Thermally conductive filler
By using inorganic powder mixture treated with different surface treatment agents as fillers, the problems of thermal conductivity and moldability in the resin composition are solved, and a resin composition with high thermal conductivity and high flowability is achieved, suitable for heat dissipation and sealing materials. .
Patent Information
- Application Number
- CN202380030053.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-26
AI Technical Summary
When the fill amount of the thermally conductive filler is increased in the resin composition, the viscosity of the resin increases, and the moldability decreases, making it difficult to take into account both high thermal conductivity and high moldability.
The inorganic powder mixture treated with different surface treatment agents is used as fillers. By using the first and second surface treatment powders with different hydrophobization degrees, the viscosity of the resin is reduced, the filling rate and thermal conductivity are improved, and the particle size is controlled to be between 0.1 and 2.0 μm. Ensure high liquidity.
The viscosity of the resin is significantly reduced, the moldability and thermal conductivity of the resin composition are improved, and it can effectively fill into narrow voids, which is suitable for heat dissipation materials and sealing materials.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to thermally conductive fillers. Background Art
[0002] In recent years, due to the demand for miniaturization and high performance of electronic components, the high integration of semiconductor devices has developed, and the amount of heat dissipation materials used to effectively dissipate the heat generated by the device is expanding. In addition, the heat dissipation performance is further improved. In order to dissipate the heat generated by semiconductor elements to heat sinks, housings, etc., heat dissipation materials are configured in various paths, and the materials and forms of heat dissipation materials are also varied. Among them, from the perspective of the type of selectable materials and the degree of freedom of form, the demand for heat dissipation materials formed by resin compositions formed by filling fillers (thermal conductive fillers) with high thermal conductivity in resins has increased in the market. As substances commonly used as thermal conductive fillers, aluminum oxide, aluminum nitride, boron nitride, zinc oxide and magnesium oxide can be listed. In addition, for the use of heat dissipation materials formed by resin compositions that expect further improvement in thermal conductivity, there are heat sinks, solid semiconductor sealing materials, liquid semiconductor sealing materials such as underfill, heat dissipation grease and heat dissipation adhesives. When filling fillers in resins, technologies for improving filling properties by surface treatment are widely used (for example, Patent Document 1).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2022-26651 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] In a resin composition, when the amount of filler added to the resin is increased in order to obtain high thermal conductivity, the viscosity of the resin composition increases and the moldability of the resin composition decreases. Therefore, in order to achieve both high thermal conductivity and high moldability, it is required to improve the filling property of the filler. Therefore, an object of the present invention is to provide a thermally conductive filler with high filling property into a resin.
[0008] Solutions for solving problems
[0009] The present inventors have conducted intensive studies to achieve the above-mentioned purpose and have found that when a mixed powder obtained by mixing a surface-treated powder with other inorganic powders treated with a different surface treatment agent is used as a filler, the viscosity of the resin composition can be reduced compared to when these powders are used alone, thereby completing the present invention.
[0010] That is, the present invention is a thermally conductive filler comprising a first surface treated powder and a second surface treated powder having a different degree of hydrophobization from the first surface treated powder. The difference between the degree of hydrophobization of the first surface treated powder and the degree of hydrophobization of the second surface treated powder is preferably 2 or more.
[0011] In addition, the first surface-treated powder is a surface-treated powder of at least one selected from the group consisting of aluminum oxide, aluminum nitride, boron nitride, magnesium oxide, zinc oxide, silicon carbide, silicon nitride, and diamond, and the content of the second surface-treated powder is preferably 2 to 100 parts by volume relative to 100 parts by volume of the first surface-treated powder. The second surface-treated powder is preferably a surface-treated powder of at least one selected from the group consisting of silicon dioxide, aluminum oxide, aluminum nitride, boron nitride, magnesium oxide, zinc oxide, silicon carbide, silicon nitride, and diamond. Furthermore, the first surface-treated powder is preferably an aluminum nitride surface-treated powder. Furthermore, the thermally conductive filler is preferably: in the particle size distribution measured using an ethanol solvent and using a laser diffraction scattering type particle size distribution analyzer, the cumulative volume 50% particle size D50 is 0.1 to 2.0 μm and the coarse particles of 5 μm or more are less than 3% by mass.
