EVA (Ethylene Vinyl Acetate) packaging adhesive film, preparation method and application
By adding polyisobutene, mesoporous materials, hydroxylamine antioxidants and β-dione to the EVA packaging film, the potential potential potential-induced attenuation problem of photovoltaic modules is solved, and the anti-PID and resistance of the modules is improved Aging performance extends service life.
Patent Information
- Application Number
- CN202310591719.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
Existing photovoltaic modules are susceptible to potential potential induced attenuation (PID) effects, resulting in output power attenuation. The existing EVA packaging film has a high sodium ion mobility under high temperature and high humidity conditions, affecting component performance.
Using an EVA encapsulation film containing polyisobutene, mesoporous materials, hydroxylamine antioxidants and β-diones, to capture sodium ions and carbon dioxide through mesoporous materials, hydroxylamine antioxidants and β-diones prevent yellowing and metal ions migration. , improve the insulation performance and anti-aging properties of the adhesive film.
It significantly reduces the incidence of PID phenomenon, improves the anti-PID performance of the components and the anti-aging properties of long-term use, reduces the penetration of moisture and organic acids, and extends the service life of the adhesive film.
Smart Images

Figure BDA0004245737870000061 
Figure BDA0004245737870000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of photovoltaic packaging materials, and in particular to an EVA packaging adhesive film, a preparation method and application thereof. Background Art
[0002] Although photovoltaic solar energy systems have long been very reliable under field conditions with low degradation and failure rates, they are still susceptible to failures such as corrosion and delamination. Among common reliability issues, the potential induced degradation effect (PID) of photovoltaic modules has attracted much attention. The PID effect can cause the output power of solar cell modules to decay by 20%, and in severe cases, it can decay by more than 50%. According to relevant research results, there are many possible causes for the PID phenomenon of modules, such as the grounding method, system, modules, and cells of the photovoltaic inverter array. It is generally believed that the main cause of PID is that under high temperature and high humidity conditions and negative voltage, the sodium ions inside the glass migrate to the surface of the cell through the packaging material, forming a reverse potential difference on the surface of the cell, which ultimately leads to the generation of PID.
[0003] In order to effectively prevent the PID effect, it can be solved from three aspects: batteries, components and systems. Among them, improving the anti-PID effect of components by improving the EVA packaging film is a more economical choice. Under the PID test environment, moisture penetrates and diffuses into the packaging film EVA, causing the ester bonds in the EVA molecules to hydrolyze and produce freely moving acetic acid. Acetic acid reacts with sodium compounds on the surface of glass containing silicate components to precipitate sodium ions. Under the action of an external electric field, sodium ions move to the surface of the battery and are enriched in the anti-reflection layer, increasing the leakage current and causing the Voc, Isc, FF and Pmax of the component to decay.
[0004] It can be seen that in order to reduce the occurrence of PID and its impact on module performance, preventing water vapor from entering photovoltaic modules through EVA packaging materials and reducing the mobility of sodium ions at a high temperature of 85°C are effective solutions.
[0005] Patent CN103254802A discloses a photovoltaic EVA encapsulation film that resists potential induced decay (PID) of photovoltaic modules. The ions in the photovoltaic modules are captured by metal ion capture agents. This method not only introduces new metal ions such as Mg2+ and Ca2+, but also generates H+ through the cation capture mechanism described therein, further promoting the generation of CH3COOH. Patent CN103756579A introduces the mixing of ionomer resin into EVA to obtain an encapsulation film with good water vapor barrier properties and hydrolysis resistance. CN103525321B provides an anti-PID photovoltaic EVA film, which uses polyolefin ionomers to lock sodium ions. CN103756578A discloses a fluorine-modified EVA encapsulation film and a preparation method thereof, and the specific measure is to add fluorine-containing compounds to ethylene-vinyl acetate copolymers. CN103897612A discloses an anti-PID EVA encapsulation film for solar encapsulation materials, in which PE resin and plasticizer are added to the EVA encapsulation film. Patent CN103146315A introduces a method of mixing a certain proportion of POE into EVA. The encapsulation film produced by this solution has a high volume resistivity. The polarity of fluorinated compounds, ionic polymers, etc. is quite different from that of EVA. If a slightly larger amount is added, the product will be difficult to process. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] The purpose of the present invention is to provide an EVA encapsulation film and a preparation method thereof for resisting potential potential induced degradation of photovoltaic modules in view of the deficiencies in the prior art. The EVA encapsulation film of the present invention has excellent inhibitory effects on degradation caused by light, heat and oxidation, and has a good effect on resisting potential potential induced degradation of photovoltaic modules.
