Preparation method of small-size transition metal nanoparticles with uniform and adjustable particle size
By regulating the thickness and annealing conditions of the transition metal layer with uniform particle size and adjustable small-size transition metal nanoparticles are prepared by using the interaction between the atmosphere decomposed products in high temperatures, the existing technology is solved The problem of poor size control and stability in the medium achieves efficient and controllable nanoparticle preparation.
Patent Information
- Application Number
- CN202410960091.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to prepare small-sized transition metal nanoparticles with uniform particle size and adjustable particle size, especially at high temperatures, which have poor dimensional control and stability, which limits their application in the fields of catalysis, optics, etc.
By regulating the thickness and annealing conditions of the transition metal layer by utilizing the atmosphere decomposed products at high temperatures, the thickness and annealing conditions of the transition metal layer are adjusted, and the preparation of diameter uniform transition metal nanoparticles of various components and sizes is achieved.
The size adjustability and high temperature stability of transition metal nanoparticles are improved, and the problems of impurities introduction and uneven size are avoided, and a fast, universal and low-cost preparation process is achieved.
Smart Images

Figure HDA0004950012730000011 
Figure HDA0004950012730000021 
Figure HDA0004950012730000022
Abstract
Description
Technical Field
[0001] The invention relates to the field of controllable preparation of nanoparticles, in particular to a method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle sizes. Background Art
[0002] Nanoparticles have high specific surface area, unique physical and chemical properties and many derivative functions, and therefore have broad application prospects in aerospace, electronic products, biotechnology, chemical engineering, environmental engineering, etc. Recent studies have shown that metal nanoparticles with uniform diameters are expected to have important applications in catalysis, optics, magnetism and other fields. However, the problem of spontaneous sintering and agglomeration of nanoparticles at high temperatures needs to be solved urgently, and the poor size control and synthesis efficiency of nanoparticles greatly limit their application development. Therefore, improving the high-temperature stability of nanoparticles and preparing nanoparticles with uniform and adjustable sizes is one of the key issues in the field of nanoscience and technology research.
[0003] At present, the commonly used methods for preparing uniform-sized nanoparticles mainly include solution dispersant method, thermal decomposition method, coprecipitation method, microemulsion method, etc., which mainly prevent agglomeration by combining reagents with the surface of nanoparticles. However, it is still very difficult to prepare nanoparticles with a narrow diameter distribution of less than 5nm with serious quantum confinement effect. That is, when the size of nanoparticles is too small, quantum effects unique to nanomaterials will appear, thereby changing their magnetic, optical, acoustic, thermal, electrical and superconducting properties. Even the use of conventional metal-substrate reaction interactions to prepare uniform-sized small-sized transition metal nanoparticles is limited by the choice of substrate, and the preparation temperature is generally low. Although the mass selection method and differential mobility analysis method for separating nanoparticles can solve the above problems to a certain extent, there are still limitations on the selection of nanoparticle components and the separation of sub-nanometer-sized metal clusters. Among them, the representative works are as follows: (1) Preparation of copper nanoparticles with a diameter of ~2.4 nm by capturing mobile copper sites on a zeolite substrate (Literature 1: Lujie Liu, Jiabi Ma. et al. Science, 2024, 383, 6678); (2) Preparation of metal nanoparticles of uniform size by balancing the infiltration and ripening of metal ions in high-temperature hydrogen, but this method has a slow preparation speed and the particle size is not adjustable (Literature 2: Shunsuke Sakurai; Kenji Hata. et al. JACS, 2012, 134, 2148); (3) Preparation of precious metal nanoparticles with narrow diameter distribution by gas aggregation technology (Literature 3: Patricia Hernandez-Fernandez, Ifan EL Stephens. et al. Nature Chemistry, 2014, 6, 8); (4) Preparation of bimetallic nanoparticles by mass selection method (Literature 4: Feng Yin, Richard E. Palmer. et al. JACS. 2011, 133, 10325).
