconium oxide (C) is as high as 6% by volume, which reduces toughness. The medium with low strength is prone to cracking and defects, and wear resistance and durability are reduced. The medium of Comparative Example 8 does not meet the minimum value of crushing load value Pmin (N) > 600 × D 2.0(Requirement (f) above), the crushing load ratio A and the crushing load ratio B also do not satisfy the requirements (n) and (o) above. The medium of Comparative Example 8 has a bending strength of 980 MPa, which does not satisfy part of the requirement (y) above.

[0239] In the medium of Comparative Example 8, it can be confirmed that there is a portion with low strength and Figure 3A The sintered body with such crack intrusion is shown. Figure 3A This is a photograph of the medium of Comparative Example 8 taken with a scanning electron microscope (SEM) before being used for pulverization and / or dispersion. The medium containing the sintered body with such cracks intruding therein receives uneven load during the dispersion process. After the dispersion process, it can be confirmed that Figure 3B Shown are fragments of such a sintered body broken off. Figure 3B This is a photograph of the medium of Comparative Example 8 after the pulverization and / or dispersion treatment, taken with a scanning electron microscope (SEM).

[0240] The media of Comparative Examples 9 and 10 had a sintering temperature outside the range of 1250° C. to 1600° C., and therefore did not satisfy the treatment (v).

[0241] The medium of Comparative Example 9 has a sintering temperature higher than 1600°C, a grain diameter that is too large, and an average grain diameter higher than 0.5 μm, which meets the requirement (e). The medium of Comparative Example 9 has a tetragonal zirconia content lower than 90% by volume, which does not meet the requirement (c). The medium of Comparative Example 9 has a cubic zirconia (C) content of up to 11% by volume, which reduces toughness. The low-strength medium is prone to cracking and defects, and has reduced wear resistance and durability. The medium of Comparative Example 9 has a coefficient of variation of ultra-fine indentation hardness that is higher than 5% and is relatively large, and a crushing load ratio B that is lower than 0.95, which does not meet the requirements (j) and (o). The medium of Comparative Example 9 has a flexural strength of 910 MPa, which does not meet some of the requirements of (y).

[0242] The medium of Comparative Example 10 has a sintering temperature lower than 1250°C, which does not meet the requirements of treatment (v). The medium of Comparative Example 10 is not sintered sufficiently, has residual defects, reduced strength, and reduced wear resistance and durability. The medium of Comparative Example 10 has a relative density of less than 90%, an average grain size of less than 0.25 μm, and a Weibull coefficient of the crushing load value of less than 10, which does not meet the requirements of (d), (e), and (g). The medium of Comparative Example 10 does not meet the minimum crushing load value Pmin (N) > 600×D 2.0 (Requirement (f) above) The medium of Comparative Example 10 has a fracture toughness of 4.9 MPa·m 1 / 2 The flexural strength is 720 MPa, which does not meet some of the requirements (x) and (y).

[0243] The medium of Comparative Example 11 does not satisfy the minimum value of the crushing load value Pmin (N)> 600×D 2.0 (Requirement (f) above). The crushing load ratio A and the crushing load ratio B also do not meet the requirements (n) and (o) above. The dielectric of Comparative Example 11 has a SiO2 content of more than 1.0 mass %, which does not meet the requirement (k) above. The dielectric of Comparative Example 11 has a fracture toughness of 4.8 MPa·m 1 / 2 , the bending strength is 1030 MPa, which does not meet some of the requirements (x) and (y). Since the content of SiO2 in the medium of Comparative Example 11 is higher than 1.0 mass %, a second phase formed by SiO2 phase is formed at the grain boundary of ZrO2, cracks or defects occur, and the wear resistance and durability are reduced. The wear resistance of the medium of Comparative Example 11 is further reduced when warm water higher than 40°C is used in the crushing and dispersion process.

[0244] The medium of Comparative Example 12 has a specific surface area of ​​more than 10 m 2 / g, which does not satisfy the treatment of (r). The medium of Comparative Example 12 has too high sinterability, so the structure cannot be sintered uniformly, and the coefficient of variation of the ultra-fine indentation hardness is higher than 5%, which does not satisfy the requirement of (j). In addition, the crushing load ratio A of the medium of Comparative Example 12 does not satisfy the requirement of (n). The Weibull modulus of the crushing load in the medium of Comparative Example 12 does not satisfy the requirement of (g). The Weibull modulus of the bending strength of the medium of Comparative Example 12 is 5.8, which does not meet some of the requirements of (y). Since the strength of the medium of Comparative Example 12 is uneven, the stress is concentrated on the medium with low strength, and the wear resistance is reduced.