[0012] One embodiment of the present invention is a heat dissipation material resin composition including a resin and the thermally conductive filler.
[0013] Effects of the Invention
[0014] By using the thermally conductive filler of the present invention, when filling in a resin, the viscosity of the resin can be reduced compared to the case of using a thermally conductive filler made of a single surface-treated powder. Therefore, it is easy to improve the moldability of the resin composition, or to increase the filling rate and improve the thermal conductivity of the resin composition.
[0015] Among them, if the cumulative volume 50% particle size D50 of the thermally conductive filler is 0.1 to 2.0 μm and the amount of coarse particles of 5 μm or more is controlled to be small, when the thermally conductive filler is mixed with the second surface-treated powder to form a resin composition, the resin composition exhibits extremely high fluidity. Therefore, when the resin composition is used as a heat dissipation material, especially an underfill sealing material, it exhibits extremely excellent characteristics such as being able to reliably fill a heat dissipation material resin composition with high thermal conductivity into a narrow gap. DETAILED DESCRIPTION
[0016] The present invention is a thermally conductive filler, which includes a first surface-treated powder and a second surface-treated powder having a different degree of hydrophobization from the first surface-treated powder. The surface-treated powder refers to a powder that has been surface-treated using a surface treatment agent. In addition, the thermally conductive filler refers to a filler that includes at least 50% by volume of a powder having a thermal conductivity of 15 W / mK or more.
[0017] Usually, a kind of surface treatment agent is used to implement surface treated powder as filler, and it is mixed with resin to make resin combination.By surface treatment, the affinity of resin and filler is improved, and filling property can be improved.On the other hand, when filling in resin, the interaction between surface treated particles can also have an impact, for example, due to the interaction between the surface treatment agents of particle surface, sometimes surface treated particles become difficult to be dispersed in resin.Here, if the surface treated powders with different hydrophobicity are mixed, the interaction between surface treatment agents can be relaxed, and compared with the situation of a kind of surface treatment agent, it is inferred that high filling property can be obtained.
[0018] The surface treatment agent in the present invention can be any known surface treatment agent without particular limitation as long as it forms a chemical bond with the hydroxyl group or the like present in the surface oxide film of the powder to be surface treated and can be bonded to the surface. Examples of the surface treatment agent include silane compounds, aluminate coupling agents, titanate coupling agents, etc. Among them, silane compounds that can react with a high reaction rate can be suitably used.
[0019] Specific examples of the silane compound used as the surface treatment agent include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-acryloxy Alkoxysilanes such as propyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminoethyl-3-aminopropyltrimethoxysilane, 2-aminoethyl-3-aminopropylmethyldimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, p-phenylenyltrimethoxysilane, and allyltrimethoxysilane.
[0020] In addition, examples of silane compounds having non-reactive functional groups include methyltrimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, trimethylmethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, cyclohexyltrimethoxysilane, cyclohexylmethyldimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropylmethyldimethoxysilane, and the like.
[0021] Examples of other silane compounds that can be used include chlorosilanes such as vinyltrichlorosilane, methyltrichlorosilane, dimethyldichlorosilane, trichloromethylsilane, ethyldimethylchlorosilane, propyldimethylchlorosilane, phenyltrichlorosilane, trifluoropropyltrichlorosilane, and isopropyldiethylchlorosilane.
[0022] As the combination of particularly preferred surface treatment agent, the combination of surface treatment agents with high affinity and different hydrophobicity with epoxy resin can be listed. As the high silane compound with affinity of epoxy resin, the silane compound with functional groups such as glycidoxy, amino and epoxy group reaction can be listed. In addition, though there is no reactivity with epoxy group, the functional groups such as methacryloyloxy, acryloxy, phenyl, vinyl and styryl are also high in affinity with epoxy resin, and the silane compound with these functional groups is also suitable. In addition, the silane compound with phenyl and the affinity of epoxy resin are high, which contributes to the low viscosity of resin combination, the improvement of the close adhesion of resin, the mechanical strength of the cured product of composition, etc. Among them, as a particularly suitable combination of silane compounds, a silane compound having a glycidoxy group and a silane compound having an amino group, a silane compound having a glycidoxy group and a silane compound having a methacryloxy group, a silane compound having a methacryloxy group and a silane compound having an amino group, a silane compound having a methacryloxy group and a silane compound having a vinyl group, a silane compound having an amino group and a silane compound having a vinyl group, and a silane compound having an amino group and a silane compound having a phenyl group can be listed. Among these preferred combinations, one can be used as the surface treatment agent for the first surface-treated powder and the other can be used as the surface treatment agent for the second surface-treated powder.