[0004] Currently, there are still many problems and challenges in preparing transition metal nanoparticles with uniform and adjustable sizes: (1) Metal nanoparticles prepared by the commonly used liquid phase method have disadvantages such as large particle size, many impurities, and poor dispersibility; (2) In dry preparation, particles smaller than 5 nm are unstable at high temperatures and are more likely to aggregate and grow; (3) Transition metal nanoparticles have lower melting points and more active chemical properties than precious metals, and their size is more difficult to control at high temperatures; (4) The preparation process is often complex, time-consuming and costly.
[0005] Therefore, if a method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size can be developed, it will not only avoid the problems of impurities and large particle size introduced by the liquid phase method, but also greatly improve the size uniformity and high-temperature stability of transition metal nanoparticles, which will have important scientific significance and practical value. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size, wherein the transition metal ions can diffuse rapidly on the surface and inside of the support through the interaction between the products of atmosphere decomposition at high temperature and the transition metal and the support; the driving force for Ostwald ripening is provided by utilizing the size difference of nanoparticles, thereby efficiently preparing transition metal nanoparticles of uniform diameter of various sizes and compositions.
[0007] The technical solution of the present invention:
[0008] A method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size, comprising annealing a carrier having a transition metal layer on its surface in a high-temperature atmosphere, and preparing transition metal nanoparticles with various compositions and uniform sizes by regulating the transition metal layer and annealing conditions; wherein the high-temperature atmosphere annealing temperature is 300 to 1000°C, the annealing atmosphere is a single or mixed gas, and the processing time is 1 to 90 minutes.
[0009] In the method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle sizes, the thickness of the transition metal layer is adjusted between 0.1 and 1.0 nm, and the transition metal is distributed on the surface or inside of the carrier in the form of a coating, particles or precursors.
[0010] The method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle sizes is suitable for growing transition metal nanoparticles of various components on oxide substrates or oxide powders, thereby quickly and universally preparing various transition metal nanoparticles of uniform size on various oxide supports.
[0011] In the method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size, the material of the oxide substrate or oxide powder is quartz, aluminum oxide, magnesium oxide or amorphous silicon oxide, and the transition metal nanoparticles are iron, cobalt or nickel.
[0012] In the method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle sizes, the annealing atmosphere is one or more of hydrogen, water vapor, dry air, oxygen and carbon dioxide with different contents and flow rates.
[0013] The method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle sizes has a particle size of 0.4 to 5.0 nm and a standard deviation of the average diameter of the prepared transition metal nanoparticles of less than ±0.17 nm.
[0014] The method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle sizes is characterized in that the size and morphology of the uniform-sized transition metal nanoparticles are maintained for at least 7 minutes in a high-temperature atmosphere of 300 to 1000°C.
[0015] The design idea of the present invention is:
[0016] The present invention utilizes the influence of high temperature atmosphere on transition metal and transition metal-support interaction to reduce the size of nanoparticles, and optimizes the annealing atmosphere and process by designing and screening the reaction system, including the type and thickness of transition metal and support, to increase its stability under high temperature atmosphere. Compared with the traditional Ostwald ripening at high temperature, the present invention achieves rapid diffusion of transition metal ions by regulating the type and content of atmosphere, thereby achieving the minimum energy of the system, that is, uniform nanoparticle size. This method not only avoids the problems of introducing impurities and excessive nanoparticle size, but also has universal applicability to the selection of transition metal and support morphology and type.
[0017] The advantages and beneficial effects of the present invention are:
[0018] 1. The present invention proposes a high-temperature atmosphere annealing treatment method, which utilizes the interaction between the high-temperature atmosphere and the transition metal and the support to achieve efficient preparation of specific small-sized transition metal nanoparticles, and at the same time, the size can continue to be maintained in this high-temperature atmosphere after preparation. This greatly improves the size adjustability and high-temperature stability of the transition metal nanoparticles, and has a very narrow size distribution.