[0245] Industrial Applicability

[0246] The zirconia medium of the present invention can suppress cracking and defects even when used under high load in a high-speed rotating bead mill, has excellent wear resistance and durability, and can maintain the high purity of the processed powder. The zirconia medium of the present invention has no deviation in sintering characteristics and high mechanical properties, so it is not limited to powders used in electronic component materials, and can also be fully utilized as a medium for crushing and dispersing pharmaceutical powders that need to maintain high purity. In addition, due to the high mechanical properties and small shape deviation, it meets the fracture toughness, flexural strength and Weibull modulus of flexural strength required by material grade III of silicon nitride (Si3N4) bearing balls specified in ASTM International's F2094 or grade 3 of silicon nitride (Si3N4) materials for rolling bearings specified in JIS R1669, so it can be fully utilized as a bearing ball. Bearings with zirconia bearing balls can be used in wind turbines, airplanes, cars, bicycles, trains, refrigerators, air conditioners, vacuum cleaners, copiers, washing machines, massage chairs, cameras, electric screwdrivers, personal computers, automatic ticket gates, sidewalks, elevators, conveyors, etc. In addition, they can also be used in medical equipment such as computed tomography (CT), magnetic resonance imaging (MRI), and dental handpieces.

[0247] Explanation of symbols

[0248] 1: bearing, 2: inner ring, 3: outer ring, 4: bearing ball.

Claims

1. A zirconium oxide medium, which satisfies the following requirements (a) to (h): (a) a sintered body comprising ZrO2-Y2O3-based zirconia, wherein the Y2O3 / ZrO2 molar ratio is within a range of 2.5 / 97.5 or more and 3.2 / 96.8 or less; (b) the content of Al2O3 is in the range of 0.1 mass % to 30.0 mass %; (c) containing 90% by volume or more of tetragonal zirconium oxide; (d) relative density is above 95%; (e) an average grain size within a range of 0.25 μm or more and 0.50 μm or less; (f) The minimum value of the crushing load measured at a crosshead speed of 0.5 mm / min satisfies Pmin (N) > 600 × D 2.0 ,in, D is the average value of the medium diameter; (g) The Weibull coefficient of the crushing load value is greater than 10; (h) The maximum diameter of the medium that can be confirmed in the SEM image confirmed by using a scanning electron microscope is defined as the medium diameter, and the coefficient of variation of the medium diameter derived from the average value and standard deviation of the medium diameters of 200 media is less than 6%.

2. The zirconium oxide medium according to claim 1, wherein: (j) In accordance with ISO 14577, a medium is embedded in a curable embedding resin, the curable embedding resin is cured, the medium is ground to 40% to 50% of its diameter and the cross section is mirror-polished, and then the hardness of the cross section of the ground medium is measured at 10 locations at equal intervals using an ultra-micro indentation hardness tester, and the coefficient of variation of the micro indentation hardness derived from the average value and standard deviation of the micro indentation hardnesses measured for the 10 media is 5% or less.

3. The zirconium oxide medium according to claim 1 or 2, wherein: (k) SiO2 is contained in a range of 0.2 mass % to 1.0 mass %.

4. The zirconium oxide medium according to any one of claims 1 to 3, wherein (n) The crushing load ratio A (Pmin(N) / Pave(N), which is the minimum crushing load value Pmin(N) measured at a crosshead speed of 0.5 mm / min, to the average crushing load value Pave(N) is 0.8 or more.

5. The zirconium oxide medium according to any one of claims 1 to 4, wherein (o) The crushing load ratio B, i.e., Pave0.1(N) / Pave(N), of the average crushing load value Pave0.1(N) measured at a crosshead speed of 0.1 mm / min to the average crushing load value Pave(N) measured at a crosshead speed of 0.5 mm / min is greater than 0.

95.

6. A zirconia bearing ball, which meets the following requirements: (a) a sintered body comprising ZrO2-Y2O3-based zirconia, wherein the Y2O3 / ZrO2 molar ratio is within a range of 2.5 / 97.5 or more and 3.2 / 96.8 or less; (b) the content of Al2O3 is in the range of 0.1 mass % to 30.0 mass %; (c) containing 90% by volume or more of tetragonal zirconium oxide; (d) relative density is above 95%; (e) an average grain size within a range of 0.25 μm or more and 0.50 μm or less; (f) The minimum value of the crushing load measured at a crosshead speed of 0.5 mm / min satisfies Pmin (N) > 600 × D 2.0 ,in, D is the average value of the medium diameter; (g) The Weibull coefficient of the crushing load value is greater than 10; (h) the maximum diameter of the medium that can be confirmed in the SEM image confirmed by using a scanning electron microscope is taken as the medium diameter, and the coefficient of variation of the medium diameter derived from the average value and standard deviation of the medium diameters of 200 media is less than 6%; (x) Fracture toughness higher than 5.0 MPa·m 1 / 2 ; (y) The flexural strength is higher than 1100MPa and the Weibull modulus of flexural strength is higher than 7.

