Method for manufacturing metal-coated flexible sheet and metal-coated flexible sheet manufactured using same

By uniform metal coating on the curved part and the back of the mounting part of the flexible plate, the problem of heavy traditional metal belts is solved, and the slimming and lightweighting of the flexible plate is achieved, which enhances the market competitiveness of the product.

CN119031586APending Publication Date: 2024-11-26PANTHEON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410508254.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-04-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The metal bands of existing flexible displays are heavy, limiting their lightweight and thinning in portable terminals, resulting in reduced market competitiveness.

Method used

Using a manufacturing method, the metal material is uniformly coated on the bends and all the backs of the mounting portion of the flexible plate to replace the traditional heavy metal tape, and the mask residue is removed by processes such as peeling liquid, cleaning liquid and plasma pretreatment. and tiny scratches are formed to improve adhesion and deposit metal coatings in the vacuum chamber by sputtering technology.

Benefits of technology

The flexible plate is uniform metal coating on the back, which improves adhesion and durability, reduces surface steps and strength differences, achieves the effect of thinning and lightweighting, and enhances the market competitiveness of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031586A_ABST
    Figure CN119031586A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a metal-coated flexible sheet and a metal-coated flexible sheet manufactured using the same, which enable the back surface of the flexible sheet to be coated with a metal material, thereby imparting electrical characteristics to all the back surfaces of the flexible sheet and achieving thinning and weight reduction. The manufacturing method comprises the following steps: (a) manufacturing a flat flexible plate, the flexible plate is made of metal or non-metal and is provided with a first mounting part and a second mounting part which are formed on the two sides of the flexible plate through a bent part, a fixing prosthesis for connecting the first mounting part and the second mounting part with each other, and a shape processing mask attached to the back surface of the flexible plate; step (b); putting the flexible plate into a stripping solution so that the mask can be stripped from the flexible plate; (c) removing the residue of the mask on the back surface of the flexible plate by spraying a cleaning solution; step (d); removing tiny residues of the mask on the back surface of the flexible plate, and damaging the back surface of the flexible plate to generate specified surface roughness; and step (e); the metal material can be applied to all of the back surfaces of the bending part, the first mounting part and the second mounting part of the flexible plate so as to impart electrical characteristics to the back surface of the flexible plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a metal-coated flexible board and a metal-coated flexible board manufactured using the same, and more specifically, to a method for manufacturing a metal-coated flexible board that can coat the back side of a flexible board with a metal material so as to apply electrical properties to the entire back side of the flexible board and achieve slimness and lightness, and a metal-coated flexible board manufactured using the manufacturing method. Background Art

[0002] As a general display, cathode ray tubes (CRTs) have been rapidly replaced by flat panel displays (hereinafter referred to as "FPDs"). Liquid crystal displays (LCDs), plasma display panels (PDPs), organic light emitting display devices (LEDs), etc. are used as FPDs. The advantages of FPDs are that they are lighter, thinner, and larger in size than CRTs. On the contrary, since FPDs use a glass substrate that can withstand the high temperatures generated in the manufacturing process, there are limitations in providing lightness, thinness, and flexibility. In order to overcome these problems, a flexible display has recently been developed that is made of a flexible material such as plastic, rather than a glass substrate, and that has its display performance even if it is bent like paper.

[0003] Figure 1 (a) to Figure 1 (c) is a perspective view showing a portable terminal having a conventional flexible display.

[0004] like Figure 1 As shown in (a), the portable terminal with a flexible display is configured so that the first body 2 and the second body 3 combined with the flexible display 1 can be unfolded side by side, as shown in FIG. Figure 1 As shown in (b), the flexible display 1 is maintained in a state of being bent at a predetermined angle. Figure 1 As shown in (c), the flexible display 1 is completely folded.

[0005] That is, the portable terminal having such a flexible display 1 is freely folded or unfolded and maintained in a state of being bent at an angle desired by the user.

[0006] Figure 2 is an exploded perspective view showing a portable terminal having a conventional flexible display.

[0007] The first housing 2b and the second housing 3b are combined with each other through the hinge portion 4, and the first plate 2a and the second plate 3a are attached to one surface of the first housing 2b and one surface of the second housing 3b. In addition, the first cover plate 2c and the second cover plate 3c are attached to the other surface of the first housing 2b and the other surface of the second housing 3b. With the movement of the hinge portion 4 covered by the hinge cover 4a, the flexible display 1 attached to the first plate 2a and the second plate 3a is freely folded or unfolded.

[0008] In this case, the folded portion of the first plate 2a and the second plate 3a is a bent portion that is deformed by bending.

