Cold treatment process for roller
Through the three-temperature cooling method and multi-stage tempering treatment, combined with CVD nanocoating and anti-rust grease treatment, the problems of stress concentration and insufficient surface treatment in the cold treatment of the roll are solved, which significantly improves the hardness and wear resistance of the roll and extends the use life.
Patent Information
- Application Number
- CN202411038444.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-26
AI Technical Summary
The existing roll cold treatment process has problems such as concentrated stress, insufficient surface treatment technology and low tempering quality, resulting in poor roll hardness, wear resistance and service life.
Three-time cooling method and multi-stage tempering treatment are used, combined with CVD technology, nanocoat is deposited on the surface of the roll, surface oil stains and impurities are removed, and appropriate anti-rust grease treatment is used.
Significantly reduce internal stress of the roll, improve hardness and wear resistance, extend service life, reduce maintenance and replacement frequency, and reduce production costs.
Smart Images

Figure CN119020581A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of roller processing, in particular to a roller cold treatment process. Background Art
[0002] Rollers are important process equipment in the steel production process. Their performance and life directly affect production efficiency and product quality. In the process of roll manufacturing and use, improving the hardness, wear resistance and toughness of the rolls is the key to ensuring their service life and stable performance. Although the existing cold treatment process has improved the hardness and wear resistance of the rolls to a certain extent, there are still some shortcomings, which are specifically manifested in the following aspects:
[0003] Stress concentration problems during cold treatment:
[0004] Traditional cold treatment processes usually use a single cryogenic treatment step, which has a fast cooling speed. The sudden temperature change can easily lead to stress concentration inside the roll, resulting in cracks and deformation, which affects the mechanical properties of the roll. The existing process lacks a multi-stage cooling strategy and cannot effectively control and reduce the generation of thermal stress.
[0005] Limitations of single tempering treatment:
[0006] The existing process mostly adopts a single tempering treatment, which cannot fully eliminate the residual stress inside the roll, resulting in the roll's hardness and toughness not being able to reach the optimal balance, affecting its service life and performance. Single tempering treatment cannot meet the higher requirements of the roll for comprehensive performance.
[0007] Disadvantages of surface treatment technology:
[0008] Traditional roller surface treatment technologies are mostly simple coating or heat treatment, which cannot effectively improve the surface hardness and wear resistance of the roller. In addition, the thickness and uniformity of the coating are difficult to control, and it is easy to cause peeling and wear problems, which affects the long-term performance and economy of the roller.
[0009] To this end, those skilled in the art provide a roll cold treatment process to solve the problems raised in the above background technology. Summary of the invention
[0010] In view of the deficiencies of the prior art, the present invention provides a roll cold treatment process, which solves the problems of stress concentration, poor surface treatment technology and low tempering quality in the prior art.
[0011] To achieve the above objectives, the present invention is implemented through the following technical solutions: A roll cold treatment process comprises the following steps:
[0012] S1. Use industrial cleaning agent to soak and scrub the rollers to remove surface oil and impurities, and use rust remover to treat surface rust. Finally, use ultrasonic flaw detector and magnetic particle flaw detector to check whether the rollers have internal and surface defects;
[0013] S2, placing the roller at room temperature to cool naturally for 12 hours, and then placing it in a cold treatment box for three cooling operations, so that the roller temperature drops to -196°C;
[0014] S3, firstly, the first tempering is performed, the roller is slowly heated from -196°C to room temperature, then the roller is heated to 200°C, kept at this temperature for 2 hours, and then naturally cooled to room temperature, and then the second deep freezing treatment is performed, after reaching room temperature, the roller is cooled to -196°C again, kept at this temperature for 4 hours, and then the second tempering is performed, after the roller is heated from -196°C to room temperature, the roller is heated to 250°C, kept at this temperature for 2 hours, and then naturally cooled to room temperature;
[0015] S4, after polishing and cleaning the surface of the roller, a coating is deposited on the surface of the roller by using a CVD technique;
[0016] S5. Use a Vickers hardness tester to test the surface hardness of the roller, and apply anti-rust grease on the surface of the roller and store it in a dry, ventilated and anti-corrosion environment.