7. A method for producing a zirconium oxide medium, wherein: The zirconium oxide medium comprises the following sintered body, and the manufacturing method of the zirconium oxide medium comprises: (p) mixing a zirconium raw material and a yttrium raw material in a manner such that a Y2O3 / ZrO2 molar ratio is within a range of 2.5 / 97.5 or more and 3.2 / 96.8 or less, hydrolyzing the mixture, and pre-calcining the resulting zirconium and yttrium hydrates at a temperature within a range of 600°C or more and 1200°C or less to obtain a synthetic powder; (q) mixing the obtained synthetic powder with Al2O3 powder to obtain a mixed powder in such a manner that the content of Al2O3 is within a range of 0.1 mass % to 30.0 mass % relative to the total amount; (r) drying a mixed powder slurry obtained by wet pulverizing and / or dispersing the mixed powder to obtain a powder having a specific surface area of ​​5 m 2 / g or more and 10m 2 / g or less, and (s) wet-grinding and / or dispersing the mixed powder slurry in such a manner that the average particle size having a cumulative frequency of 50% in a volume-based particle size distribution measured by a laser diffraction method in accordance with JIS Z8825 is within a range of 0.3 μm to 0.6 μm; (t) preparing a molding powder obtained by drying and granulating powder in a slurry for measuring the average particle size of agglomerated powder obtained by mixing 1 part by mass of a powder obtained by drying the mixed powder slurry with 100 parts by mass of a molding solvent in such a manner that the average particle size of agglomerated powder having a cumulative frequency of 50% in a volume-based particle size distribution measured in accordance with JIS Z8825 is within a range of 1 μm to 5 μm; (u) granulating the molding powder to obtain a molded body; (v) The molded body is sintered at a temperature within a range of 1250° C. to 1600° C. to obtain a ZrO 2 —Y 2 O 3 -based zirconia sintered body.

8. The method for producing a zirconium oxide medium according to claim 7, wherein: In the mixed powder, (w) a SiO 2 raw material is contained in such a manner that the content of SiO 2 is within a range of 0.2 mass % to 1.0 mass % based on the total amount.

9. A method for manufacturing a zirconia bearing ball, wherein: The zirconia bearing ball comprises the following sintered body, and the manufacturing method of the zirconia bearing ball comprises: (p) mixing a zirconium raw material and a yttrium raw material in a manner such that a Y2O3 / ZrO2 molar ratio is within a range of 2.5 / 97.5 or more and 3.2 / 96.8 or less, hydrolyzing the mixture, and pre-calcining the resulting zirconium and yttrium hydrates at a temperature within a range of 600°C or more and 1200°C or less to obtain a synthetic powder; (q) mixing the obtained synthetic powder with Al2O3 powder to obtain a mixed powder in such a manner that the content of Al2O3 is within a range of 0.1 mass % to 30.0 mass % relative to the total amount; (r) drying a mixed powder slurry obtained by wet pulverizing and / or dispersing the mixed powder to obtain a powder having a specific surface area of ​​5 m 2 / g or more and 10m 2 / g or less; (s) wet-grinding and / or dispersing the mixed powder slurry in such a manner that the average particle size having a cumulative frequency of 50% in a volume-based particle size distribution measured by a laser diffraction method in accordance with JIS Z8825 is within a range of 0.3 μm to 0.6 μm; (t) preparing a molding powder obtained by drying and granulating powder in a slurry for measuring the average particle size of agglomerated powder obtained by mixing 1 part by mass of a powder obtained by drying the mixed powder slurry with 100 parts by mass of a molding solvent in such a manner that the average particle size of agglomerated powder having a cumulative frequency of 50% in a volume-based particle size distribution measured in accordance with JIS Z8825 is within a range of 1 μm to 5 μm; (u) granulating the molding powder to obtain a molded body; (v) The molded body is sintered at a temperature within a range of 1250° C. to 1600° C. to obtain a ZrO 2 —Y 2 O 3 -based zirconia sintered body.

10. The method for manufacturing a zirconia bearing ball according to claim 9, wherein: In the mixed powder, (w) a SiO 2 raw material is contained in such a manner that the content of SiO 2 is within a range of 0.2 mass % to 1.0 mass % based on the total amount.

Citation Information

Patent Citations

  • Material Vickers hardness determining method based on instrumented indentation of Berkovich and O-P hardness

    CN104101550A

  • Sintered body and cutting tool

    CN106232553A

  • Zirconia powder and zirconia molded body

    JP1999035323A

  • Zirconia ceramic material and method of producing the same

    JP2001163666A

  • Image recording material

    JP2004061945A