Film forming method, film forming apparatus, and laminate

By configuring a channel plate and controlling the temperature in the film-forming device, the problems of uneven film formation and foreign matter adhesion on large-diameter substrates were solved, and the stable manufacturing of high-quality films was achieved.

CN119032418APending Publication Date: 2024-11-26SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034925.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-25
Filing Date
2023-04-12
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing film-forming devices struggle to achieve uniform film thickness on large-diameter substrates, and temperature variations in the raw material mist lead to foreign matter adhesion and film quality degradation.

Method used

By configuring channel plates on the substrate with a space between them, controlling the temperature of the mixed gas supply element and the channel plates, a straight-flowing mixed gas flow is formed. Combined with the temperature control of the exhaust element, the deterioration of the raw material mist and the generation of powder are suppressed.

Benefits of technology

This technology enables the stable fabrication of high-quality membranes on large-diameter substrates, improving productivity and membrane quality while reducing foreign matter density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032418A_ABST
    Figure CN119032418A_ABST
Patent Text Reader

Abstract

The present invention is a film forming method comprising: a step for forming a raw material mist by atomizing a raw material solution; mixing the raw material mist with a carrier gas to form a mixed gas; a step in which the substrate is placed on a stage; a film formation step in which the mixed gas is supplied from a mixed gas supply element to the substrate, and a film is formed on the substrate by a thermal reaction; and an exhaust step for exhausting the gas mixture after film formation by means of an exhaust element, characterized in that a channel plate is disposed on the substrate so as to face the substrate with a space therebetween, and the channel plate is disposed on the substrate so as to face the substrate with the gas mixture along at least a part of the main surface of the substrate in the space on the substrate. In the film forming step and the exhausting step, at least the temperature T1 of the mixed gas supply element and the temperature T2 of the channel plate are controlled, and a mixed gas flow that flows linearly from the mixed gas supply element to the exhausting element is formed. As a result, provided are a film forming method and a film forming apparatus with which it is possible to stably produce a high-quality film on the surface of a large-diameter substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a film forming method and a film forming device. Background Art

[0002] As a method capable of forming an epitaxial film at low temperature and atmospheric pressure, a film forming method using water particles such as an atomized CVD method is known. Patent document 1 shows a film forming device that forms a film by supplying a raw material mist to a substrate from a nozzle arranged obliquely relative to the substrate. In addition, patent document 2 describes a film forming method that uses a carrier gas to transport a raw material mist into a reaction container, thereby generating a vortex flow to cause the mist to react with the substrate.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-142637

[0006] Patent Document 2: Japanese Patent Application Publication No. 2016-146442 Summary of the invention

[0007] 1. Technical issues to be resolved

[0008] However, in these existing film forming devices, it is impossible to fully control the raw material mist on the substrate, resulting in difficulty in forming a film of uniform thickness on a large diameter substrate of practical size. In addition, by continuously heating the nozzle or the film forming chamber, the temperature of the mist changes, so the mist evaporates and the powder adheres to the surface of the substrate, or abnormal growth grains are formed in the case of crystal growth. These foreign matter not only have an adverse effect on the characteristics of semiconductor devices, for example, but also become a stress source when the film is grown in a manner that covers the above-mentioned foreign matter, causing cracks in the film over a wide range, resulting in problems such as reduced film quality and yield.

[0009] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a film forming method and a film forming apparatus capable of stably producing a high-quality film on the surface of a large-diameter substrate.

[0010] (II) Technical solution

[0011] In order to solve the above problems, the present invention provides a film forming method, comprising:

[0012] A step of atomizing the raw material solution to form raw material mist;

[0013] The step of mixing the raw material mist with a carrier gas to form a mixed gas;

[0014] The step of placing a substrate on a stage;

[0015] a film forming step of supplying the mixed gas from a mixed gas supplying means to the substrate and forming a film on the substrate by a thermal reaction; and

[0016] an exhaust step of exhausting the mixed gas after film formation by using an exhaust element,

[0017] A channel plate is disposed on the substrate so as to face the substrate with a space therebetween.

[0018] In the space on the substrate, a mixed gas flow is formed so as to flow linearly from the mixed gas supply element toward the exhaust element in a manner such that the mixed gas flows along at least a portion of the main surface of the substrate,

[0019] In the film forming step and the exhaust step, at least the temperature T1 of the mixed gas supplying element and the temperature T2 of the channel plate are controlled.

[0020] Such a film forming method suppresses the deterioration of raw material mist and the generation of powder, thereby suppressing the formation of defects and maintaining a good raw material yield, thereby becoming a film forming method that can stably produce a high-quality film on a large-diameter substrate surface.

[0021] At this time, the temperature T3 of the exhaust element may be further controlled.