[0017] Preferably, the three cooling steps in step S2 are as follows:
[0018] S21, cooling: placing the roll in a cold treatment box, and rapidly cooling the roll to -50°C by ultra-fast cooling, and keeping the temperature for 2 hours;
[0019] S22, secondary cooling: continue cooling to -100°C and keep warm for 2 hours;
[0020] S23, final cooling: lower the temperature to -196°C and keep warm for 6 hours.
[0021] Preferably, the cooling rate in step S23 is maintained within 5°C / min.
[0022] Preferably, in the step S3, the first tempering heating rate is controlled within 3°C / min.
[0023] Preferably, in step S4, the coating is made of nano-ceramics.
[0024] Preferably, in step S4, the coating thickness is maintained within 10 μm.
[0025] Preferably, the anti-rust grease in step S5 is specifically poly-α-olefin.
[0026] Preferably, the rust remover in step S1 is ethylenediaminetetraacetic acid.
[0027] The present invention provides a roll cold treatment process, which has the following beneficial effects:
[0028] 1. The present invention uses a three-step cooling method to gradually reduce the temperature of the roll to -196°C. Gradual cooling can reduce the generation of thermal stress and avoid cracks caused by stress concentration in the material. Multi-stage cold treatment can significantly reduce the internal stress of the roll and improve its toughness and overall strength.
[0029] 2. The present invention performs two cryogenic treatments and two tempering treatments. The first cryogenic treatment stabilizes the metal structure, and the first tempering eliminates stress. The second cryogenic treatment further refines the organizational structure, and the second tempering optimizes the organizational properties. Through this composite treatment, the hardness and wear resistance of the rolling mill are significantly improved while retaining sufficient toughness.
[0030] 3. The present invention can significantly improve the hardness and wear resistance of the roller surface by depositing a nano-coating on the roller surface, thereby increasing the service life of the roller, reducing the maintenance and replacement frequency, and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the method flow of the present invention. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Embodiment 1:
[0034] Please refer to the attached Figure 1 The embodiment of the present invention provides a roll cold treatment process, comprising the following steps:
[0035] S1. Use industrial cleaning agent to soak and scrub the roller to remove surface oil and impurities, and use EDTA to treat surface rust. Finally, use ultrasonic flaw detector and magnetic particle flaw detector to check whether the roller has internal and surface defects.
[0036] S2, placing the roller at room temperature to cool naturally for 12 hours, and then placing it in a cold treatment box for three cooling operations, so that the roller temperature drops to -196°C;
[0037] The specific steps of three cooling steps are:
[0038] S21, cooling: placing the roll in a cold treatment box, and rapidly cooling the roll to -50°C by ultra-fast cooling, and keeping the temperature for 2 hours;
[0039] S22, secondary cooling: continue cooling to -100°C and keep warm for 2 hours;
[0040] S23, final cooling: lower the temperature to -196°C, keep warm for 6 hours, and keep the cooling rate within 5°C / min.
[0041] S3, firstly, the first tempering is performed, the roller is slowly heated from -196°C to room temperature, the tempering heating rate is controlled within 3°C / min, then the roller is heated to 200°C, kept at this temperature for 2 hours, and then naturally cooled to room temperature, and then the second deep freezing treatment is performed, after reaching room temperature, the roller is cooled to -196°C again, kept at this temperature for 4 hours, and then the second tempering is performed, after the roller is heated from -196°C to room temperature, the roller is heated to 250°C, kept at this temperature for 2 hours, and then naturally cooled to room temperature;
[0042] S4, after polishing and cleaning the surface of the roller, a coating is deposited on the surface of the roller by CVD technology, the coating is made of nano-ceramics, and the coating thickness is maintained within 10 μm;
[0043] S5. Use a Vickers hardness tester to test the surface hardness of the roller, and apply anti-rust grease on the surface of the roller and store it in a dry, ventilated and corrosion-resistant environment. The anti-rust grease is specifically poly-α-olefin.