[0019] 2. The present invention utilizes a high-temperature atmosphere annealing method to directly prepare transition metal nanoparticles of uniform diameter in various sizes and compositions on various supports, thus avoiding the problem of requiring secondary processing in liquid phase method, mass selection method and differential mobility analysis method, and has the advantages of simple method, low cost and good controllability.
[0020] 3. The present invention proposes a simple and quick method for obtaining transition metal nanoparticles of uniform diameter in various sizes and compositions, that is, the size of the nanoparticles can be uniformed within 3 minutes, which provides a new idea for material selection in industries such as catalysis and micro-nano manufacturing.
[0021] In summary, the present invention takes the preparation of transition metal nanoparticles of uniform diameter of various sizes and compositions as its starting point, and adopts the method of high-temperature atmosphere annealing to achieve the dry preparation of transition metal nanoparticles of uniform size with adjustable size without introducing impurities and ensuring the high-temperature stability of the nanoparticles, providing a new way to achieve the controllable preparation of transition metal nanoparticles of specific size and composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1.Atomic force microscopy characterization and diameter statistics of Fe nanoparticles grown on ST-cut quartz substrates before and after annealing. Among them, a is the first annealing, b is the second annealing, c is the third annealing, and d is the statistics of nanoparticle diameters in Figures ac.
[0023] Figure 2 .Atomic force microscopy characterization and diameter statistics of Co and Ni nanoparticles grown on ST-cut quartz substrates before and after annealing. Among them, a is the first annealing of Co nanoparticles, b is the second annealing of Co nanoparticles, c is the third annealing of Co nanoparticles, and d is the statistics of Co nanoparticle diameters in ac; e is the first annealing of Ni nanoparticles, f is the second annealing of Ni nanoparticles, g is the third annealing of Ni nanoparticles, and h is the statistics of Ni nanoparticle diameters in eg.
[0024] Figure 3 Atomic force microscopy characterization and diameter statistics of Fe nanoparticles grown on ST-cut quartz substrates after annealing in different atmospheres at 780°C. The annealing atmosphere in Figure a is different flow rates of hydrogen (atmosphere 1) + 250sccm argon + 12sccm argon flowing through 30°C deionized water (atmosphere 2), and Figure b is different flow rates of atmosphere 2 + 250sccm argon + 25sccm hydrogen (atmosphere 1). The bar graphs are the diameter statistics of nanoparticles in the corresponding atmospheres. DETAILED DESCRIPTION
[0025] In the specific implementation process, the present invention uses a carrier containing a transition metal solute or a transition metal film as a raw material and performs an appropriate high-temperature atmosphere annealing treatment to prepare a method for preparing transition metal nanoparticles of uniform diameter of various sizes and compositions. The specific process is as follows:
[0026] The present invention realizes the efficient preparation of transition metal nanoparticles with uniform diameters of various sizes and compositions by annealing in a high temperature atmosphere. In order to increase the rate of homogenization of the nanoparticle size, annealing is selected at a relatively high temperature. During the annealing process, a carrier with a low transition metal content on the surface or inside is selected as much as possible to ensure that the nanoparticles will not sinter due to an excessively high density. Finally, the coupling effect of the high temperature atmosphere on the transition metal and the carrier is utilized to realize the controllable preparation of nanoparticles with uniform diameters of various sizes and compositions, thereby improving the control accuracy of the nanomaterial structure and laying a material foundation for promoting practical applications in the fields of catalysis and micro-nano manufacturing.
[0027] The preferred method is: during the sample preparation process, the process parameters involved are: the voltage and current of the argon ion beam coating instrument are adjusted to 1-5 keV and 10-50 μA respectively, and the transition metal film is plated on the surface of the oxide substrate for 1-100 seconds, that is, a transition metal film with a thickness of 0.1-1.0 nm on the substrate surface is prepared. In the high-temperature atmosphere annealing, the process parameters involved mainly include annealing temperature, time, atmosphere and its content, the annealing temperature is 300°C-1000°C (preferably 700-800°C), the processing time is 1-90 min (preferably 2-5 min), the atmosphere is an inert atmosphere, 0-100% hydrogen and 0-100% oxidizing atmosphere, to achieve efficient preparation of uniform-sized transition metal nanoparticles of various sizes and compositions. In the preferred annealing atmosphere, the argon flow rate is 200-350 sccm, the hydrogen flow rate is 1-30 sccm, and the argon flow rate flowing through 0-50°C deionized water is 5-15 sccm. Among them, the role of argon is carrier gas, the role of hydrogen is to reduce the nanoparticles and promote their precipitation and agglomeration, and the role of water vapor is to promote the dissolution of nanoparticles into the substrate.