[0022] According to such a film forming method, the mixed gas can be discharged more efficiently, and it becomes a film forming method capable of more stably manufacturing a high-quality film.

[0023] In addition, the present invention provides a film forming method, comprising:

[0024] A step of atomizing the raw material solution to form raw material mist;

[0025] The step of mixing the raw material mist with a carrier gas to form a mixed gas;

[0026] The step of placing a substrate on a stage;

[0027] a film forming step of supplying the mixed gas from a mixed gas supplying means to the substrate and forming a film on the substrate by a thermal reaction; and

[0028] an exhaust step of exhausting the mixed gas after film formation by using an exhaust element,

[0029] A channel plate is disposed on the substrate so as to face the substrate with a space therebetween.

[0030] In the space on the substrate, a mixed gas flow is formed so as to flow linearly from the mixed gas supply element toward the exhaust element in a manner such that the mixed gas flows along at least a portion of the main surface of the substrate,

[0031] In the film forming step and the exhaust step, at least the temperature T2 of the channel plate is controlled.

[0032] Such a film forming method suppresses the deterioration of raw material mist and the generation of powder, thereby suppressing the formation of defects and maintaining a good raw material yield, thereby becoming a film forming method that can stably produce a high-quality film on a large-diameter substrate surface.

[0033] At this time, the temperature T3 of the exhaust element may be further controlled.

[0034] According to such a film forming method, the mixed gas can be discharged more efficiently, and it becomes a film forming method capable of more stably manufacturing a high-quality film.

[0035] In addition, the present invention provides a film forming device comprising:

[0036] an atomizing element, which atomizes the raw material solution to form a raw material mist;

[0037] a carrier gas supply element for conveying the raw material mist;

[0038] A mixed gas supply element supplies a mixed gas formed by mixing the raw material mist and a carrier gas to the surface of the substrate;

[0039] a table on which the substrate is placed;

[0040] an exhaust element for exhausting the mixed gas;

[0041] a channel plate disposed on the base body so as to face the base body with a space therebetween; and

[0042] A temperature control element controls at least the temperature T1 of the mixed gas supply element and the temperature T2 of the channel plate.

[0043] Such a film forming apparatus can suppress the deterioration of raw material mist and the generation of powder, thereby suppressing the formation of defects and maintaining a good raw material yield, thereby becoming a film forming apparatus that can stably produce high-quality films on the surface of a large-diameter substrate.

[0044] In this case, the film forming apparatus further includes a temperature control element for controlling the temperature T3 of the exhaust element.

[0045] With such a film forming apparatus, the mixed gas can be discharged more efficiently, and a high-quality film can be produced more stably.

[0046] In addition, the present invention provides a laminate comprising:

[0047] a crystalline substrate; and

[0048] a crystalline film formed by epitaxial growth on the crystalline substrate,

[0049] The density of foreign matter with a diameter of 0.3 μm or more on the surface of the crystal film is 1 cm -2 the following.

[0050] Such a laminated body has a high-quality film on the surface of a large-diameter substrate.

[0051] At this time, the film thickness of the crystal film is preferably 0.3 μm or more.

[0052] The laminate of the present invention is more preferably such a laminate.

[0053] (III) Beneficial effects

[0054] According to the present invention, a highly productive film-forming method and a film-forming apparatus are provided, which can stably produce a high-quality film on the surface of a large-diameter substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 This is a diagram showing one embodiment of the film forming apparatus of the present invention.

[0056] Figure 2 This is a diagram showing one embodiment of the film forming portion of the present invention.

[0057] Figure 3 It is a figure which shows another form of the film forming part of this invention. DETAILED DESCRIPTION

[0058] As described above, it is desired to develop a film forming method and a film forming apparatus capable of stably producing a high-quality film on the surface of a large-diameter substrate.

[0059] The inventors of the present invention have conducted intensive research on the above-mentioned technical problem and have found that by configuring a channel plate on a substrate so as to be opposite to the substrate with a space therebetween, and controlling the temperature T1 of the mixed gas supply element and the temperature T2 of the channel plate, a high-quality membrane can be stably manufactured on the surface of a large-diameter substrate, thereby completing the present invention.

[0060] That is, the present invention is a film forming method comprising:

[0061] A step of atomizing the raw material solution to form raw material mist;

[0062] The step of mixing the raw material mist with a carrier gas to form a mixed gas;

[0063] The step of placing a substrate on a stage;

[0064] a film forming step of supplying the mixed gas from a mixed gas supplying means to the substrate and forming a film on the substrate by a thermal reaction; and

[0065] an exhaust step of exhausting the mixed gas after film formation by using an exhaust element,

[0066] A channel plate is disposed on the substrate so as to face the substrate with a space therebetween.