[0023] The raw materials of the first surface-treated powder and the second surface-treated powder of the present invention are not particularly limited, and known powders that can be surface-treated can be used. For example, as the first surface-treated powder and the second surface-treated powder of the present invention, surface-treated powders made of silicon dioxide, aluminum oxide, aluminum nitride, boron nitride, magnesium oxide, zinc oxide, silicon carbide, silicon nitride, or diamond as raw materials can be listed. Among these, the first surface-treated powder is preferably a surface-treated powder of aluminum oxide (thermal conductivity 20W / mK), aluminum nitride (thermal conductivity 180W / mK), boron nitride (thermal conductivity 200W / mK), magnesium oxide (thermal conductivity 40W / mK), zinc oxide (thermal conductivity 50W / mK), silicon carbide (thermal conductivity 270W / mK), silicon nitride (thermal conductivity 30-80W / mK), or diamond (thermal conductivity 2000W / mK) with high thermal conductivity, more preferably a surface-treated powder of aluminum oxide, aluminum nitride, or silicon nitride, and particularly preferably a surface-treated powder of aluminum nitride. In addition, the second surface-treated powder is preferably a surface-treated powder of silicon dioxide, aluminum oxide, aluminum nitride, or silicon nitride, and more preferably a surface-treated powder of aluminum nitride.
[0024] In the present invention, it is important that the first surface treated powder and the second surface treated powder have different hydrophobicity. As mentioned above, by making the hydrophobicity different, the interaction between the particles can be suppressed and the filling property can be improved. The difference in hydrophobicity is preferably 2 or more, and more preferably 5 or more.
[0025] The hydrophobicity of the surface treated powder can be evaluated by the sedimentation in a mixed solvent of water and methanol. This method is a method in which the surface treated powder floats in water but is completely suspended in methanol. That is, in a beaker with a capacity of 200cc, 100cc of methanol aqueous solution is prepared at a concentration of 1% by volume, 1g of surface treated powder is added to each aqueous solution, and the solution in the beaker is stirred for 5 minutes with a magnetic stirrer. The value of the volume percentage of methanol at the time point when 50% of the surface treated powder is suspended in the solution is taken as the hydrophobicity.
[0026] The hydrophobization degree of the first surface-treated powder and the second surface-treated powder is not particularly limited, but is preferably 1 to 25 from the viewpoint of affinity with epoxy resins and (meth)acrylic resins which are preferred as resins of the resin composition described later.
[0027] The particle size of the first surface-treated powder and the second surface-treated powder is not particularly limited. Among them, in the thermally conductive filler of the first surface-treated powder and the second surface-treated powder with different hydrophobicity, the situation where the viscosity reduction effect is particularly easy to obtain when mixing with the resin is the situation where the particle size of the first surface-treated powder and the second surface-treated powder is relatively small. In addition, the small particles of the first surface-treated powder and the second surface-treated powder are advantageous for making the obtained resin composition penetrate into narrow gaps. Therefore, the first surface-treated powder and the second surface-treated powder are preferably 0.1 to 2.0 μm in the particle size distribution measured by a laser diffraction scattering type particle size distribution instrument using an ethanol solvent, and the cumulative volume 50% particle size D50 is preferably 0.1 to 2.0 μm, more preferably 0.1 to 1.5 μm, and further preferably 0.1 to 1.2 μm. The coarse particles of 5 μm or more are preferably less than 3% by mass, and more preferably less than 1% by mass. In the thermally conductive filler obtained by mixing the first surface treated powder and the second surface treated powder, the cumulative volume 50% particle size D50 is also preferably 0.1 to 2.0 μm, more preferably 0.1 to 1.5 μm, and even more preferably 0.1 to 1.2 μm. The coarse particles of 5 μm or more are preferably less than 3% by mass, and more preferably less than 1% by mass.