[0009] Specifically, the flexible display 1 is attached to the front of the first plate 2a and the second plate 3a having a bent portion, and various types of main components and accessories for providing the functions of the display and the portable terminal are combined to the front of the first plate 2a and the second plate 3a. In addition, a metal tape is attached to the back of the first plate 2a and the second plate 3a having a bent portion to remove the shape processing mask attached when manufacturing the first plate 2a or the second plate 3a, and to give electrical characteristics to the first plate 2a and the second plate 3a.

[0010] The metal strips attached to the backs of the first and second boards 2a and 3a are used to impart electrical characteristics to the first and second boards 2a and 3a, but disadvantageously, the metal strips are thick and heavy. When considering the market situation where the demand for lightweight and slim portable terminals is increasing, the competitiveness of such thick and heavy flexible boards in the market is reduced. Summary of the invention

[0011] Technical issues

[0012] Therefore, the present invention is made in view of the above-mentioned problems existing in the prior art, and an object of the present invention is to provide a method for manufacturing a metal-coated flexible board and a metal-coated flexible board manufactured by the method, which can enable the back side of the flexible board to be coated with metal material, thereby imparting electrical properties to the entire back side of the flexible board and achieving slimming and lightweight.

[0013] Technical Solution

[0014] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for manufacturing a metal-coated flexible board is provided, the manufacturing method comprising the following steps: step (a): manufacturing a flat flexible board, which is made of metal or non-metal and has a first mounting portion and a second mounting portion formed on both sides of the flexible board with a bent portion therebetween, a fixing prosthesis for connecting the first mounting portion and the second mounting portion to each other, and a shape processing mask attached to the back side of the flexible board; step (b): placing the flexible board in a stripping liquid so that the mask can be stripped from the flexible board; step (c): removing the residue of the mask on the back side of the flexible board by spraying a cleaning liquid; step (d): removing tiny residues of the mask on the back side of the flexible board and causing damage to the back side of the flexible board to produce a specified surface roughness; and step (e): allowing a metal material to be coated on all the back sides of the bent portion, the first mounting portion, and the second mounting portion of the flexible board to impart electrical properties to the back side of the flexible board.

[0015] Preferably, step (b) may be performed in a stripping device in the shape of a container storing a stripping solution prepared by mixing sodium hydroxide with water in a ratio of 20 to 30 wt % sodium hydroxide to 70 to 80 wt % water.

[0016] Preferably, step (c) may be performed by a cleaning device having a nozzle shape for discharging a cleaning liquid toward the back side of the flexible board, and the cleaning liquid is water.

[0017] Preferably, if the flexible board is made of non-metal, step (d) can be performed for 90 to 150 seconds by a first pretreatment device having a nozzle shape for discharging a stripping liquid toward the back side of the flexible board, so that the stripping liquid can be sprayed on the back side of the flexible board to remove minute residues of the mask while causing damage to the back side of the flexible board to produce minute scratches with a depth of less than 1 μm on the back side of the flexible board, and each stripping liquid is made by mixing sodium hydroxide and water in a ratio of 20 weight % to 30 weight % of sodium hydroxide and 70 weight % to 80 weight % of water.

[0018] Preferably, if the flexible board is made of metal or non-metal, step (d) can be performed by a second pretreatment device configured as a plasma chamber, in which plasma is generated and the plasma collides with the back side of the flexible board, so that accelerated plasma ions, electrons and reactive atoms collide with the back side of the flexible board to remove tiny residues and at the same time cause damage to the back side of the flexible board to produce tiny scratches with a depth of less than 1 μm on the back side of the flexible board.

[0019] Preferably, step (e) can be carried out in a coating device, in which a sputtering target is provided and the flexible plate is placed on a placement fixture in a position facing the sputtering target, and the placement fixture is capable of moving in the coating device so that a target material produced by a sputtering target made of metal moves to all back sides of the bent portion, the first mounting portion, and the second mounting portion and is deposited on all back sides.

[0020] Preferably, if it is necessary to fix the flexible plate to a placement jig in a coating device, a fixing tape may be attached to a fixing dummy of the flexible plate so that all back sides of the bent portion, the first mounting portion and the second mounting portion of the flexible plate are exposed toward the sputtering target.

[0021] In order to achieve the above-mentioned purpose, according to another aspect of the present invention, there is provided a flexible board manufactured by a method according to any one of the above-mentioned aspects of the present invention, the flexible board comprising: a bending portion, on one side of the interior of the flexible board, a plurality of slits in a direction perpendicular to the bending direction are arranged; a first mounting portion and a second mounting portion are formed on both sides of the flexible board with the bending portion interposed therebetween; a fixing prosthesis protrudes horizontally from the first mounting portion and the second mounting portion to connect the first mounting portion and the second mounting portion to each other with the bending portion interposed therebetween; and a metal coating layer deposited on all back sides of the bending portion, the first mounting portion and the second mounting portion.