[0067] In the space on the substrate, a mixed gas flow is formed so as to flow linearly from the mixed gas supply element toward the exhaust element in a manner such that the mixed gas flows along at least a portion of the main surface of the substrate,

[0068] In the film forming step and the exhaust step, at least the temperature T1 of the mixed gas supplying element and the temperature T2 of the channel plate are controlled.

[0069] In addition, the present invention provides a film forming device comprising:

[0070] an atomizing element, which atomizes the raw material solution to form a raw material mist;

[0071] a carrier gas supply element for conveying the raw material mist;

[0072] A mixed gas supply element supplies a mixed gas formed by mixing the raw material mist and a carrier gas to the surface of the substrate;

[0073] a table on which the substrate is placed;

[0074] an exhaust element for exhausting the mixed gas;

[0075] a channel plate disposed on the base body so as to face the base body with a space therebetween; and

[0076] A temperature control element controls at least the temperature T1 of the mixed gas supply element and the temperature T2 of the channel plate.

[0077] Hereinafter, the present invention will be described in detail with reference to the drawings, but the present invention is not limited thereto.

[0078] [Film forming device]

[0079] First, an example of a film forming apparatus that can be used in the film forming method of the present invention will be described.

[0080] Figure 1The following are representative examples of film forming apparatuses that can be used in the film forming method of the present invention. However, the film forming apparatuses that can be used in the film forming method of the present invention are not limited to Figure 1 The film forming device shown.

[0081] Figure 1 The film forming apparatus 1 shown in the figure includes a carrier gas 11, a carrier gas pipe 12, an atomizing element 20, a mist pipe 24, a mixed gas supply element 35, a stage 32, a channel plate 31, and an exhaust element 36. A substrate 34 to be formed with a film is placed on the stage 32. In addition, the mixed gas supply element 35 and the channel plate 31 include temperature adjustment parts 35b and 31b, and the temperature adjustment parts 35b and 31b are connected to a temperature control part 37 via a connection part 38 to form a temperature control element. The carrier gas 11 and the carrier gas pipe 12 constitute a carrier gas supply element 10. In addition, the mixed gas supply element 35, the stage 32, the channel plate 31, the exhaust element 36, the temperature control part 37 and the connection part 38 constitute a film forming part 30. In addition, 35a is an exhaust port, and 36a is an exhaust port.

[0082] A raw material solution 21 is contained as a raw material in the atomizing element 20. The raw material solution 21 is not particularly limited, as long as it is a solution that can be atomized (also called "mist"), and an aqueous solution containing a raw material that meets the purpose, an organic solvent solution such as alcohols, ketones, esters, ethers, amides, halogenated solvents, aromatic compounds, etc. can be used.

[0083] The raw material solution 21 is atomized using a known element to form a raw material mist 22 .

[0084] The carrier gas 11 is further supplied to the atomizing element 20, and is mixed with the raw material mist 22 to form a mixed gas 23. It can also be said that the carrier gas supply element 10 and the atomizing element 20 constitute a mechanism 40 for forming the mixed gas 23.

[0085] The base body 34 may be placed on the stage 32 and the base body 34 may be heated to a temperature suitable for film formation by a heating element (not shown).

[0086] The mixed gas 23 is conveyed by the mist pipe 24 and supplied to the mixed gas supply unit 35 .

[0087] The mixed gas 33 is supplied from the mixed gas supply element 35 to the space 39 formed between the channel plate 31 and the stage 32, and is supplied to the substrate 34 mounted on the stage 32, particularly the surface of the substrate 34, while flowing in parallel with the substrate mounting surface of the stage 32. In this process, the mixed gas 33 reacts on the substrate 34, and a film is formed on the substrate 34.

[0088] During this period, the mixed gas supply element 35 and the channel plate 31 are controlled by the temperature control unit 37 to a temperature suitable for film formation.

[0089] The remaining components of the mixed gas 33 that do not contribute to the film formation and the by-products generated when the mixed gas 33 reacts on the substrate 34 are sucked into the exhaust element 36 as the mixed gas after film formation and discharged to the outside of the system. The exhaust gas from the exhaust element 36 can be processed by a particle collector, a scrubber, etc., which are not shown in the figure, as needed.

[0090] The atomization of the raw material solution 21 is not particularly limited, as long as the raw material solution 21 can be atomized or dropletized, it can be a known element, and in the present invention, it is preferably an atomizing element 20 using ultrasonic waves. The initial velocity of the mist or droplets obtained using ultrasonic waves is zero and floats in the air, so it is preferred. For example, it is not sprayed like a sprayer, but the mist floats in the space and can be transported as a gas, so there is no damage caused by the collision energy, so it is very preferred. The droplet size is not particularly limited, and it can be a droplet of about several mm, preferably less than 50 μm, and more preferably 0.1~10 μm.