[0028] The specific surface areas of the first surface-treated powder and the second surface-treated powder of the present invention are not particularly limited. The BET specific surface area measured by a nitrogen adsorption one-point method is 0.5 m 2 / g or more, preferably 12.0m 2 In addition, for the thermally conductive filler obtained by mixing the first surface-treated powder and the second surface-treated powder, the BET specific surface area measured by the nitrogen adsorption single-point method is preferably 0.5 m 2 / g or more, more preferably 2.0m 2 / g or more, preferably 12.0m 2 / g or less, more preferably 11.0m 2 / g or less.
[0029] The mixing ratio of the first surface-treated powder and the second surface-treated powder can be appropriately selected according to the target thermal conductivity and fluidity. Relative to 100 parts by volume of the first surface-treated powder, the second surface-treated powder is preferably 2 parts by volume or more, more preferably 5 parts by volume or more, particularly preferably 10 parts by volume or more, preferably less than 100 parts by volume, more preferably less than 70 parts by volume, and particularly preferably less than 60 parts by volume.
[0030] When the thermally conductive filler of the present invention is used as a filler for a semiconductor sealing material, the α-ray dose generated by the filler is preferably 0.005 counts / cm 2 h or less, and the α-ray dose is more preferably 0.003 counts / cm 2·h or less. Thus, the amount of α rays generated by the semiconductor sealing material can be reduced. When the amount of α rays generated is large, it becomes a cause of semiconductor malfunction, but by using a filler with a low α ray amount, the probability of such an error can be reduced. In the use of bottom filling sealing materials used in a position particularly close to the semiconductor, a low α ray amount is particularly required. It should be noted that the measurement of the α ray amount is performed by counting the α ray amount generated by the powder sample within a certain period of time. α rays are mainly released by radioactive elements such as uranium and thorium derived from natural raw materials. Therefore, by using a refined raw material with less influence from natural raw materials as the raw material of the powder, the α ray amount can be effectively reduced.
[0031] The thermally conductive filler of the present invention may be composed of only the first surface treated powder and the second surface treated powder, or may contain other powders other than the first surface treated powder and the second surface treated powder within the range that does not hinder the effect of the present invention. The content of other powders is preferably 15 volume % or less, and more preferably 10 volume % or less relative to the thermally conductive filler.
[0032] [Method for producing thermally conductive filler]
[0033] The thermally conductive filler of the present invention can be produced simply by preparing a first surface-treated powder and a second surface-treated powder having different degrees of hydrophobization and mixing them at a desired blending ratio.
[0034] The method for producing the first surface-treated powder and the second surface-treated powder is not particularly limited. As a method that can be easily produced, a method of bringing a predetermined amount of a surface treatment agent into contact with a raw material powder and performing a heat treatment can be cited. The amount of the surface treatment agent in contact can be appropriately adjusted according to the type of raw material powder. For example, when the raw material powder is aluminum nitride powder, the amount of the surface treatment agent in contact is 0.1 to 5 parts by mass, preferably 0.5 to 4 parts by mass, relative to 100 parts by mass of the raw material powder. It should be noted that in this specification, the powder before the surface treatment is performed is referred to as "raw material powder".
[0035] In the above-mentioned production method, when the surface-treated powder is an aluminum nitride powder, as the raw aluminum nitride powder before the surface treatment, a powder obtained by a conventionally known method can be used without particular limitation. Examples of methods for producing the raw aluminum nitride powder include direct nitridation, reduction nitridation, and vapor phase synthesis.
[0036] The particle size distribution of the raw aluminum nitride powder is not particularly limited and can be appropriately determined in consideration of the change in particle size caused by the surface treatment of the target surface-treated aluminum nitride powder. The particle size distribution of the raw aluminum nitride powder, for example, is preferably such that the cumulative volume 50% particle size D50 is in the range of 0.1 to 2.0 μm in the particle size distribution measured using a laser diffraction scattering type particle size distribution analyzer. Furthermore, the specific surface area of the raw aluminum nitride powder measured by the BET method is preferably 0.5 m 2 / g or above.