[0022] Beneficial Effects

[0023] According to the present invention, a method of manufacturing a metal-coated flexible board enables the back side of the flexible board to be coated with a metal material, thereby imparting electrical characteristics to all of the back side of the flexible board and achieving slimming and lightness.

[0024] In addition, the method according to the present invention enables the shape processing mask attached to the back of the flexible board to be completely removed through the pretreatment process of metal coating, while generating micro-roughness on the back of the flexible board, thereby improving the adhesion of the coated metal on the back of the flexible board and the durability of the product.

[0025] Furthermore, the conventional metal tape is attached to the back sides of the first mounting portion and the second mounting portion except for the bent portion, thereby causing surface steps and strength differences between the area to which the metal tape is attached and the area to which the metal tape is not attached, but according to the present invention, the metal coating layer is uniformly formed on the back sides of the first mounting portion, the second mounting portion, and the bent portion, and such surface steps and strength differences are not generated at all. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 (a) to (c) are diagrams illustrating the operation of a portable terminal having a conventional flexible display.

[0027] Figure 2 is an exploded perspective view of a portable terminal having a conventional flexible display.

[0028] Figure 3 (a) and (b) are top views showing a flexible board according to a conventional embodiment.

[0029] Figure 4 is a flow chart of a method for manufacturing a metal-coated flexible board according to an embodiment of the present invention.

[0030] Figure 5 (a) to (i) are cross-sectional views illustrating a method of manufacturing a metal-coated flexible board according to an embodiment of the present invention.

[0031] Figure 6(a) to (d) are plan views showing a metal coating process in a method for manufacturing a metal-coated flexible board according to an embodiment of the present invention. DETAILED DESCRIPTION

[0032] The present invention can be modified in various ways and can have multiple exemplary embodiments. Specific exemplary embodiments of the present invention are shown in the drawings and described in detail in the specific embodiments. However, this does not limit the present invention to the specific embodiments, and it should be understood that the present invention covers all modifications, equivalents and replacements within the concept and technical scope of the present invention. In the specification, the same reference numerals will be used to describe the same parts.

[0033] Terms such as first, second, A and B can be used to describe various elements, but elements should not be limited by these terms. These terms are only used to distinguish one element from another element. For example, without departing from the scope of the present invention, the first element can be named as the second element. Likewise, the second element can be named as the first element. The term "and / or" includes a combination of multiple related and described items or any one of multiple related and described items.

[0034] When an element is described as being "connected" or "coupled" to another element, the element may be directly connected or coupled to the other element, but it should be understood that other elements may exist between the two elements. Conversely, when an element is described as being "directly connected" or "directly coupled" to another element, it should be understood that other elements do not exist between the two elements.

[0035] The terms used in this application are only used to describe specific exemplary embodiments and are not intended to limit the present invention. Unless the context clearly limits otherwise, the expression of the singular reference also refers to the corresponding expression of the plural. In this application, terms such as "include", "comprise" or "have" are intended to represent those features, quantities, steps, operations, elements or parts described in the specification, or any combination thereof that exists, and it should be understood that the possibility of the existence or addition of one or more additional features, quantities, steps, operations, elements or parts or their combinations is not excluded.

[0036] Unless otherwise defined, all terms (including technical or scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art. Unless explicitly defined in the specification, terms (such as those defined in common dictionaries) should be interpreted as having the same meaning as terms in the context of the relevant technology, and should not be interpreted as having an ideal or overly formal meaning.

[0037] Hereinafter, embodiments according to the present invention will be described in detail with reference to the accompanying drawings.

[0038] Figure 3 (a) and (b) are top views showing a flexible board according to a conventional embodiment.

[0039] Reference Figure 3 In (a) and (b), the flexible board 100 according to the conventional embodiment has a substantially flat shape, and each flexible board 100 has a bent portion 130 formed on one side of the inside thereof in a deformable and bendable manner. Each flexible board 100 has mounting portions 110 and 120 formed on both sides thereof, and the bent portion 130 is interposed between the mounting portions 110 and 120.

[0040] The flexible board 100 may be made of metal or non-metal.

[0041] The flexible board 100 made of metal is made by cutting a board made of a material such as stainless steel, titanium, aluminum, etc. into individual units using etching. In this case, a display is attached to the front side of the flexible board 100 made of metal, and further, since various types of main components and accessories (e.g., computer chips, charging elements, transmission coils, pressure-sensitive switches, etc.) for providing functions of a display and a portable terminal are bonded to the front side of the flexible board 100, only a prescribed area of ​​the front side of the flexible board 100 becomes conductive. Therefore, the entire area of ​​the back side of the flexible board 100 made of metal is not conductive.