[0028] The present invention is further described in detail below through examples and drawings.
[0029] Example 1.
[0030] In this embodiment, the preparation and characterization of small-sized Fe nanoparticles with uniform and adjustable particle size on the substrate surface are as follows:
[0031] The voltage and current of the argon ion beam coating instrument were adjusted to 2.5 keV and 22 μA, respectively, and a Fe film was deposited on the cleaned ST tangential quartz substrate for 10 s. The Fe film thickness was about The coated sample was taken out and placed in a quartz tube of a tube furnace. The quartz tube was first cleaned with 1000 sccm argon for 2 minutes, and then 250 sccm argon, 25 sccm hydrogen (atmosphere 1) and 12 sccm argon flowing through 30°C deionized water (atmosphere 2) were introduced. At the same time, the sample was quickly heated to 780°C and annealed for 3 minutes. Finally, the sample was cooled to room temperature without damaging the sample, taken out and its structure was characterized.
[0032] The characterized sample was loaded into the quartz tube of the tube furnace again, and the quartz tube was cleaned with 1000sccm argon for 2 minutes. Then, 250sccm argon, 1sccm hydrogen (atmosphere 1) and 12sccm argon flowing through 30℃ deionized water (atmosphere 2) were introduced. At the same time, the sample was quickly heated to 780℃ and annealed for 2 minutes. Finally, the sample was cooled to room temperature without damaging the sample, taken out and its structure was characterized.
[0033] Repeat the previous annealing operation. After annealing for 4 minutes, cool the sample to room temperature without damaging it, take it out and characterize its structure.
[0034] Characterization of the structure of Fe nanoparticles: Atomic force microscopy was used to characterize the diameter and distribution of Fe nanoparticles.
[0035] like Figure 1 As shown in (ad), the atomic force microscopy characterization results show that the Fe nanoparticles prepared by annealing the Fe film sample at 780℃ in 250sccm argon + 25sccm hydrogen (atmosphere 1) + 12sccm argon flowing through 30℃ deionized water (atmosphere 2) for 3min are large in size and have good size uniformity. Thereafter, after the sample was further annealed in 250sccm argon + 1sccm hydrogen (atmosphere 1) + 12sccm argon flowing through 30℃ deionized water (atmosphere 2) for 2min and 4min, the average size of the Fe nanoparticles decreased significantly, and the diameter distribution was still very narrow. The above atomic force characterization results were statistically analyzed and found that the diameters of the nanoparticles after the first, second and third annealing were 3.12±0.16nm, 2.05±0.14nm and 0.99±0.13nm, respectively. This strategy of preparing uniform-sized sub-nanoparticles with adjustable size is difficult to match with conventional methods. Therefore, by controlling the annealing time, the nanoparticles can grow and shrink quickly and uniformly, thereby preparing uniform Fe nanoparticles of various sizes.
[0036] Example 2.
[0037] In this embodiment, the preparation and characterization of small-sized Co and Ni nanoparticles with uniform and adjustable particle sizes on the substrate surface are as follows:
[0038] The voltage and current of the argon ion beam coating instrument were adjusted to 2.5 keV and 22 μA, respectively. Co film and Ni film were coated on the cleaned ST tangential quartz substrate for 10 s, respectively. The thickness of the Co film and Ni film were both about The coated samples were taken out and placed in the quartz tube of the tube furnace. The quartz tube was first cleaned with 1000 sccm argon for 2 minutes, and then 250 sccm argon and 25 sccm hydrogen (atmosphere 1) were introduced. At the same time, the sample was quickly heated to 780°C and annealed for 4 minutes. Finally, the sample was cooled to room temperature without damaging the sample, and then taken out for structural characterization.