[0037] The raw aluminum nitride powder may also contain impurities such as alkaline earth elements and rare earth elements that are intentionally added in terms of the source of the raw materials or the synthesis method, with an upper limit of about 5 parts by mass. In addition, the raw aluminum nitride powder may also contain boron nitride as an impurity from the source of a deflocculant or a precipitant, with an upper limit of 5 parts by mass. Among them, the amount of impurities that significantly reduce the crystallinity of aluminum nitride becomes a cause of reduced thermal conductivity, so it is not preferred. The aluminum nitride content in the raw aluminum nitride powder is preferably 90% by mass or more, more preferably 95% by mass or more, and further preferably 99% by mass or more.
[0038] The raw aluminum nitride powder needs to have a surface oxide layer in order to react with the surface treatment agent. Generally, the surface oxide layer is formed by natural oxidation during storage of the raw aluminum nitride powder, so there is no need to perform a special operation for providing the oxide layer. However, in order to improve the reaction efficiency of the surface treatment agent, an oxidation treatment step may be deliberately performed.
[0039] It should be noted that, regarding the oxide layer of the raw aluminum nitride powder, the density of the hydroxyl groups in the raw aluminum nitride powder is 0.8 / nm. 2 Above, especially 0.9 / nm 2 Above, 2.0 / nm 2 Below, particularly preferably 1.6 / nm 2 The oxidation treatment was carried out in the following manner. The density of hydroxyl groups was more than 2.0 / nm. 2 The excessively oxidized particles are different from the surface of ordinary aluminum nitride, and there may be a state where the oxidation reaction is excessively advanced, or a state where hydrolysis is advanced and deteriorates into aluminum hydroxide. Such a state will become a surface with low thermal conductivity and is not preferred.
[0040] In the above-mentioned production method, the method of bringing the raw material powder into contact with the surface treatment agent is not particularly limited, and may be any method of dry surface treatment or wet surface treatment.
[0041] Dry surface treatment is a method based on dry mixing of raw material powder and surface treatment agent without the aid of a large amount of solvent. Examples thereof include: a method of vaporizing the surface treatment agent and mixing it with the powder, a method of spraying or dropping a liquid surface treatment agent and mixing it with the powder, a method of diluting the surface treatment agent with a small amount of organic solvent to increase the amount of liquid and then spraying or dropping it, etc.
[0042] Wet surface treatment is a method in which a solvent is used when mixing the raw material powder and the surface treatment agent. For example, there is a method in which the raw material powder and the surface treatment agent are mixed with a solvent and then dried to remove the solvent.
[0043] Sometimes the aggregation of particles is carried out by surface treatment reaction, and sometimes the powder properties and the filling property into the resin are impaired. It is preferred to remove the coarse particles by crushing and classification at this time. As a crushing method, for example, crushing based on dry crushing devices such as mortar grinders, stone crushers, shredders, hammer mills, and pin mills can be listed. As classification treatment, air flow classification, classification using a vibrating screen machine, etc. can be listed.
[0044] [Resin composition]
[0045] The thermally conductive filler of the present invention has high filling properties, and when filled in a resin to constitute a resin composition, the resin composition exhibits excellent viscosity characteristics and fluidity.
[0046] As the resin constituting the resin composition, thermosetting resins and thermoplastic resins can be used without limitation.
[0047] As thermosetting resins, phenolic resins, epoxy resins, melamine resins, urea resins, unsaturated polyester resins, diallyl phthalate resins, polyurethane resins, silicone resins, etc. can be cited. In addition, as thermoplastic resins, vinyl polymerized resins such as (meth) acrylic resins, polystyrene, polyamide, nylon, polyacetal, polycarbonate, polyphenylene ether, polyester, polyethylene terephthalate, cyclic polyolefins, polyphenylene sulfide, polytetrafluoroethylene, polysulfone, liquid crystal polymer, polyetheretherketone, thermoplastic polyimide, polyamideimide, etc. can be cited. Among them, epoxy resins and (meth) acrylic resins are preferred from the viewpoint of adaptability in heat dissipation material applications and ease of processing.
[0048] Examples of epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, glycidyl ester epoxy resins, glycidyl amine epoxy resins, biphenyl epoxy resins, naphthalene ring-containing epoxy resins, cyclopentadiene-containing epoxy resins, and polyfunctional epoxy resins. Among these, bisphenol A epoxy resins, bisphenol F epoxy resins, and biphenyl epoxy resins are preferred.