[0008] (II) Technical solution
[0009] To achieve the above object, the present invention is implemented by the following technical scheme: an EVA encapsulation film, the EVA encapsulation film comprising the following components in mass percentage:
[0010] EVA resin 90-98.5%;
[0011] Polyisobutylene 0.1-2%;
[0012] Mesoporous materials 0.1-4%;
[0013] Hydroxylamine antioxidant 0.1-1%;
[0014] β-diketone 0.1-1%;
[0015] Peroxide crosslinking agent 0.3-1.0%;
[0016] Auxiliary cross-linking agent 0.3-1.0%.
[0017] Preferably, the vinyl acetate content in the EVA resin is 27-37% by mass, and the melt index value is 6-40 g / 10 min.
[0018] Preferably, the molecular weight of the polyisobutylene is 350-20,000.
[0019] The molecular weight of the polyisobutylene is further preferably 1000-10000. Polyisobutylene can significantly improve the insulation and sealing properties of the adhesive film, and prevent moisture from entering from the edge during the aging process of the component.
[0020] Preferably, the mesoporous material is any one or more combinations of molecular sieve, sepiolite, zirconium hydrogen phosphate, titanium hydrogen phosphate and silica gel, and the molecular sieve is ZSM-5 and / or MCM-41.
[0021] The average particle size of the mesoporous material is 0.5-10um. The preferred average particle size is 0.5-2um. This type of mesoporous material can timely capture carbon dioxide generated by the decomposition of peroxide crosslinking agents, acetate ions generated by the decomposition of EVA, isocyanic acid generated by the decomposition of co-crosslinking agents, and freely movable sodium ions generated by the reaction of acetic acid and alkali precipitated on the glass surface, thereby significantly reducing the occurrence of PID phenomenon, and it can continue to work. After the mesoporous materials are vacuum dried, their ability to absorb moisture, organic acids, carbon dioxide gas, and sodium ions can be significantly improved.
[0022] Preferably, the hydroxylamine antioxidant is any one or more combinations of N,N-bis(n-octadecyl)hydroxylamine, N,N-dibenzylhydroxylamine and N-benzoylphenylhydroxylamine; the hydroxylamine antioxidant can significantly reduce the yellowing phenomenon of the film.
[0023] Preferably, the β-diketone is any one or more combinations of stearoylbenzoylmethane, dibenzoylmethane and acetylbenzoylmethane; it has excellent anti-ultraviolet function and significantly reduces the yellowing phenomenon of the film.
[0024] The hindered phenol antioxidants, phosphite antioxidants and UV absorbers currently used in EVA encapsulation films improve the long-term anti-aging properties of the film, but the existing anti-aging system EVA film will produce yellowing after long-term use, affecting the light transmittance of the film, and then affecting the photoelectric conversion efficiency. For example, benzophenone UV absorbers, hindered phenol antioxidants and benzotriazole UV absorbers, in addition to the function of absorbing ultraviolet rays, have chromophores that can react with free radicals to form quinone compounds. Hydroxylamine antioxidants and β-diketones will not generate quinone compounds, which improves the anti-yellowing properties of EVA films in long-term use. In addition, β-diketones and hydroxylamine antioxidants can also coordinate with metal ions to form complexes to prevent the migration of metal ions.