[0042] In addition, the flexible board 100 made of non-metal is made by cutting a board made of a material such as plastic, carbon, carbon fiber reinforced plastic (CFRP), glass fiber reinforced plastic (GFRP), etc. into individual units using sandblasting. In this case, the back side of the flexible board 100 made of non-metal does not have conductivity.

[0043] As described above, the display is attached to the front surface of the flexible board 100 , and further, various types of main components and accessories for providing functions of the display and the portable terminal are coupled to the front surface 100 of the flexible board.

[0044] In a state where the flexible display is mounted on the front surface of the flexible board 100, the flexible board 100 has a bending portion 130, and the flexible display is folded or unfolded to an angle within 180° required by the user through the bending portion 130, as shown in FIG. Figure 1 (a) to Figure 2 As described.

[0045] The bending portion 130 has a plurality of slits extending in a direction perpendicular to the bending direction in such a manner as to be arranged to cross each other using micro through-hole processing, and such that the bending portion 130 has a fragile structure.

[0046] The first mounting portion 110 and the second mounting portion 120 are provided on both sides of the flexible board 100 opposite to the bending portion 130 .

[0047] like Figure 3 The flexible board 100 shown in (a) has the first mounting portion 110 and the second mounting portion 120 provided on the left and right sides with respect to the bending portion 130, and thus the flexible board 100 is suitable for a flexible display that can be folded vertically.

[0048] On the contrary, if Figure 3 The flexible board 100 shown in (b) has the first mounting portion 110 and the second mounting portion 120 provided at the top and bottom sides with respect to the bending portion 130 , and thus the flexible board 100 is suitable for a flexible display that can be horizontally folded.

[0049] In order to prevent the minute positional movement of the mounting parts 110 and 120 in the actual assembly process of the components, a fixation prosthesis 200 is further provided to connect the two mounting parts 110 and 120 across the bending part 130. The configuration and function of the fixation prosthesis 200 have been described in detail in Korean Patent Application Publication Nos. 2022-0003920 and 2022-0003921 filed by the same applicant as the present invention, and therefore, will not be described herein. The contents of the above patent applications are incorporated herein by reference in their entirety.

[0050] In the manufacturing process of a conventional flexible board, a metal tape is attached to the back side of the first mounting portion 110 and the back side of the second mounting portion 120 except the bent portion 130 to remove the shape processing mask attached to the back sides of the first mounting portion 110, the second mounting portion 120 and the bent portion 130 when they are manufactured, and to impart electrical characteristics to their entire areas.

[0051] The metal tape attached to the back of the flexible board is used to impart electrical properties to the back of the flexible board, but the disadvantage is that the metal tape is thick (about 30 to 50 μm) and heavy. Considering the increasing market demand for lightweight and slim portable terminals, the market competitiveness of such a thick and heavy flexible board is reduced.

[0052] Specifically, since the metal tape is attached to the back side of the first mounting portion 110 and the back side of the second mounting portion 120 except the bending portion 130, an area to which the metal tape is attached and an area to which the metal tape is not attached are divided on one surface by the tape, thereby generating steps on the surface, and further, there is a strength difference between the area to which the metal tape is attached and the area to which the metal tape is not attached.

[0053] Figure 4 is a flow chart of a method for manufacturing a metal-coated flexible plate according to an embodiment of the present invention, Figure 5(a) to (i) are cross-sectional views illustrating a method of manufacturing a metal-coated flexible board according to an embodiment of the present invention.

[0054] According to the most important feature of the present invention, as described above, the metal tape attached to the back surface of the flexible board 100 to impart electrical characteristics is replaced with a metal coating.

[0055] Although the existing metal tape is thick and heavy, the metal tape is firmly attached to the back side of the flexible board 100, so that the metal tape can be continuously used.

[0056] In order to replace the metal tape, first, when manufacturing the flexible board 100, the shape processing mask attached to the back side of the flexible board 100 must be completely peeled off from the flexible board 100, and further, the residue of the mask remaining on the back side of the flexible board 100 must be cleaned. In addition, micro-roughness is imparted to the back side of the flexible board 100 so that the nano-sized metal material can be firmly deposited on the back side of the flexible board 100.

[0057] Hereinafter, various processing processes and coating processes of the back surface of the flexible board 100 will be described in detail, and it can be understood from these descriptions that the metal coating replacing the metal tape is firmly coated on all the back surfaces of the flexible board 100 .

[0058] In the first process (step S10) (see Figure 5 In (a)), the flexible board 100 is manufactured using the shape processing mask 150 .

[0059] The flexible board 100 is generally flat and has a bent portion 130 formed on one side of the inside thereof in a deformable and bendable manner and mounting portions 110 and 120 formed on both sides thereof across the bent portion 130. In addition, in an actual assembly process of the components, the flexible board 100 has a fixing prosthesis 200 adapted to connect both the mounting portions 110 and 120 across the bent portion 130 to prevent micro-position flow of the mounting portions 110 and 120.