[0091] The carrier gas 11 is not particularly limited. For example, in addition to air, oxygen, and ozone, an inert gas such as nitrogen and argon, or a reducing gas such as hydrogen and forming gas (Japanese: フォーミングガス) can be used appropriately. The type of the carrier gas 11 can be one, or two or more. The flow rate of the carrier gas can be appropriately set according to the size of the substrate and the size of the film forming part, for example, it can be set to about 0.01 to 100 L / min.

[0092] In addition, although not shown, a dilution gas may be further added to adjust the ratio of the raw material mist 22 to the carrier gas 11. The flow rate of the dilution gas may be appropriately set, for example, it may be set to 0.1 to 10 times that of the carrier gas. The dilution gas may be supplied, for example, to the downstream side of the atomizing element 20. The dilution gas may be the same gas as the carrier gas 11, or a different gas may be used.

[0093] The film formation may be performed under any of atmospheric pressure, increased pressure, and reduced pressure. However, it is preferably performed under atmospheric pressure from the viewpoint of equipment cost and productivity.

[0094] In addition, Figure 1 The method of using one atomizing element 20 is shown in the figure, but the film forming device 1 that can be used in the film forming method of the present invention is not limited to this, and multiple atomizing elements 20 can also be connected in series or in parallel for use. In this case, different raw material solutions can be placed in each atomizing element 20 for use, or the same raw material solution can be placed in each atomizing element 20 for use. In addition, each raw material solution can be atomized separately and supplied to the mixed gas supply element 35 independently, or it can be supplied to the mixed gas supply element 35 after mixing multiple raw material mists.

[0095] The mist pipe 24 is not particularly limited as long as it has sufficient stability in terms of the temperature of the raw material solution 21, the mixed gas supply element 35 and the carrier gas pipe 12 used. It can be made of resin, metal, glass or a combination of these materials according to the purpose.

[0096] The form and supply method of the mixed gas supply element 35 are not particularly limited, and a widely known mixed gas supply element can be widely used. In addition, the shape of the discharge port 35a is not particularly limited, and can include a single or multiple circular, elliptical, or polygonal shapes. In order to make the flow of the mixed gas 33 more uniform laminar flow, for example, a single or multiple slits with a ratio of the short axis length to the long axis length of about 10 times or more can be used. In this case, the length of the discharge port 35a in the longitudinal direction can be set to a sufficient length to match the shape of the substrate 34.

[0097] The mixed gas supply element 35 is not particularly limited as long as it has sufficient stability with respect to the raw material solution 21 used and the operating temperature, and can be made of resin, metal, glass, ceramic, or a combination thereof according to the purpose.

[0098] The shape of the channel plate 31 is not particularly limited, and in order to set the flow of the mixed gas 33 to a more uniform laminar flow, it can be set to a flat plate. At this time, the length of the direction parallel to the long side direction of the slit-shaped discharge port 35a can be set to a sufficient length to match the shape of the substrate, preferably set to be greater than the length of the long side direction of the discharge port 35a. In addition, the length of the flow direction of the mixed gas 33 (referred to as the channel length) can be appropriately set according to various film forming conditions including the physical properties of the raw material solution 21. For example, when the raw material mist 22 is easy to evaporate, that is, the mist life is short, by setting the channel length shorter, the adhesion of the powder body can be more effectively prevented. In addition, when the mist life is long, the raw material yield can be increased by setting the channel length longer.

[0099] The channel plate 31 is not particularly limited as long as it has sufficient stability to the raw material solution 21 used and the operating temperature, and can be made of resin, metal, glass, ceramic, or a combination thereof according to the purpose.

[0100] The form of the exhaust element 36 is not particularly limited, and a widely known exhaust element can be applied. The exhaust port 36a preferably has an opening with a length equal to or longer than the length of the channel plate 31 perpendicular to the gas flow direction. Thus, the flow of the mixed gas 33 can be maintained more effectively. In addition, the exhaust element 36 is not particularly limited, as long as it has sufficient stability with respect to the raw material solution 21 used and the use temperature, and can be made of resin, metal, glass, or a combination thereof according to the purpose.

[0101] The exhaust volume of the exhaust element 36 can be appropriately adjusted according to the film forming conditions. In order to maintain the laminar flow of the mixed gas 33, it is preferably set to about 70 to 250% relative to the flow rate of the mixed gas 33, and more preferably to about 80 to 200%. In addition, when the exhaust volume relative to the flow rate of the mixed gas 33 is small, the mixed gas 33 is directly discharged to the exhaust element side. In this case, for example, it can be discharged to the outside of the device through a shell exhaust member, which is provided in a shell including the film forming section 30 not shown in the figure. In addition, when the exhaust volume relative to the flow rate of the mixed gas 33 is large, the atmosphere of the phase difference flows in from the mixed gas supply element 35 side together with the mixed gas 33, so that the flow of the mixed gas 33 flowing in the space 39 can be maintained without turbulence in any case.