[0025] Preferably, the peroxide crosslinking agent is tert-butyl peroxycarbonate-2-ethylhexyl ester.
[0026] Preferably, the auxiliary cross-linking agent is any one of triallyl isocyanurate, trimethylolpropane trimethacrylate, and triallyl cyanurate, or a combination of at least two thereof.
[0027] The auxiliary cross-linking agent is most preferably a compound prepared by mixing triallyl isocyanurate and trimethylolpropane trimethacrylate in a mass ratio of 1:1.
[0028] The second aspect of the present application provides a method for preparing an EVA encapsulation film, which is characterized by comprising the following steps:
[0029] (1) The mesoporous material is vacuum dried at 150° C. for 3-5 hours, and immediately mixed with polyisobutylene at high speed for 2-3 minutes after drying, and then EVA resin, alkylhydroxylamine, β-diketone, peroxide crosslinking agent, and auxiliary crosslinking agent are added in sequence and stirred slowly and evenly.
[0030] (2) After mixing, the mixture is put into an extruder for mixing and plasticizing. The extrudate is subjected to embossing, shaping, cooling, pulling, and winding processes to obtain an EVA encapsulation film that resists potential potential induced degradation of photovoltaic modules.
[0031] A third aspect of the present application provides an application of an EVA encapsulation film in resisting potential potential induced degradation of photovoltaic modules.
[0032] (III) Beneficial effects
[0033] The present invention provides an EVA encapsulation film, a preparation method and an application thereof, which have the following beneficial effects:
[0034] The present invention adopts polyisobutylene to significantly improve the insulation and sealing properties of the EVA film, and prevents external moisture from entering the film. Hydroxylamine antioxidants and β-diketones can effectively improve the anti-aging and yellowing properties of the EVA packaging film and reduce the decomposition of EVA. The mesoporous material can absorb moisture, organic acids, carbon dioxide gas, and sodium ions, thereby effectively improving the anti-PID performance of the component. DETAILED DESCRIPTION
[0035] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0036] Example 1
[0037] 2% of molecular sieve (ZSM-5) with an average particle size of 2um, 1% of sepiolite with an average particle size of 1.5um, and 1% of titanium hydrogen phosphate with an average particle size of 0.5um are vacuum dried at 150°C for 5 hours. After drying, they are immediately mixed with 1% polyisobutylene with a molecular weight of 1300 at high speed for 2 minutes, and then 92.7% of EVA resin with a VA content of 28% and a melt index of 25g / 10min, 0.3% of N,N-bis(n-octadecane)hydroxylamine, 0.5% of stearylbenzoylmethane, 0.5% of 2-ethylhexyl peroxycarbonate, 0.5% of triallyl isocyanurate, and 0.5% of trimethylolpropane trimethacrylate are added and stirred evenly at a slow speed. The mixed material is then put into an extruder for mixing and plasticization, and the extrudate is subjected to embossing, cooling, pulling, and winding processes to obtain an EVA encapsulation film that resists the potential potential induced attenuation of photovoltaic modules.
[0038] Example 2
[0039] 0.1% titanium hydrogen phosphate and 0.1% zirconium hydrogen phosphate were vacuum dried at 150°C for 5h. After drying, they were immediately mixed with 0.5% polyisobutylene with a molecular weight of 400, 0.5% polyisobutylene with a molecular weight of 5000, and 1% polyisobutylene with a molecular weight of 10000 at high speed for 2min. Then, 94.4% EVA resin with a VA content of 28% and a melt index of 25g / 10min, 0.5% N,N-dibenzylhydroxylamine, 0.5% N-benzoylphenylhydroxylamine, 0.5% stearylbenzoylmethane, 0.5% dibenzoylmethane, 1% 2-ethylhexyl peroxycarbonate, 0.2% triallyl isocyanurate, and 0.2% trimethylolpropane trimethacrylate were added and stirred evenly at a slow speed. The mixed material is then put into an extruder for mixing and plasticizing, and the extrudate is subjected to embossing, shaping, cooling, pulling, and winding processes to obtain an EVA encapsulation film that is resistant to potential potential induced attenuation of photovoltaic modules.