[0060] The flexible board 100 may be made of metal or non-metal.

[0061] The flexible board 100 made of metal is made by cutting a board made of a material such as stainless steel, titanium, aluminum, etc. into individual units using etching. In this case, a display is attached to the front side of the flexible board 100 made of metal, and further, since various types of main components and accessories (e.g., computer chips, charging elements, transmission coils, pressure-sensitive switches, etc.) for providing functions of a display and a portable terminal are bonded to the front side of the flexible board 100, only a prescribed area of ​​the front side of the flexible board 100 becomes conductive. Therefore, the entire area of ​​the back side of the flexible board 100 made of metal is not conductive.

[0062] In addition, the flexible board 100 made of non-metal is made by cutting a board made of a material such as plastic, carbon, carbon fiber reinforced plastic (CFRP), glass fiber reinforced plastic (GFRP), etc. into individual units using sandblasting. In this case, the back side of the flexible board 100 made of non-metal does not have conductivity.

[0063] According to the method of manufacturing the flexible board 100 made of metal using etching or according to the method of manufacturing the flexible board 100 made of non-metal using sandblasting, the shape processing mask 150 is attached to the back surface of the flexible board 100 .

[0064] The shape processing mask 150 may be a dry film resist (DFR).

[0065] In the second process (step S20) (see Figure 5 (b) and Figure 5 In (c)), the shape processing mask 150 attached to the back surface of the flexible board 100 is peeled off.

[0066] The peeling device 210 is used to peel off the mask 150 attached to the back side of the flexible board 100 .

[0067] like Figure 5 As shown in (b), the peeling device 210 has a shape of a container storing a peeling liquid (SL), and puts the flexible board 100 attached with the mask 150 into the peeling liquid for a predetermined time.

[0068] Alternatively, the peeling device 210 has a nozzle shape for discharging the peeling liquid toward the back surface of the flexible board 100, and sprays the peeling liquid toward the back surface of the flexible board 100 to which the mask 150 is attached for a predetermined time.

[0069] In this case, a sodium hydroxide solution is used as the stripping liquid. The sodium hydroxide solution is prepared by mixing sodium hydroxide with water and diluting it to a ratio of 20 wt % to 30 wt % of sodium hydroxide to 70 wt % to 80 wt % of water, and in this case, the flexible board 100 is placed in the stripping liquid until the production film 150 attached to the flexible board 100 is fully stripped.

[0070] Results, such as Figure 5 As shown in (c), the mask 150 is peeled off from the back surface of the flexible board 100, but mask residues are left on the back surface of the flexible board 100.

[0071] In the third process (step S30) (see Figure 5 (d) and Figure 5 In (e)), the residue is removed from the back side of the flexible board 100 .

[0072] In order to remove the residue from the back side of the flexible board 100 , the cleaning device 220 is used.

[0073] like Figure 5 As shown in (d) of FIG. 1 , the cleaning device 220 has a nozzle shape for discharging cleaning liquid (CL), and sprays the cleaning liquid toward the back surface of the flexible board 100 for a predetermined time.

[0074] In this case, water is used as the cleaning liquid. The water is sprayed onto the back surface of the flexible board 100 until the residue of the mask 150 is sufficiently removed from the back surface of the flexible board 100.

[0075] Results, such as Figure 5 As shown in (e), the residue of the mask 150 is cleaned and removed from the back side of the flexible board 100, but minute residues such as adhesion residues of the mask 150, transfer materials, and adhesion stains remain on the back side of the flexible board. In a state where the minute residue of the mask 150 remains, a metal tape may be attached to the back side of the flexible board 100 in conventional practice, but if a metal coating is applied to the back side of the flexible board 100 in a state where the minute residue of the mask 150 remains, the minute residue causes the thickness of the coating to become irregular, thereby undesirably reducing the quality of the metal coating.

[0076] The tiny residues of the mask 150 remaining on the back side of the flexible board 100 cannot be removed by general water or alcohol cleaning, and if the metal coating is applied to the back side of the flexible board 100 in a state where the tiny residues of the mask 150 remain, the adhesion of the coating is reduced, causing the coated metal to easily separate from the back side of the flexible board 100, making it difficult for the flexible board 100 to provide stable functions.

[0077] Thereafter, in the fourth step (step S40) (see Figure 5 (f-1), Figure 5 (f-2) and Figure 5 In (g), the minute residues remaining on the back side of the flexible board 100 are completely removed by pretreatment, and the back side of the flexible board 100 is damaged by pretreatment to obtain the surface roughness of the back side of the flexible board 100.

[0078] The fourth process may be performed differently according to the material of the flexible board 100 .

[0079] As described above, the flexible board 100 is made of metal or non-metal.