[0102] The mixed gas supply element 35 and the channel plate 31 include temperature adjustment parts 35b and 31b, and the temperature adjustment parts 35b and 31b are connected to the temperature control part 37. The temperature T1 of the mixed gas supply element 35 and the temperature T2 of the channel plate 31 are controlled to predetermined temperatures by the temperature control part 37 via the temperature adjustment parts 35b and 31b.

[0103] The measurement of the temperatures T1 and T2 is not particularly limited, and they can be set as the measured values ​​of the outer surface, respectively. The temperature T2 of the channel plate 31 is preferably set as the temperature of the contact surface with the mixed gas 33. For example, when the film formation is accompanied by heating of the substrate 34, it is preferably performed at the mixed gas supply element 35 and the channel plate at a location close to the heat source of the heating element. This measurement can be performed by a known temperature measurement method, and can be measured by a thermocouple or a radiation thermometer.

[0104] (Temperature conditions)

[0105] Temperatures T1 and T2 are appropriately set and controlled based on various conditions such as the temperature and physical properties (mainly vapor pressure) of the raw material solution 21 or the solvent used in the raw material solution 21, the supply amount of the mixed gas 33, the mist concentration in the mixed gas 33, and the flow rate between the channel plate 31 and the substrate 34. For example, under normal conditions when water is used as the solvent, it can be set to 35°C to 150°C.

[0106] That is, the setting range of the appropriate temperature T1 and T2 is mainly related to the heat received by the mixed gas 33 after being introduced into the mixed gas supply element 35. For example, if the heat in the system from the mixed gas supply element 35 to the exhaust element 36 is too small relative to the mist concentration and temperature of the mixed gas 33, the raw material mist 22 in the system will condense and no normal film formation will be performed, and the condensation will fall on the substrate and form defects. On the contrary, if the heat in the system is too much, the solvent of the raw material solution 21 will evaporate excessively, so that most of the raw material will become powder and be consumed, not only the growth rate of the film will be reduced, but also the powder will adhere to the film, and defects will be introduced into the film, resulting in a decrease in film quality. In addition, depending on the situation, the solid content concentration in the mist increases with the increase in the mist temperature, and some unpreferred chemical reactions are carried out, which sometimes causes abnormalities in the target film formation. For example, in the case of epitaxial growth of α-phase gallium oxide on a sapphire substrate, if the temperature of the mist as described above rises excessively, abnormal growth particles will be formed and crystal phase transformation will occur.

[0107] The abnormal growth particles at this time are mainly amorphous or crystalline fine particles grown on the precipitates from the solid components of the mist, and most of the diameters range from ultrafine to about 1 μm. In addition, the crystal phase transition here has the same composition as the growth film, but exhibits other polymorphs, specifically, each phase including β, γ, ε, and δ. These crystal phase transitions vary in shape and size depending on the crystal phase, and are usually mostly produced in the form of islands of 1 to 5 μm. Each of these abnormal growth particles itself becomes a source of dislocation, causing the quality of the film to deteriorate. In addition, if the film growth proceeds and these foreign objects enter the film, stress is generated between the growth film and cracks are generated on the film, causing a significant reduction in the quality of the film.

[0108] In addition, these foreign substances can be detected by known methods such as optical microscopy and light scattering.

[0109] (Control Method)

[0110] The temperature control unit 37 measures the temperatures T1 and T2, or the temperature T1' of the temperature adjustment unit 35b and the temperature T2' of the temperature adjustment unit 31b, and controls the temperatures T1 and T2 directly or indirectly through the temperature adjustment units 35b and 31b in such a manner as to eliminate the deviation between the measured values ​​and the set values ​​(reference values) of the temperatures T1 and T2. For the control of the temperatures T1 and T2 using the temperatures T1' and T2', for example, the correlation between the temperatures T1 and T2 under the predetermined film forming conditions and the temperatures T1' and T2' at that time can be measured in advance.

[0111] The method for calculating the deviation is not particularly limited, and a known method can be used. In addition, the method of temperature control is not particularly limited, and a known method such as on / off control, PID control, and cascade control can be used.

[0112] The structure of the stage 32 is not particularly limited as long as it has sufficient stability according to the characteristics of the raw materials used and the temperature conditions. In this case, metals such as aluminum and stainless steel can be used. When the film is formed at a higher temperature than the heat-resistant temperature of these metals or when an acidic or alkaline raw material is used, alloys such as Hastelloy, soda-lime glass, borosilicate glass, quartz, silicon carbide, or ceramics such as silicon nitride and aluminum nitride can also be used.