[0040] Example 3
[0041] 0.5% of molecular sieve (MCM-41) with an average particle size of 2um and 0.5% of titanium hydrogen phosphate are vacuum dried at 150°C for 5 hours. After drying, they are immediately mixed with 1% of polyisobutylene with a molecular weight of 2400 at high speed for 2 minutes, and then 95.7% of EVA resin with a VA content of 27% and a melt index of 6g / 10min, 0.5% of N,N-bis(n-octadecane)hydroxylamine, 0.3% of acetylbenzoylmethane, 0.3% of dibenzoylmethane, 0.4% of 2-ethylhexyl peroxycarbonate, 0.4% of triallyl isocyanurate, and 0.4% of trimethylolpropane trimethacrylate are slowly stirred evenly. The mixture is then put into an extruder for mixing and plasticizing. After the extrudate is embossed, shaped, cooled, pulled, and coiled, an EVA encapsulation film that resists the potential potential induced attenuation of photovoltaic modules is obtained.
[0042] Comparative Example
[0043] Add 96.8% EVA resin with VA content of 28% and melt index of 25g / 10min, 0.1% titanium hydrogen phosphate, 0.1% zirconium hydrogen phosphate, antioxidant, EVA resin, 0.5% antioxidant 1010, 0.5% UV-531, 0.5% UV-P, 1% 2-ethylhexyl peroxycarbonate, 0.2% triallyl isocyanurate, 0.2% trimethylolpropane trimethacrylate and stir evenly at a slow speed. Then put the mixture into the extruder for mixing and plasticization, and the extrudate is embossed, cooled, pulled and coiled to obtain the EVA packaging film.
[0044] The examples and comparative examples were subjected to volume resistivity, UV accelerated aging, constant humidity and heat aging and PID tests. The specific test methods are as follows:
[0045] 1) Volume resistivity test method: Take an uncured film with a size of 80mm×80mm and a glass with a size greater than 100mm×100mm, 2 non-stick films, and 1 sample backing plate, and stack them in the order of glass / non-stick film / EVA film / non-stick film / sample backing plate, put them into a vacuum laminator, and laminate them at 140℃ for 15min. The sample removed from the non-stick film is required to have a flat upper and lower surface and uniform thickness, and then cooled to room temperature. The sample volume resistivity is tested according to the provisions of GB / T1410-2006, and 3 samples are tested, and the results are averaged.
[0046] 2) UV accelerated aging test
[0047] Cut the glass, EVA film and sample backing board into 300mm×150mm size, and stack them in the order of glass / two layers of EVA film / sample backing board, and laminate them at 140℃ for 15min to obtain laminated samples with no defects in appearance. The crosslinking degree of EVA film reaches more than 75%, and 3 laminated samples are prepared in each group. Carry out irradiation test according to the provisions of IEC61215-2:2016, and cumulative irradiation is 120kWh / m2 at 60℃±5℃. The yellowness index Y1 of the laminated samples before and after the test is determined according to ASTME313-2010, and each sample is measured at no less than 3 points, and the average value is taken. Record the absolute value of the difference between the yellowness index Y1 after aging and the yellowness index Y2 before aging, which is the yellowing index UV-DY.
[0048] 3) Constant humidity and heat aging test
[0049] Take 2 pieces of EVA film with a size of 300mm×300mm, sandwich them between glass with a size of 300mm×300mm and the back plate for the sample, and laminate them at 140℃ for 15min to obtain laminated samples with no defects in appearance. Prepare 3 laminated samples in each group. Put all samples into a high temperature and high humidity aging test chamber. Test conditions: temperature 85℃±2℃. Relative humidity 85%±5%, test 1000h; take out the samples, and then measure the yellowness index Y1 of the laminated samples before and after the test according to ASTME313-2010, measure no less than 3 points for each sample, and take the average value. Record the absolute value of the difference between the yellowness index Y1 after aging and the yellowness index Y2 before aging, which is the yellowing index DH-DY.