[0039] The characterized samples were loaded into the quartz tube of the tube furnace again, and the quartz tube was cleaned with 1000 sccm argon for 2 minutes. Then, 225 sccm argon + 25 sccm hydrogen (atmosphere 1) + 12 sccm argon flowing through 30°C deionized water (atmosphere 2) (Co) / 350 sccm argon + 30 sccm hydrogen (atmosphere 1) + 13 sccm argon flowing through 30°C deionized water (atmosphere 2) (Ni) were introduced respectively. At the same time, the sample was quickly heated to 780°C and annealed for 2 minutes. Finally, the sample was cooled to room temperature without damaging the sample, taken out and its structure was characterized.
[0040] The sample after the second characterization was loaded into the quartz tube of the tube furnace again, and the quartz tube was cleaned with 1000sccm argon for 2 minutes, and then 225sccm argon + 1sccm hydrogen (atmosphere 1) + 12sccm argon flowing through 30℃ deionized water (atmosphere 2) (Co) / 350sccm argon + 1sccm hydrogen (atmosphere 1) + 13sccm argon flowing through 30℃ deionized water (atmosphere 2) (Ni) were introduced respectively, and the sample was quickly heated to 780℃ for annealing for 4 minutes. Finally, the sample was cooled to room temperature without damaging the sample, and then taken out and its structure was characterized. Characterization of the structure of Co and Ni nanoparticles: Atomic force microscopy was used to characterize the diameter and distribution of nanoparticles.
[0041] like Figure 2 As shown in (ad), the atomic force microscopy characterization results show that the size distribution of Co nanoparticles prepared by annealing the Co film sample in 250sccm argon + 25sccm hydrogen (atmosphere 1) at 780°C for 4 minutes has a wide distribution. Thereafter, the sample continued to be annealed in 225sccm argon + 25sccm hydrogen (atmosphere 1) + 12sccm argon flowing through 30°C deionized water (atmosphere 2) for 2 minutes, and the diameter distribution of the Co nanoparticles became narrower; after annealing it in 225sccm argon + 1sccm hydrogen (atmosphere 1) + 12sccm argon flowing through 30°C deionized water (atmosphere 2) for 4 minutes, the changes in the Co nanoparticles were similar to those of the Fe nanoparticles in Example 1, that is, the size was uniformly reduced and could also reach the sub-nanometer level. The above atomic force characterization results were statistically analyzed and it was found that the diameters of the nanoparticles after the first, second, and third annealing were 2.80±0.41nm, 2.74±0.16nm, and 0.96±0.11nm, respectively. Comparison Figure 2(eh) It can be seen that only after the introduction of high concentration atmosphere 2, the non-uniform Ni nanoparticles can be quickly homogenized within 2 minutes of annealing, and annealing in low concentration atmosphere 1 and high concentration atmosphere 2 can also make the Ni nanoparticles uniformly reduced. Therefore, by controlling the particle composition and annealing atmosphere, the non-uniform transition metal nanoparticles can be quickly homogenized and the diameter can be adjusted, so that uniform nanoparticles of arbitrary diameter can be prepared using non-uniform nanoparticles of various compositions.
[0042] Comparative Example 1: Effect of the Content of Atmosphere 1 and Atmosphere 2 on the Preparation of Nanoparticles
[0043] The Fe-filmed samples in Example 1 were annealed at 780°C in a single variable controlled atmosphere for 3 min, and the atomic force images and nanoparticle statistics were obtained as shown in 3 (ab). Figure 3 As shown in a, when the flow rates of argon and atmosphere 2 remain unchanged and only the flow rate of atmosphere 1 is changed, the diameter of the nanoparticles first increases and then decreases with the increase of the flow rate of atmosphere 1, and the degree of size homogenization is the same as the diameter change, that is, when the flow rate of atmosphere 1 is 25 sccm, the diameter of the nanoparticles is the largest and the size is most uniform; Figure 3 As shown in Figure b, when the flow rates of argon and atmosphere 1 remain unchanged and only the flow rate of atmosphere 2 is changed, the diameter and size uniformity of the nanoparticles change similarly to those in Figure a as the flow rate of atmosphere 2 increases, that is, the diameter is the largest and the size is the most uniform when the flow rate of atmosphere 2 is 12 sccm.