[0080] In the case of the fourth process for the flexible board 100 made of non-metal, the removal of the micro residue and the formation of the surface roughness are performed by spraying the stripping liquid (SL). In addition, in the case of the fourth process for the flexible board 100 made of metal or non-metal, the removal of the micro residue and the formation of the surface roughness are performed by plasma etching.

[0081] In the process of spraying the stripping liquid onto the non-metallic flexible board 100 , the first pre-treatment device 230 is used.

[0082] like Figure 5 As shown in (f-1), the first pretreatment device 230 has a nozzle shape for discharging a stripping liquid toward the back side of the flexible board 100. In this case, the stripping liquid is sprayed toward the back side of the flexible board 100 made of non-metal for about 90 to 150 seconds. The stripping liquid is sprayed onto the micro-resin layer formed on the back side of the flexible board 100 made of non-metal, thereby removing minute residues, and in this process, the surface of the micro-resin layer on the back side of the flexible board 100 made of non-metal is damaged to generate minute scratches with a depth of 1 μm or less on the surface of the micro-resin layer.

[0083] In this case, a sodium hydroxide solution is used as the stripping liquid. The sodium hydroxide solution is prepared by mixing sodium hydroxide with water and diluting it to a ratio of 20 to 30 weight % of sodium hydroxide to 70 to 80 weight % of water, but the ratio of sodium hydroxide can be increased according to the state of the micro-residues or the target value of the surface roughness.

[0084] In the process of plasma etching the flexible board 100 made of metal or non-metal, the second pre-processing device 240 is used.

[0085] like Figure 5 As shown in (f-2), the second pretreatment device 240 is configured to enable the flexible board 100 to move in the chamber to cause the injection of reaction gas and the application of strong electric field to generate plasma, so that the accelerated plasma ions, electrons and reaction atoms can collide with the back side of the flexible board 100, thereby removing the micro residue from the back side of the flexible board 100. In this process, the surface of the micro resin layer on the back side of the flexible board 100 is damaged to generate micro scratches with a depth of less than 1 μm on the back side of the flexible board 100.

[0086] Results, such as Figure 5 As shown in (g), the minute residues of the mask 150 are completely removed from the back surface of the flexible board 100, and at the same time, minute scratches are generated on the back surface of the flexible board 100, thereby forming a predetermined surface roughness.

[0087] Removing minute residues from the back surface of the flexible board 100 and forming a prescribed surface roughness by minute scratches enables coating adhesion to be improved at the time of metal coating as a subsequent process.

[0088] Next, in the fifth process (step S50) (see Figure 5 (h) and Figure 5 In (i)), a metal material is coated on the back surface of the flexible board 100 to impart electrical properties to the back surface of the flexible board 100 .

[0089] As described above, the entire area or a prescribed area of ​​the back surface of the flexible board 100 made of metal or non-metal has no conductivity, and thus a metal material needs to be coated thereon to impart electrical characteristics thereto.

[0090] In order to perform such metal coating on the back side of the flexible board 100 , a coating device 250 is used.

[0091] The coating device 250 is a vacuum chamber in which a sputtering target is disposed, and it moves in a state where the flexible board 100 is placed on a placement jig that can move in the vacuum chamber. Argon gas is put into the vacuum chamber, and then a strong voltage is applied to cause free electrons and the argon gas to collide with each other. Positive ions of argon are thus generated, and the positive ions move to the sputtering target in a negatively charged direction and collide with the negative charges. The target material generated by the sputtering target moves to the back side of the flexible board 100 moving on the opposite side thereof by its kinetic energy.

[0092] In this case, the sputtering target is made of a metal material, and the metal material can be selected from aluminum (Al), antimony (Sb), barium (Ba), bismuth (Bi), boron (B), cadmium (Cd), calcium (Ca), cerium (Ce), chromium (Cr), cobalt (Co), copper (Cu), dysprosium (Dy), erbium (Er), europium (Eu), gadolinium (Gd), germanium (Ge), gold (Au), graphite (C), holmium (Ho), hafnium (Hf), indium (In), iridium (Ir), iron (Fe), lanthanum (La), lead (Pb), lithium (Li), lutetium (Lu), magnesium (Mg), manganese (Mn), molybdenum (Mo) , neodymium (Nd), nickel (Ni), niobium (Nb), osmium (Os), palladium (Pd), phosphorus (P), platinum (Pt), potassium (K), praseodymium (Pr), rhenium (Re), rhodium (Rh), rubidium (Rb), ruthenium (Ru), samarium (Sm), scandium (Sc), selenium (Se), silicon (Si), silver (Ag), sodium (Na), strontium (Sr), sulfur (S), tantalum (Ta), tellurium (Te), terbium (Tb), thallium (Tl), thulium (Tm), tin (Sn), titanium (Ti), tungsten (W), vanadium (V), ytterbium (Yb), yttrium (Y), zinc (Zn), zirconium (Zr). Alternatively, multiple metal targets are sequentially used for multi-metal coating (e.g., nickel-silver-titanium).