[0113] Although not shown, the film forming unit 30 may further include a known heating element such as a resistance heating heater or a lamp heater in order to heat the substrate 34. In this case, the heater may be built into the stage 32, or may be provided outside the stage 32. In addition, the stage 32 may include a mechanism for holding the substrate 34. In this case, a known substrate holding method such as a vacuum chuck, a mechanical chuck, or an electrostatic chuck may be applied.

[0114] The substrate 34 is not particularly limited as long as it can support the formed film. The material of the substrate 34 is also not particularly limited, and it can be a known material, an organic compound, an inorganic monomer or an inorganic compound. For example, polysulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, polyimide, polyetherimide, fluororesin, iron, aluminum, stainless steel, gold and other metals, silicon, sapphire, quartz, glass, calcium carbonate, lithium tantalate, lithium niobate, gallium oxide, SiC, ZnO, GaN, etc., but not limited to these materials. As the shape of the substrate, for example, there are: flat plates, circular plates and other plates, fibers, rods, cylinders, angular columns, tubes, spirals, spheres, rings, etc., especially when the substrate is a plate-like body, it is not particularly limited in the present invention, and an area of ​​5cm can be appropriately used. 2 More than 10 cm 2 The substrate has a thickness of 50 to 2000 μm, more preferably 100 to 800 μm.

[0115] In addition, in the film forming method of the present invention, the film formation may be performed while the substrate 34 and the channel plate 31 are opposed to each other and maintained stationary at a predetermined position, or a moving element (not shown) or a rotating element (not shown) that can change the relative position with respect to the substrate 34 in the horizontal direction may be provided. By providing the moving element and the rotating element, the thickness distribution of the formed film can be improved, and the film formation can be performed on a substrate with a large diameter or a long substrate.

[0116] The moving element can be a mechanism that moves back and forth in a horizontal axial direction. For example, the moving speed when moving in a direction parallel to the direction of the mist flow can be appropriately adjusted according to the purpose, and can be set to 0.1mm / s to 100mm / s, and more preferably can be set to 1mm / s to 30mm / s. If it is above 1mm / s, it is possible to prevent film formation from becoming reaction rate control, achieve full benefits of raw materials, and reduce the chance of abnormal reactions. If it is below 100mm / s, the mixed gas 33 can fully follow the moving motion, and an excellent film thickness distribution can be achieved. In addition, the rotation speed during rotation is not particularly limited, as long as it is within the range that does not generate turbulence of the mixed gas 33, and it can usually be carried out at 1° to 18° per second.

[0117] in addition, Figure 1 In the embodiment, the channel plate 31 is arranged above the table 32, and the film forming surface of the substrate 34 is facing upward to form the film, but the film forming device used in the film forming method of the present invention is not limited to this. The channel plate 31 can also be arranged below the table 32, and the film forming surface of the substrate 34 is facing downward to form the film.

[0118] Figure 1 1 shows an example of a method for controlling the temperature of the mixed gas supply element 35 and the channel plate 31, but the present invention is not limited thereto, and a method may be further provided in the exhaust element 36 to control the temperature T3 of the exhaust element 36 by connecting to the temperature control unit 37. In this case, the temperature T3 can be controlled in the same manner as in the case of the above-mentioned temperatures T1 and T2. In addition, the temperature T3 is appropriately set and controlled according to various conditions such as the temperature and physical properties (mainly vapor pressure) of the raw material solution 21 or the solvent used in the raw material solution 21, the supply amount of the mixed gas 33, the mist concentration in the mixed gas 33, and the flow rate between the channel plate 31 and the substrate 34. For example, under normal conditions when water is used as the solvent, it can be set to 35° C. to 150° C. If the temperature T3 is above a certain temperature, the raw material mist 22 will not condense in the exhaust element 36 and will not fall on the substrate 34 to form a defect. In addition, if the temperature T3 is below a certain temperature, the solid components of the raw material mist 22 will not precipitate in the exhaust element 36, so that the exhaust port will not be blocked and normal film formation can be performed, and the precipitates will not fall on the substrate 34 and form defects. By controlling the temperature T3 in this way, the mixed gas can be discharged more effectively, so that high-quality films can be manufactured more stably.

[0119] Next, use Figure 2 and Figure 3 The embodiment of the film forming unit 30 of the present invention will be described in more detail.