[0044] Summarize:
[0045] This embodiment improves the surface hardness and wear resistance of the roller through standard ultra-fast cooling and deep cold tempering treatment combined with CVD nano-ceramic coating, and uses poly-α-olefin anti-rust grease to ensure its anti-corrosion effect during long-term storage.
[0046] Embodiment 2:
[0047] step:
[0048] S1. Use industrial cleaning agent to soak and scrub the rollers to remove surface oil and impurities, and use citric acid to treat surface rust. Finally, use ultrasonic flaw detector and magnetic particle flaw detector to check whether the rollers have internal and surface defects.
[0049] S2, placing the roller at room temperature to cool naturally for 12 hours, and then placing it in a cold treatment box for three cooling operations, so that the roller temperature drops to -196°C;
[0050] S21, cooling: placing the roll in a cold treatment box, and rapidly cooling the roll to -60°C by ultra-fast cooling, and keeping the temperature for 3 hours;
[0051] S22, secondary cooling: continue cooling to -120°C, keep warm for 3 hours;
[0052] S23, final cooling: lower the temperature to -196°C, keep warm for 8 hours, and keep the cooling rate within 4°C / min.
[0053] S3, firstly, the first tempering is performed, the roller is slowly heated from -196°C to room temperature, the tempering heating rate is controlled within 2°C / min, then the roller is heated to 210°C, kept at this temperature for 2.5 hours, and then naturally cooled to room temperature, and then the second deep freezing treatment is performed, after reaching room temperature, the roller is cooled to -196°C again, kept at this temperature for 5 hours, and then the second tempering is performed, after the roller is heated from -196°C to room temperature, the roller is heated to 260°C, kept at this temperature for 2.5 hours, and then naturally cooled to room temperature;
[0054] S4, after polishing and cleaning the surface of the roller, a coating is deposited on the surface of the roller by PVD technology, the coating adopts nano diamond, and the coating thickness is kept within 5 μm;
[0055] S5. Use a Rockwell hardness tester to test the surface hardness of the roller, and apply anti-rust grease on the surface of the roller and store it in a dry, ventilated and anti-corrosion environment. The anti-rust grease is specifically calcium-based anti-rust grease.
[0056] Summarize:
[0057] This embodiment improves the wear resistance and corrosion resistance of the roller by adjusting cooling and tempering parameters and using PVD nano-diamond coating technology and calcium-based anti-rust grease.
[0058] Embodiment three:
[0059] step:
[0060] S1. Use industrial cleaning agent to soak and scrub the rollers to remove surface oil and impurities, and use hydrochloric acid to treat surface rust. Finally, use ultrasonic flaw detector and magnetic particle flaw detector to check whether the rollers have internal and surface defects;
[0061] S2, placing the roller at room temperature to cool naturally for 12 hours, and then placing it in a cold treatment box for three cooling operations, so that the roller temperature drops to -196°C;
[0062] S21, cooling: placing the roll in a cold treatment box, and rapidly cooling the roll to -45°C by ultra-fast cooling, and keeping the temperature for 2 hours;
[0063] S22, secondary cooling: continue cooling to -90°C and keep warm for 2 hours;
[0064] S23. Final cooling: lower the temperature to -196°C and keep it for 5 hours, keeping the cooling rate within 6°C / min.