[0093] In the fifth process (step S50), the metal atoms enter the tiny spaces of the tiny scratches formed on the back surface of the flexible board 100 through the fourth process (step S40) as the surface pretreatment process and firmly adhere thereto without any escape, thereby improving the adhesion of the metal coating layer 160 to the back surface of the flexible board 100. In the fifth process (step S50), further, a prescribed heat is applied to the flexible board 100 to cause the metal atoms deposited on the back surface of the flexible board 100 to deeply enter the tiny spaces of the tiny scratches.

[0094] The metal coating layer 160 firmly deposited on the back side of the flexible board 100 imparts electrical properties to the back side of the flexible board 100, enhances the rigidity of the flexible board 100, prevents the flexible board 100 from being corroded, and enables the heat generated during use to be dissipated to the outside. Most importantly, the metal coating layer 160 deposited on the back side of the flexible board 100 prevents the flexible display attached to the front side of the flexible board 100 from malfunctioning. In addition, the metal coating layer 160 is thin (about 1 μm) and light in weight, thereby achieving slimming and lightweighting.

[0095] In addition, since the existing metal tape is attached to the back sides of the first mounting portion 110 and the second mounting portion 120 except the bending portion 130, a surface step and a strength difference are generated between the area to which the metal tape is attached and the area to which the metal tape is not attached, but according to the present invention, since the metal coating layer 160 is uniformly formed on the back sides of the first mounting portion 110, the back sides of the second mounting portion 120, and the back sides of the bending portion 130, there are no such surface steps and strength differences at all.

[0096] In this case, the flexible board 100 in the coating device 250 is fixed to the placement jig while being in a posture facing the sputtering target fixed in its facing direction so that the target material is uniformly deposited on the bent portion 130 and the two mounting portions 110 and 120 of the flexible board 100 .

[0097] Therefore, if it is desired to fix the flexible board 100 to the placement fixture in the coating device 250, the bent portion 130 and the mounting portions 110 and 120 of the flexible board 100 must not be covered with fixing tools, and further, no obstacles must exist in the path of the target material produced by the sputtering target moving toward the flexible board 100 and thus being deposited on the flexible board 100.

[0098] To this end, in the fifth process (step S50), if the flexible board 100 needs to be fixed to the placement jig in the coating device 250, the fixing tape 251 is attached to the fixing dummy 200 of the flexible board 100. That is, if the flexible board 100 needs to be fixed to the placement jig in the coating device 250, the fixing tape 251 is attached to the fixing dummy 200 of the flexible board 100, and then the flexible board 100 is fixed to the placement jig so that all the back surfaces of the bent portion 130 and the two mounting portions 110 and 120 of the flexible board 100 are exposed toward the sputtering target.

[0099] The fixation prosthesis 200 is made of the same material as the flexible plate 100 and extends from the flexible plate 100 when the flexible plate 100 is manufactured. Each fixation prosthesis 200 protrudes horizontally from the flexible plate 100 and is shaped like a If the component assembling process is completed, the fixation prosthesis 200 is pulled or torn by the worker's hand to be removed from the flexible plate 100.

[0100] Therefore, the fixation prosthesis 200 is an area that does not need to be coated with a metal material.

[0101] like Figure 6 As shown in (a), in the case of a flexible board 100 suitable for a vertically foldable display (in which the first mounting portion 110 and the second mounting portion 120 are formed on the left and right sides relative to the bending portion 130), the fixing belt 251 is attached to the fixing prosthesis 200 located at the top and bottom of the flexible board 100, as shown in FIG. Figure 6 As shown in (b), the flexible plate 100 is fixed in a position facing the sputtering target in the coating device 250. The fixing tape 251 does not cover the bent portion 130 and the two mounting portions 110 and 120 of the flexible plate 100, so that the movement and deposition of the target material produced by the sputtering target are not disturbed, and if it is necessary to remove the fixing tape 251, the fixing tape 251 is completely removed together with the fixing prosthesis 200 when the fixing prosthesis 200 is pulled and removed.

[0102] like Figure 6 As shown in (c), in the case of a flexible board 100 suitable for a horizontally foldable display (in which the first mounting portion 110 and the second mounting portion 120 are formed at the top and bottom thereof with respect to the bent portion 130), the fixing belt 251 is attached to the fixing prosthesis 200 located on the left and right sides of the flexible board 100, as shown in FIG. Figure 6As shown in (d), the flexible plate 100 is fixed in a position facing the sputtering target in the coating device 250. The fixing tape 251 does not cover the bent portion 130 and the two mounting portions 110, 120 of the flexible plate 100, so that the movement and deposition of the target material generated by the sputtering target are not disturbed, and if it is necessary to remove the fixing tape 251, when the fixing prosthesis 200 is pulled and the fixing prosthesis 200 is pulled, the fixing tape 251 is completely removed together with the fixing prosthesis 200.