[0049] As the curing agent for curing the epoxy resin, a substance generally used as a curing agent for epoxy resin can be used. Specific examples of the curing agent include thermosetting curing agents such as amines, polyamides, imidazoles, acid anhydrides, boron trifluoride-amine complexes, cyanoguanidine, organic hydrazides, phenol novolac resins, bisphenol novolac resins, and cresol novolac resins, and photocuring agents such as diphenyliodonium hexafluorophosphate and triphenylsulfonium salt hexafluorophosphate.
[0050] Examples of the (meth)acrylic resin include (meth)acrylonitrile, (meth)acrylamide, (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, hydroxyethyl (meth)acrylate, butyl (meth)acrylate, hydroxybutyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl maleate and its salts, 2-(meth)acryloyloxyethyl phthalate, trifluoroethyl (meth)acrylate, perfluorobutylethyl (meth)acrylate, perfluorooctylethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, (meth)acryloyloxyethyl phosphate, and ethylene glycol di(meth)acrylate. Acrylate, propylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, glycerol di(meth)acrylate, tetrafluoroethyl di(meth)acrylate, hexafluoropropyl di(meth)acrylate, octylfluorobutyl di(meth)acrylate, bis[2-(meth)acryloyloxyethyl]phosphate, di(meth)acrylate of ethylene oxide adduct or propylene oxide adduct of bisphenol A, bisphenol A-diepoxy-acrylic acid adduct, tricyclodecane dimethanol diacrylate, polyurethane di(meth)acrylate, pentaerythritol tri(meth)acrylate, etc.
[0051] The acrylic resin can be obtained by polymerizing the corresponding (meth)acrylic acid monomer. As a polymerization initiator for polymerizing and curing the (meth)acrylic acid monomer, a known polymerization initiator such as a thermal polymerization initiator and a photopolymerization initiator can be used. As a thermal polymerization initiator, organic peroxides such as dioctanoyl peroxide, dilauroyl peroxide, tert-butyl peroxide (2-ethylhexanoate), dibenzoyl peroxide, tert-butyl peroxyisobutyrate, tert-butyl peroxylaurate, tert-hexyl peroxybenzoate, and di-tert-butyl peroxide, and azo polymerization initiators such as 2,2-azobisisobutyronitrile and 2,2-azobis-(2,4-dimethylvaleronitrile) can be listed as suitable polymerization initiators. Among them, when the polymerization is carried out at 80°C to 160°C, benzoyl peroxide and tert-butyl peroxide (2-ethylhexanoate) can be used appropriately. These polymerization initiators are usually used in an amount of 0.1 to 20 parts by mass, preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the monomer.
[0052] The resin composition preferably contains the thermally conductive filler of the present invention in a ratio of 20 to 200 parts by volume relative to 100 parts by volume of the resin. In the present invention, the curing agent and polymerization initiator for curing the resin are also included in the resin in the calculation of the blending ratio.
[0053] The resin composition may contain other components in addition to the resin and the thermally conductive filler of the present invention. Examples of other components include inorganic fillers other than the thermally conductive filler of the present invention, anti-discoloration agents, surfactants, dispersants, coupling agents, colorants, plasticizers, viscosity modifiers, antibacterial agents, and the like.
[0054] The aforementioned resin composition is suitable for use as a material for heat dissipation components that effectively dissipate heat generated by semiconductor components mounted on home appliances, automobiles, notebook computers, etc. As their specific examples, heat dissipation grease, heat dissipation gel, heat sink, phase change plate, adhesive, etc. can be cited. In addition to these, the aforementioned resin composition can also be used as an insulating layer, semiconductor sealant, bottom filling glue, housing, or heat sink used in, for example, a metal base substrate, a printed substrate, a flexible substrate, etc. In particular, the thermally conductive filler of the present invention has a high filling property, so the resin composition containing it can take into account both high filling rate and low viscosity, and can be suitably used as a semiconductor resistant sealing material that requires high permeability to narrow gaps, especially a bottom filling sealing material.
[0055] Example
[0056] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples. The raw materials used and the conditions for measuring physical properties are described below.
[0057] [Raw material powder]
[0058] Table 1 shows the raw material powders.