[0044] Comparison of the atomic force images of the Fe nanoparticles obtained in the above comparative example with the nanoparticles obtained by the first annealing in Example 1 shows that when the argon flow rate is controlled at 250 sccm, only when the flow rate of atmosphere 1 is around 25 sccm (~8.7%) and the flow rate of atmosphere 2 is around 12 sccm (~1300 ppm) can Fe nanoparticles with uniform size and large diameter be quickly prepared. The Fe nanoparticles prepared without the appropriate flow rate and content of atmosphere 1 and atmosphere 2 have a wider diameter distribution, which confirms that the appropriate atmosphere flow rate and content in Example 1 are conducive to the efficient preparation of Fe nanoparticles with uniform size.
[0045] Comparative Example 2: Effect of the Existence Form of Transition Metals on the Preparation of Nanoparticles
[0046] The sample coated with Fe film in Example 1 was annealed at 780°C in 250sccm argon + 1sccm hydrogen (atmosphere 1) + 12sccm argon flowing through 30°C deionized water (atmosphere 2) for 4 minutes, and other treatment conditions were the same as in Example 1. After the treatment, the Fe film on the ST tangential quartz surface had completely penetrated into it. Then the sample was annealed in 250sccm argon + 25sccm hydrogen (atmosphere 1) + 12sccm argon flowing through 30°C deionized water (atmosphere 2) for 4 minutes, and it was found that Fe nanoparticles were uniformly precipitated.
[0047] Comparing the atomic force images of the Fe nanoparticles obtained in the above comparative example with the nanoparticles obtained by the first annealing in Example 1, it is found that the average diameter of the nanoparticles is smaller than that of the nanoparticles in Example 1, but the diameter distribution is still very narrow. This confirms that the method of coating the Fe film on the surface of the substrate in Example 1 and the method of solid solution of iron ions in the substrate in Comparative Example 2 can both quickly prepare Fe nanoparticles of uniform size.
[0048] Comparative Example 3: Effects of atmosphere type and annealing temperature on nanoparticle preparation
[0049] The Fe film-coated sample in Example 1 was annealed in 250sccm argon + 25sccm hydrogen (atmosphere 1) + 0.04sccm oxygen, carbon dioxide and dry air (~1300ppm) for 4 minutes respectively, and the annealing temperature was changed at 300-1000℃ to study the effects of the type of oxidizing atmosphere and annealing time on the preparation of Fe nanoparticles. The results show that the size distribution of the Fe nanoparticles is narrower than when the oxidizing atmosphere is not introduced, and the size is smaller. As the annealing temperature increases, the diameter and size distribution of the nanoparticles show a trend of first increasing and then decreasing. This confirms that annealing at 780℃ in atmosphere 1 and atmosphere 2 in Example 1 is more conducive to the efficient preparation of Fe nanoparticles of uniform size.
[0050] Comparative Example 4: Effect of Oxide Support Morphology and Composition on Nanoparticle Preparation
[0051] Magnesium oxide, aluminum oxide, and amorphous silicon oxide substrates were treated under the coating and annealing conditions of Example 1. Quartz, magnesium oxide, aluminum oxide, and amorphous silicon oxide powders were mixed with Fe(OH)3 colloid and dried and then treated under the annealing conditions of Example 1 to study the effects of the morphology and composition of the oxide support on the preparation of Fe nanoparticles. The results show that the Fe nanoparticles on quartz powder, amorphous silicon oxide substrates, and their powders are larger in diameter and uniform in size, while the nanoparticles on magnesium oxide and aluminum oxide substrates and powders are not as uniform in size as quartz and amorphous silicon oxide, but are higher than the samples that were not annealed in atmosphere 2. This further confirms that the quartz in Example 1 is more conducive to the efficient preparation of Fe nanoparticles of uniform size, and has a certain universality for the morphology and composition of oxide supports.