[0103] The foregoing description of the embodiments of the present invention is presented for the purpose of illustration and is not intended to be exhaustive or limit the present invention to the disclosed precise form. It will be appreciated by those skilled in the relevant art that many modifications and variations may be made according to the above teachings. Therefore, the scope of the present invention is not limited to this detailed description, but is limited by the appended claims.

[0104] Description of Reference Numerals

[0105] 100: flexible board 110: first mounting portion

[0106] 120: first mounting portion 130: bending portion

[0107] 150: Mask 160: Metal coating

[0108] 200: Fixed prosthesis 210: Stripping device

[0109] 220: cleaning device 230: first pre-treatment device

[0110] 240: Second pretreatment device 250: Coating device

Claims

1. A method for manufacturing a metal-coated flexible plate, the method comprising the following steps: Step (a): manufacturing a flat flexible board, the flexible board being made of metal or non-metal and having a first mounting portion and a second mounting portion formed on both sides of the flexible board across a bent portion, a fixing prosthesis for connecting the first mounting portion and the second mounting portion to each other, and a shape processing mask attached to the back side of the flexible board; Step (b): placing the flexible board in a stripping solution so that the mask can be stripped from the flexible board; Step (c): removing residues of the mask on the back side of the flexible board by spraying a cleaning liquid; Step (d); removing tiny residues of the mask on the back side of the flexible board, while damaging the back side of the flexible board to produce a specified surface roughness; as well as Step (e); enabling metal material to be coated on all back surfaces of the bent portion, the first mounting portion, and the second mounting portion of the flexible board to impart electrical characteristics to the back surface of the flexible board.

2. The manufacturing method according to claim 1, wherein: The step (b) is performed in a stripping device having a shape of a container storing the stripping solution, wherein the stripping solution is prepared by mixing sodium hydroxide and water in a ratio of 20 to 30 wt % of sodium hydroxide and 70 to 80 wt % of water.

3. The manufacturing method according to claim 1, wherein: The step (c) is performed by a cleaning device having a nozzle shape for discharging the cleaning liquid toward the back surface of the flexible board, and the cleaning liquid is water.

4. The manufacturing method according to claim 1, wherein: If the flexible board is made of non-metal, the step (d) is performed for 90 to 150 seconds by a first pretreatment device having a nozzle shape for discharging a stripping liquid toward the back side of the flexible board, so that the stripping liquid can be sprayed on the back side of the flexible board to remove minute residues of the mask, while causing damage to the back side of the flexible board to produce minute scratches with a depth of less than 1 μm on the back side of the flexible board, and each stripping liquid is made by mixing sodium hydroxide and water in a ratio of 20 weight % to 30 weight % of sodium hydroxide and 70 weight % to 80 weight % of water.

5. The manufacturing method according to claim 1, wherein: If the flexible board is made of metal or non-metal, the step (d) is performed by a second pretreatment device configured as a plasma chamber, in which plasma is generated, and the plasma collides with the back side of the flexible board, so that accelerated plasma ions, electrons and reactive atoms collide with the back side of the flexible board to remove tiny residues and at the same time cause damage to the back side of the flexible board to generate tiny scratches with a depth of less than 1 μm on the back side of the flexible board.

6. The manufacturing method according to claim 1, wherein: The step (e) is performed in a coating device in which a sputtering target is provided and the flexible plate is placed on a placement fixture in a manner facing the sputtering target, and the placement fixture is movable in the coating device so that a target material produced by a sputtering target made of metal moves to and is deposited on all back sides of the bent portion, the first mounting portion, and the second mounting portion of the flexible plate.

7. The manufacturing method according to claim 6, wherein: If it is necessary to fix the flexible plate to the placement jig in the coating device, a fixing tape is attached to the fixing dummy of the flexible plate so that all rear surfaces of the bent portion, the first mounting portion, and the second mounting portion of the flexible plate are exposed toward the sputtering target.

8. A flexible board manufactured by the manufacturing method according to any one of claims 1 to 7, the flexible board comprising: a bending portion, wherein a plurality of slits are arranged on one side inside the flexible plate in a direction perpendicular to the bending direction; A first mounting portion and a second mounting portion are formed on both sides of the flexible board across the bending portion; a fixing prosthesis protruding horizontally from the first mounting portion and the second mounting portion to connect the first mounting portion and the second mounting portion to each other across the curved portion; as well as A metal coating layer is deposited on all back surfaces of the bending portion, the first mounting portion, and the second mounting portion.