[0050] (3)PID test
[0051] Component preparation: conventional cells were used, and the Example and Comparative Example components were prepared in sequence by cell string welding, glass-EVA film-cell-EVA film-backboard stacking and lamination (140°C lamination, vacuuming for 6 minutes, and holding pressure for 10 minutes). The PID test was conducted on the prepared components with power attenuation test in accordance with the standard IEC62804, at 85°C, 85% humidity, and -1500V voltage, and the test was conducted for 192 hours. The power changes of the Example and Comparative Example components before and after the test were compared, and the specific data are shown in the table below:
[0052]
[0053]
[0054] From the test results, the UV accelerated aging and constant humidity and heat aging yellowing value and PID power attenuation of the embodiment are significantly lower than those of the comparative example, indicating that the EVA encapsulation film has good anti-yellowing and anti-PID performance. The film has good reliability and stability.
[0055] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An EVA encapsulation film, characterized in that: The EVA encapsulation film comprises the following components in percentage by mass: EVA resin 90-98.5%; Polyisobutylene 0.1-2%; Mesoporous materials 0.1-4%; Hydroxylamine antioxidant 0.1-1%; β-diketone 0.1-1%; Peroxide crosslinking agent 0.3-1.0%; Auxiliary cross-linking agent 0.3-1.0%.
2. The EVA encapsulation film according to claim 1, characterized in that: The mass content of vinyl acetate in the EVA resin is 27-37%, and the melt index value is 6-40g / 10min.
3. The EVA encapsulation film according to claim 1, characterized in that: The molecular weight of the polyisobutylene is 350-20000.
4. The EVA encapsulation film according to claim 1, characterized in that: The mesoporous material is any one or more combinations of molecular sieve, sepiolite, zirconium hydrogen phosphate, titanium hydrogen phosphate and silica gel, and the molecular sieve is ZSM-5 and / or MCM-41.
5. The EVA encapsulation film according to claim 1, characterized in that: The hydroxylamine antioxidant is any one or more combinations of N,N-bis(n-octadecyl)hydroxylamine, N,N-dibenzylhydroxylamine and N-benzoylphenylhydroxylamine.
6. The EVA packaging film according to claim 1, characterized in that: The β-diketone is any one or more combinations of stearoylbenzoylmethane, dibenzoylmethane and acetylbenzoylmethane.
7. The EVA encapsulation film according to claim 1, characterized in that: The peroxide crosslinking agent is tert-butyl peroxycarbonate-2-ethylhexyl ester.
8. The EVA packaging film according to claim 1, characterized in that: The auxiliary cross-linking agent is any one of triallyl isocyanurate, trimethylolpropane trimethacrylate, and triallyl cyanurate, or a combination of at least two thereof.
9. The method for preparing the EVA encapsulation film according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) The mesoporous material is vacuum dried at 150° C. for 3-5 hours, and immediately mixed with polyisobutylene at high speed for 2-3 minutes after drying, and then EVA resin, alkylhydroxylamine, β-diketone, peroxide crosslinking agent, and auxiliary crosslinking agent are added in sequence and stirred slowly and evenly. (2) After mixing, the mixture is put into an extruder for mixing and plasticizing. The extrudate is subjected to embossing, shaping, cooling, pulling, and winding processes to obtain an EVA encapsulation film that resists potential potential induced degradation of photovoltaic modules.
10. Use of the EVA encapsulation film according to any one of claims 1 to 8 or the EVA encapsulation film prepared by the preparation method according to claim 9 in resisting potential potential induced degradation of photovoltaic modules.
Citation Information
Cited By
Self-repairing EVA (Ethylene Vinyl Acetate) adhesive film and preparation method thereof
CN121271465A
Self-repairable EVA adhesive film and preparation method thereof
CN121271465B