[0052] Comparative Example 5: Effect of annealing time on nanoparticle preparation
[0053] The coated samples in Example 1 were annealed for 1 min, 3 min, 5 min, and 7 min, respectively, and the other treatment conditions were the same as in Example 1. It can be seen that the diameter of the Fe nanoparticles is small when annealed for 1 min, but the size distribution is not uniform. With the increase of annealing time, the diameter of the nanoparticles is larger and the size is uniform at 3 min, while there is no obvious change in the nanoparticles after annealing for 3 min, and only the size of the nanoparticles increases slightly. This confirms that the sample annealing for 3 min in Example 1 can achieve efficient preparation of Fe nanoparticles of uniform size, and the nanoparticles have excellent high temperature stability in this high temperature atmosphere.
[0054] The results of the embodiments and comparative examples show that the present invention utilizes a simple high-temperature atmosphere annealing method, adopts reasonable carrier morphology, composition and transition metal introduction method, appropriate atmosphere type, flow rate and concentration, higher annealing temperature and shorter annealing time, which are conducive to the efficient and rapid preparation of uniform-sized transition metal nanoparticles. By utilizing the interaction between the transition metal and the carrier in the high-temperature atmosphere, we have achieved the controllable preparation of small-sized transition metal nanoparticles with uniform and adjustable particle size. The present invention realizes the rapid, universal and efficient dry preparation of a variety of uniform-sized transition metal nanoparticles without introducing impurities and ensuring the high-temperature stability of the nanoparticles. The preparation process is simple, controllable and low-cost, laying a material foundation for the practical application of nanometal particles in the field of micro-nano manufacturing and catalysis.
[0055] The present invention is not limited to the above-mentioned embodiments and comparative examples, and all modifications and improvements made to the present solution by engineers and technicians in this field under the concept of the present invention should be protected by the claims of the present invention.
Claims
1. A method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size, characterized in that: The support having a transition metal layer on its surface is annealed in a high-temperature atmosphere, and transition metal nanoparticles of various compositions and uniform sizes are prepared by regulating the transition metal layer and annealing conditions; wherein the high-temperature atmosphere annealing temperature is 300 to 1000°C, the annealing atmosphere is a single or mixed gas, and the processing time is 1 to 90 minutes.
2. The method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size according to claim 1, characterized in that: The thickness of the transition metal layer is adjusted between 0.1 and 1.0 nm, and the transition metal is distributed on the surface or inside of the support in the form of a coating, particles or precursors.
3. The method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size according to claim 1, characterized in that: The support is suitable for growing transition metal nanoparticles of various compositions on oxide substrates or oxide powders, thereby rapidly and universally preparing various transition metal nanoparticles of uniform size on various oxide supports.
4. The method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size according to claim 3, characterized in that: The material of the oxide substrate or oxide powder is quartz, aluminum oxide, magnesium oxide or amorphous silicon oxide, and the transition metal nanoparticles are iron, cobalt or nickel.
5. The method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size according to claim 1, characterized in that: The annealing atmosphere is one or more of hydrogen, water vapor, dry air, oxygen and carbon dioxide with different contents and flow rates.
6. The method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size according to claim 1, characterized in that: The particle size of the prepared transition metal nanoparticles is adjusted within the range of 0.4-5.0 nm, and the standard deviation of the average diameter thereof is less than ±0.17 nm.
7. The method for preparing small-sized transition metal nanoparticles with uniform and adjustable particle size according to claim 1, characterized in that: The size and morphology of transition metal nanoparticles of uniform size are maintained for at least 7 minutes in a high temperature atmosphere of 300 to 1000°C.