[0120] exist Figure 2In the film forming unit 30 shown, the channel plate 31 is arranged parallel to the stage 32, and the mixed gas supply element 35 and the exhaust element 36 are arranged with the mist outlet 35a of the mixed gas supply element 35 facing the exhaust outlet 36a of the exhaust element 36 across the channel plate 31. The mixed gas supply element 35, the channel plate 31 and the exhaust element 36 are respectively provided with temperature adjustment parts 35b, 31b and 36b, and are connected in series with the temperature control part 37 via the connection part 38. In addition, 33 is the mixed gas and 34 is the substrate.

[0121] The arrangement and form of the temperature adjustment parts 35b, 31b, and 36b can be appropriately adjusted according to the shapes and forms of the mixed gas supply element 35, the channel plate 31, and the exhaust element 36. In addition, the temperature adjustment parts 35b, 31b, and 36b can also use liquid or gas heat media for heat exchange, or can be elements that apply the Peltier effect. As the heat medium, well-known heat media can be widely used, such as liquid heat media such as water, glycols, alcohols, and silicone oils; and gas heat media such as air, helium, or fluorocarbons. The connection part 38 can be set as an electrical wiring or a pipe suitable for the heat medium according to the form of the temperature adjustment parts 35b, 31b, and 36b.

[0122] In addition, the distance h between the channel plate 31 and the main surface of the substrate 34 can be appropriately adjusted according to the supply amount of the mixed gas 33, and is generally set to be greater than 1 mm and less than 40 mm. If it is greater than 1 mm, there is a tendency for the film thickness distribution to become smaller, and if it is less than 40 mm, the supply amount of the mixed gas to the substrate 34 increases, the productivity is improved, the raw material profit increases, and the cost is reduced.

[0123] Figure 2 In the embodiment, the temperature adjustment parts 35b, 31b, 36b are connected in series with the temperature control part 37, but the present invention is not limited thereto. Figure 3 The following method is shown: temperature control parts 371, 372, 373 are provided for the mixed gas supply element 35, the channel plate 31, and the exhaust element 36, respectively, and the temperature adjustment parts 35b, 31b, 36b are adjusted separately. In addition, 32 is a stage, 34 is a base, and 381, 382, ​​383 are connecting parts.

[0124] in addition, Figure 1 , 2 In the example shown in FIG. 3 , a device is shown in which the mixed gas supply element 35, the channel plate 31, and the exhaust element 36 are separately configured, but the present invention is not limited to this. The mixed gas supply element 35, the channel plate 31, and the exhaust element 36 may be partially or entirely constructed as an integral unit.

[0125] In the laminate of the present invention, the density of foreign matter with a diameter of 0.3 μm or more on the surface of the crystal film is 1 cm-2 The lower limit is not particularly limited, and can be set to 0.1 cm, for example. -2 above.

[0126] The film thickness of the crystal film is preferably 0.3 μm or more, and the upper limit thereof is not particularly limited, but can be, for example, 100 μm or less.

[0127] [Film Forming Method]

[0128] The present invention provides a film forming method, comprising:

[0129] A step of atomizing the raw material solution to form raw material mist;

[0130] The step of mixing the raw material mist with a carrier gas to form a mixed gas;

[0131] The step of placing a substrate on a stage;

[0132] a film forming step of supplying the mixed gas from a mixed gas supplying means to the substrate and forming a film on the substrate by a thermal reaction; and

[0133] an exhaust step of exhausting the mixed gas after film formation by using an exhaust element,

[0134] A channel plate is disposed on the substrate so as to face the substrate with a space therebetween.

[0135] In the space on the substrate, a mixed gas flow is formed so as to flow linearly from the mixed gas supply element toward the exhaust element in a manner such that the mixed gas flows along at least a portion of the main surface of the substrate,

[0136] In the film forming step and the exhaust step, at least the temperature T1 of the mixed gas supplying element and the temperature T2 of the channel plate are controlled.

[0137] Such a film forming method suppresses the deterioration of raw material mist and the generation of powder, thereby suppressing the formation of defects and maintaining a good raw material yield, thereby becoming a film forming method that can stably produce a high-quality film on a large-diameter substrate surface.

[0138] In addition, the temperature T3 of the exhaust element can be controlled. According to such a film forming method, the mixed gas can be exhausted more efficiently, and it becomes a film forming method capable of more stably manufacturing a high-quality film.

[0139] Example

[0140] Hereinafter, the present invention will be specifically described using Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0141] (Example 1)

[0142] In Figure 1 the film forming apparatus, the film forming section of Figure 3 was used to form an α-gallium oxide film.

[0143] As the raw material solution, gallium acetylacetonate was dissolved in a dilute hydrochloric acid aqueous solution in which 34% hydrochloric acid was added at a volume ratio of 1% at a ratio of 0.02 mol / L, and it was filled into an atomizing device (atomizing element).