[0065] S3, firstly, the first tempering is performed, the roller is slowly heated from -196°C to room temperature, the tempering heating rate is controlled within 4°C / min, then the roller is heated to 190°C, kept at this temperature for 1.5 hours, and then naturally cooled to room temperature, and then the second deep freezing treatment is performed, after reaching room temperature, the roller is cooled to -196°C again, kept at this temperature for 3 hours, and then the second tempering is performed, after the roller is heated from -196°C to room temperature, the roller is heated to 240°C, kept at this temperature for 1.5 hours, and then naturally cooled to room temperature;
[0066] S4, after polishing and cleaning the surface of the roller, a coating is deposited on the surface of the roller by CVD technology, the coating is made of nano-aluminum oxide, and the coating thickness is kept within 8 μm;
[0067] S5. Use a Rockwell hardness tester to test the surface hardness of the roller, and apply anti-rust grease on the surface of the roller and store it in a dry, ventilated and corrosion-resistant environment. The anti-rust grease is specifically zinc-based anti-rust grease.
[0068] Summarize:
[0069] This embodiment uses different acidic rust removers and adjusted cold treatment and tempering parameters, and deposits a nano-aluminum oxide coating on the surface, combined with zinc-based anti-rust grease, which significantly improves the hardness and corrosion resistance of the roller.
[0070] Embodiment 4:
[0071] step:
[0072] S1. Use industrial cleaning agent to soak and scrub the rollers to remove surface oil and impurities, and use oxalic acid to treat surface rust. Finally, use ultrasonic flaw detector and magnetic particle flaw detector to check whether the rollers have internal and surface defects.
[0073] S2, placing the roller at room temperature to cool naturally for 12 hours, and then placing it in a cold treatment box for three cooling operations, so that the roller temperature drops to -196°C;
[0074] S21, cooling: placing the roll in a cold treatment box, and rapidly cooling the roll temperature to -55°C by ultra-fast cooling method, and keeping the temperature for 2.5 hours;
[0075] S22, secondary cooling: continue cooling to -110°C, keep warm for 2.5 hours;
[0076] S23, final cooling: lower the temperature to -196°C, keep warm for 7 hours, and keep the cooling rate within 4.5°C / min.
[0077] S3, firstly, the first tempering is performed, the roller is slowly heated from -196°C to room temperature, the tempering heating rate is controlled within 3.5°C / min, then the roller is heated to 220°C, kept at this temperature for 2 hours, and then naturally cooled to room temperature, and then the second deep cold treatment is performed, after reaching room temperature, the roller is cooled to -196°C again, kept at this temperature for 4 hours, and then the second tempering is performed, after the roller is heated from -196°C to room temperature, the roller is heated to 270°C, kept at this temperature for 2 hours, and then naturally cooled to room temperature;
[0078] S4. After polishing and cleaning the surface of the roller, a coating is deposited on the surface of the roller using PVD technology. The coating uses nano-tungsten carbide and the coating thickness is maintained within 6 μm.
[0079] S5. Use a Vickers hardness tester to test the surface hardness of the roller, and apply anti-rust grease on the surface of the roller and store it in a dry, ventilated and corrosion-resistant environment. The anti-rust grease is specifically barium-based anti-rust grease.
[0080] Summarize:
[0081] This embodiment uses oxalic acid to remove rust, combined with optimized cold treatment and tempering steps, and deposits nano-tungsten carbide coatings through PVD, using barium-based anti-rust grease to improve the wear resistance and corrosion resistance of the roller.
[0082] Embodiment five:
[0083] step:
[0084] S1. Use industrial cleaning agent to soak and scrub the rollers to remove surface oil and impurities, and use lactic acid to treat surface rust. Finally, use ultrasonic flaw detector and magnetic particle flaw detector to check whether the rollers have internal and surface defects;
[0085] S2, placing the roller at room temperature to cool naturally for 12 hours, and then placing it in a cold treatment box for three cooling operations, so that the roller temperature drops to -196°C;
[0086] S21, cooling: placing the roll in a cold treatment box, and rapidly cooling the roll to -40°C by ultra-fast cooling, and keeping the temperature for 2 hours;
[0087] S22, secondary cooling: continue cooling to -85°C, keep warm for 2 hours;
[0088] S23, final cooling: lower the temperature to -196°C, keep warm for 6 hours, and keep the cooling rate within 5.5°C / min.