[0059] [Table 1]
[0060] Table 1
[0061] abbreviation Raw material powder Average particle size D50 I Aluminum Nitride 0.9μm II Aluminum Nitride 0.7μm III Alumina 0.5μm IV Alumina 0.2μm V Silicon dioxide 0.3μm VI Silicon dioxide 0.1μm VII Alumina 1.2μm VIII Silicon dioxide 1.0μm
[0062] [Surface treatment agent]
[0063] GPS: 3-glycidoxypropyltrimethoxysilane (Tokyo Chemical Industry, >97%)
[0064] MPS: 3-methacryloxypropyltrimethoxysilane (Tokyo Chemical Industry, >98%)
[0065] ·VMS: Vinyltrimethoxysilane (Tokyo Chemical Industry, >98%)
[0066] ·PMS: Phenyltrimethoxysilane (Tokyo Chemical Industry, >98%)
[0067] PAPS: N-phenyl-3-aminopropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., >95%)
[0068] [Epoxy resin]
[0069] C1: A mixture of epoxy resin YDF-8170c (manufactured by NIPPON STEEL Chemical & Material Co., Ltd.) and amine curing agent KAYAHARD AA (manufactured by Nippon Kayaku Co., Ltd.). The mixing ratio is 4:1 (mass ratio).
[0070] [D50]
[0071] The particle size distribution was measured using a laser diffraction scattering type particle size distribution analyzer for a liquid obtained by dispersing a powder sample in a solvent at a concentration of 0.2 mass % and irradiating the liquid with an ultrasonic wave of about 200 W for 2 minutes. It should be noted that water was used as a solvent for the raw material powder and ethanol was used for the surface treated powder. In the volume frequency distribution of the particle size, the volume frequency was accumulated from the particle with the smallest particle size, and the value of the particle size when the cumulative value reached 50% was taken as D50.
[0072] [Specific surface area]
[0073] The specific surface area was determined by the BET method (nitrogen adsorption single-point method) using a specific surface area measuring device (FlowSorb 2-2300 manufactured by Shimadzu Corporation). 2 g of a powder sample was used for the measurement, which was previously dried at 100° C. for 1 hour by passing nitrogen gas.
[0074] [Amount of coarse particles]
[0075] 10 g of the powder sample is mixed with 200 g of isopropyl alcohol solvent, and then ultrasonic irradiation at about 200 W is performed for 10 minutes to prepare a slurry. A nylon mesh with a mesh size of 5 μm (NYTAL NY5-HC) is prepared, and the mass (m1[g]) is measured. Next, the nylon mesh is installed on a Buchner funnel, and the slurry is filtered through the nylon mesh, and then 200 g of isopropyl alcohol is passed through the nylon mesh to clean it. The nylon mesh is dried at 80°C for 12 hours, and the mass (m2[g]) is measured. The mass increase before and after filtration (m2-m1) is divided by the amount of powder (10 g) provided for the slurry production, and the amount of coarse particles (mass %) above 5 μm is calculated as shown in formula (1).
[0076] Coarse particle amount [%] = (m2-m1) × 100 / 10 (1)
[0077] [Hydrophobicity]
[0078] In a 200cc beaker, 100cc of methanol aqueous solution was prepared at a concentration of 1% by volume, 1g of surface treated powder was added to each aqueous solution, and the solution in the beaker was stirred for 5 minutes with a magnetic stirrer. The volume percentage of methanol at which 50% of the surface treated powder was suspended in the solution was taken as the hydrophobicity.
[0079] [Surface treatment]
[0080] 600 g of the raw material powder shown in Table 2, a predetermined amount of the surface treatment agent, and 1200 g of isopropyl alcohol were placed in a glass eggplant-shaped flask and stirred for 30 minutes with a fluororesin stirring blade. After isopropyl alcohol was removed by a rotary evaporator at 50°C under reduced pressure, the mixture was dried under reduced pressure at 100°C to obtain a surface-treated powder. The raw materials and physical properties of each surface-treated powder are shown in Table 2.
[0081] [Table 2]
[0082] Table 2
[0083]
[0084] [Examples 1 to 42 and Comparative Examples 1 to 10]
[0085] [Thermal conductive filler]
[0086] Predetermined amounts of each surface-treated powder were weighed and mixed thoroughly to prepare a thermally conductive filler. The content and physical properties of each surface-treated powder are shown in Tables 3 and 4. The content of the powder in the table is the ratio of the powder when the total thermally conductive filler is 100 vol.%.