[0089] S3, firstly, the first tempering is performed, the roller is slowly heated from -196°C to room temperature, the tempering heating rate is controlled within 2.5°C / min, then the roller is heated to 180°C, kept at this temperature for 1 hour, and then naturally cooled to room temperature, and then the second deep freezing treatment is performed, after reaching room temperature, the roller is cooled to -196°C again, kept at this temperature for 3 hours, and then the second tempering is performed, after the roller is heated from -196°C to room temperature, the roller is heated to 230°C, kept at this temperature for 1 hour, and then naturally cooled to room temperature;
[0090] S4, after polishing and cleaning the roller surface, a coating is deposited on the roller surface by CVD technology, the coating adopts nano-silicide, and the coating thickness is kept within 7 μm;
[0091] S5. Use a Rockwell hardness tester to test the surface hardness of the roller, and apply anti-rust grease on the surface of the roller and store it in a dry, ventilated and corrosion-resistant environment. The anti-rust grease is specifically organic acid ester anti-rust grease.
[0092] Summarize:
[0093] This embodiment uses lactic acid to remove rust, combined with adjusted cold treatment and tempering parameters, and deposits a nano-silicide coating by CVD, and uses organic acid ester anti-rust grease, which significantly improves the surface hardness and corrosion resistance of the roller.
[0094] Summary
[0095] These five examples show how to optimize the cold treatment process of the roll by selecting different rust removers, adjusting cold treatment and tempering parameters, and selecting different nano-coating materials and anti-rust greases. Each example provides detailed operating steps for different materials and process parameters to achieve higher hardness, wear resistance and corrosion resistance.
[0096] Test experiment
[0097] Experimental conditions:
[0098] Test material: High speed steel roll
[0099] Each treatment process is tested for hardness, wear resistance and corrosion resistance;
[0100] Experimental table:
[0101]
[0102] Summarize:
[0103] All examples showed significantly improved hardness and wear resistance, and the anti-corrosion performance was excellent in a 48-hour salt spray test.
[0104] Comparative experiment
[0105] Comparative experiment 1: Effects of different rust removers
[0106]
[0107] Comparative experiment 2: Effects of different cold treatment parameters
[0108]
[0109] Comparative experiment 3: Effects of different coating materials
[0110]
[0111] Summary:
[0112] Through these comparative experiments, it can be clearly seen that different rust removers, cold treatment parameters and coating materials have a significant impact on the final properties of the roll. Optimizing these process steps can significantly improve the hardness, wear resistance and corrosion resistance of the roll, thereby improving its service life and performance.
[0113] Control group experiment
[0114] Experimental Materials:
[0115] Roller treated with existing process (control group)
[0116] Roller treated by the process of the present invention (experimental group)
[0117] Experimental steps:
[0118] Materials preparation:
[0119] Rollers of the same material and specification are selected and processed using the existing process and the process of the present invention respectively.
[0120] Treatment method:
[0121] Control group: standard treatment according to the existing cold treatment process, including conventional cleaning, single deep cryogenic treatment, single tempering and no coating treatment.
[0122] Experimental group: treated according to the process of the present invention, the specific steps are as follows:
[0123] S1. Treat the roller surface with industrial cleaning agent and EDTA, and inspect with ultrasonic flaw detector and magnetic particle flaw detector.
[0124] S2, pre-cooling for 12 hours, then cooling to -196°C three times:
[0125] S21, cool to -50°C and keep warm for 2 hours;
[0126] S22, cool down to -100°C and keep warm for 2 hours;
[0127] S23. Cool down to -196°C and keep warm for 6 hours.
[0128] S3, two tempering and two deep cooling treatments:
[0129] First tempering: slowly raise the temperature to room temperature, heat to 200℃, and keep warm for 2 hours;
[0130] Second cryogenic treatment: cool to -196℃ and keep warm for 4 hours;
[0131] Second tempering: heat to 250℃ and keep warm for 2 hours.
[0132] S4. Use CVD technology to deposit a nano-ceramic coating on the surface of the roller with a thickness of 10 μm.
[0133] S5. Use a Vickers hardness tester to test the surface hardness of the roller and apply poly-α-olefin anti-rust grease.
[0134] Test items:
[0135] Hardness test: Use Vickers hardness tester and Rockwell hardness tester to measure the surface hardness respectively.
[0136] Wear resistance test: The wear amount was measured using a wear tester.
[0137] Anti-corrosion test: Conduct a 48-hour salt spray test and observe the rust condition.
[0138] Experimental data record:
[0139]
[0140] Experimental analysis:
[0141] Hardness test: The hardness of the roller processed by the process of the present invention is significantly higher than that of the roller processed by the existing process.
[0142] Wear resistance test: The wear amount of the roller treated by the process of the present invention is significantly lower than that of the roller treated by the existing process, indicating that it has better wear resistance.
[0143] Corrosion resistance test: The roller treated by the process of the present invention had no rust in the salt spray test, while the roller treated by the existing process had rust, indicating that the process of the present invention has better corrosion resistance.
[0144] Summarize
[0145] Through the above comparative test experiments, it can be clearly seen that the cold treatment process of the roll of the present invention has obvious advantages over the existing process in terms of improving hardness, wear resistance and corrosion resistance. These improvements can significantly extend the service life of the roll and improve its performance and reliability in industrial applications.
[0146] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A roll cold treatment process, characterized in that: The following steps are involved: S1. Use industrial cleaning agent to soak and scrub the rollers to remove surface oil and impurities, and use rust remover to treat surface rust. Finally, use ultrasonic flaw detector and magnetic particle flaw detector to check whether the rollers have internal and surface defects; S2, placing the roller at room temperature to cool naturally for 12 hours, and then placing it in a cold treatment box for three cooling operations, so that the roller temperature drops to -196°C; S3, firstly, the first tempering is performed, the roller is slowly heated from -196°C to room temperature, then the roller is heated to 200°C, kept at this temperature for 2 hours, and then naturally cooled to room temperature, and then the second deep freezing treatment is performed, after reaching room temperature, the roller is cooled to -196°C again, kept at this temperature for 4 hours, and then the second tempering is performed, after the roller is heated from -196°C to room temperature, the roller is heated to 250°C, kept at this temperature for 2 hours, and then naturally cooled to room temperature; S4, after polishing and cleaning the surface of the roller, a coating is deposited on the surface of the roller by using a CVD technique; S5. Use a Vickers hardness tester to test the surface hardness of the roller, and apply anti-rust grease on the surface of the roller and store it in a dry, ventilated and anti-corrosion environment.
2. A roll cold treatment process according to claim 1, characterized in that: The specific steps of cooling down three times in step S2 are as follows: S21, cooling: placing the roll in a cold treatment box, and rapidly cooling the roll to -50°C by ultra-fast cooling, and keeping the temperature for 2 hours; S22, secondary cooling: continue cooling to -100°C and keep warm for 2 hours; S23, final cooling: lower the temperature to -196°C and keep warm for 6 hours.
3. A roll cold treatment process according to claim 2, characterized in that: The cooling rate in step S23 is maintained within 5°C / min.
4. A roll cold treatment process according to claim 1, characterized in that: In the step S3, the first tempering heating rate is controlled within 3°C / min.
5. A roll cold treatment process according to claim 1, characterized in that: In the step S4, the coating is made of nano-ceramics.
6. A roll cold treatment process according to claim 1, characterized in that: In the step S4, the coating thickness is maintained within 10 μm.
7. A roll cold treatment process according to claim 1, characterized in that: In the step S5, the anti-rust grease is specifically poly-α-olefin.
8. A roll cold treatment process according to claim 1, characterized in that: In step S1, the rust remover is specifically ethylenediaminetetraacetic acid.
Citation Information
Patent Citations
Processing method for increasing service life of cutting wire of strip-cutting and brick-cutting machine
CN104087743A
Subzero treatment method of hard alloy for cold heading mold
CN105132839A