[0087] [Table 3]
[0088] Table 3
[0089]
[0090] [Table 4]
[0091] Table 4
[0092]
[0093] [Examples 43 to 84 and Comparative Examples 11 to 20]
[0094] [Resin composition]
[0095] 0.12 g of epoxy resin YDF-8170c (manufactured by NIPPON STEEL Chemical & Material Co., Ltd.), 0.03 g of curing agent KAYAHARD AA (manufactured by Nippon Kayaku Co., Ltd.), and a predetermined amount of thermally conductive filler were weighed and kneaded in a mortar by applying a strong shear force for 15 minutes. The obtained kneaded product was further kneaded for 20 minutes using a three-roll kneader to obtain a resin composition. The composition and evaluation results of the resin composition are shown in Tables 5 and 6.
[0096] [Table 5]
[0097] Table 5
[0098]
[0099] [Table 6]
[0100] Table 6
[0101]
[0102] <Evaluation of performance of resin composition>
[0103] Viscosity
[0104] The obtained resin composition was measured by cone-plate viscometer (RVDV-II manufactured by Brookfield, with a probe of Angle 2 degrees), measured at 30 ° C. For shear rate 2s- 1 The viscosity at the time of was evaluated and was rated as ◎ to × based on the following criteria.
[0105] ◎: Less than 50000mPa·s
[0106] ○: 50000 mPa·s or more and less than 100000 mPa·s
[0107] △: 100000mPa·s or more and less than 200000mPa·s
[0108] ×: 200000 mPa·s or more
[0109] Gap permeability
[0110] Use a new polished glass slide and a 30μm thick double-sided tape (manufactured by Nitto Denko) to form a gap of 30μm and 1cm wide (as fixture A). Place fixture A on a hot plate at 110°C and keep it for more than 10 minutes, then drip the aforementioned resin composition at the end of the gap. After dripping, observe that the resin composition penetrates into the gap, and measure the time when the penetration distance of the resin composition reaches 1cm. According to the penetration time, it is set as ◎~× as follows.
[0111] ◎: Less than 60 seconds
[0112] ○: 60 seconds or more and less than 180 seconds △: 180 seconds or more
[0113] ×: Not penetrated to 1 cm.
Claims
1. A thermally conductive filler comprising a first surface-treated powder and a second surface-treated powder having a hydrophobization degree different from that of the first surface-treated powder.
2. The thermally conductive filler according to claim 1, wherein The difference between the hydrophobization degree of the first surface-treated powder and the hydrophobization degree of the second surface-treated powder is 2 or more.
3. The thermally conductive filler according to claim 1, wherein The first surface-treated powder is at least one surface-treated powder selected from the group consisting of aluminum oxide, aluminum nitride, boron nitride, magnesium oxide, zinc oxide, silicon carbide, silicon nitride, and diamond, and the content of the second surface-treated powder is 2 parts by volume to 100 parts by volume relative to 100 parts by volume of the first surface-treated powder.
4. The thermally conductive filler according to claim 1, wherein The second surface-treated powder is at least one surface-treated powder selected from the group consisting of silicon dioxide, aluminum oxide, aluminum nitride, boron nitride, magnesium oxide, zinc oxide, silicon carbide, silicon nitride, and diamond.
5. The thermally conductive filler according to claim 1, wherein The first surface-treated powder is aluminum nitride surface-treated powder.
6. The thermally conductive filler according to claim 1, wherein In the particle size distribution measured by a laser diffraction scattering type particle size distribution analyzer using an ethanol solvent, the cumulative volume 50% particle diameter D50 was 0.1 to 2.0 μm, and coarse particles of 5 μm or more accounted for less than 3% by mass. 7 . A heat dissipation material resin composition comprising a resin and the thermally conductive filler according to claim 1 .
Citation Information
Patent Citations
Preparation method of silicon rubber material and electronic product
CN109401322A
Epoxy resin composition and semiconductor device
JP2003213095A
Composition for heat-dissipation members, heat-dissipation member, electronic device, and heat-dissipation-member production method
US20170306207A1
Curable particulate silicone composition, semiconductor member comprising curable particulate silicone composition, and method for molding semiconductor member
US20190177488A1