[0144] Next, ultrasonic vibration was transmitted through water to the raw material solution in the atomizing device by an ultrasonic vibration plate to atomize the raw material solution (mist atomization).

[0145] Next, a c-plane single crystal sapphire wafer with a thickness of 0.35 mm and a diameter of 4 inches (about 10 cm) was placed on a stage and heated to a substrate temperature of 450°C.

[0146] In addition, for the mixed gas supply element and the exhaust element, aluminum nozzles with anodized aluminum treatment on the surface were used, and for the channel plate, aluminum plates with anodized aluminum treatment on the surface were also used. In the temperature adjustment parts of these nozzles and channel plates, water was circulated as a heat medium in a cooler to keep the temperature of the bottom surface of each component at 60°C.

[0147] For the carrier gas supply, a gas cylinder filled with nitrogen was used. The gas cylinder and the atomizing device were connected by a polyurethane resin tube, and further, the atomizing device and the nozzle unit were connected by a quartz tube.

[0148] Next, nitrogen was added to the raw material container at a flow rate of 20 L / min, a mixed gas of mist and nitrogen was supplied to the nozzle unit, and exhaust was performed at an exhaust flow rate of 25 L / min. Further, during this period, while keeping the distance between the channel plate and the surface of the substrate at 3 mm, the stage was horizontally transported, and film formation was performed for 20 minutes.

[0149] Immediately after that, the supply of nitrogen was stopped, and the supply of the mixed gas to the nozzle unit was stopped.

[0150] For the produced film, it was confirmed by X-ray diffraction measurement that it was α-phase Ga2O3.

[0151] Thereafter, by ellipsometry analysis measurement method, the film thickness of the produced film was measured at 9 points in the in-plane cross direction from the center of the substrate, and the average value was calculated. In addition, the density of foreign substances (with a diameter of 0.3 μm or more) in the region of the film formation surface except for the outer peripheral width of 5 mm was evaluated by a substrate inspection machine (KLAcandela-CS10).

[0152] (Example 2)

[0153] Film formation was carried out in the same manner as in Example 1 except that the temperature of the mixed gas supply nozzle and the bottom surface of the channel plate was maintained at 60° C. and the temperature of the exhaust nozzle was not adjusted (circulating water was not flowed).

[0154] The produced film was confirmed to be α-phase Ga2O3 by X-ray diffraction measurement.

[0155] After that, the thickness of the film was measured at nine points in the plane by polarization analysis, and the average value was calculated. In addition, the density of foreign matter (with a diameter of 0.3 μm or more) in the area other than the outer circumference width of 5 mm on the film formation surface was evaluated by a substrate inspection machine (KLA candela-CS10).

[0156] (Comparative Example 1)

[0157] Film formation was carried out in the same manner as in Example 1 except that the temperature of the bottom surface portion of the mixed gas supply nozzle was maintained at 60° C. and a film formation apparatus without a channel plate and a temperature adjustment element of an exhaust nozzle was used.

[0158] The produced film was confirmed to be α-phase Ga2O3 by X-ray diffraction measurement.

[0159] After that, the thickness of the film was measured at nine points in the plane by polarization analysis, and the average value was calculated. In addition, the density of foreign matter (with a diameter of 0.3 μm or more) in the area other than the outer circumference width of 5 mm on the film formation surface was evaluated by a substrate inspection machine (KLA candela-CS10).

[0160] (Comparative Example 2)

[0161] Film formation was performed in the same manner as in Example 1 except that a film formation apparatus was used which did not include any temperature adjustment elements including the mixed gas supply nozzle, the channel plate, and the exhaust nozzle.

[0162] The produced film was confirmed to be Ga2O3 of the α phase by X-ray diffraction measurement, but it was further confirmed to contain a trace amount of the ε phase.

[0163] After that, the thickness of the film was measured at nine points in the plane by polarization analysis, and the average value was calculated. In addition, the density of foreign matter (with a diameter of 0.3 μm or more) in the area other than the outer circumference width of 5 mm on the film formation surface was evaluated by a substrate inspection machine (KLA candela-CS10).

[0164] (Example 3)

[0165] exist Figure 1In the film forming device, use Figure 2 The film forming portion forms a film of hafnium oxide.

[0166] As a raw material solution, a solution prepared by dissolving hafnium (IV) acetylacetonate in ethanol at a ratio of 0.02 mol / L was prepared and filled into an atomizer equipped with two ultrasonic vibration plates (frequency 2.4 MHz).

[0167] Next, the ultrasonic vibration plate propagates ultrasonic vibration through the water to the raw material solution in the atomizing device, thereby atomizing (misting) the raw material solution.

[0168] Next, a single crystal silicon wafer having a thickness of 0.35 mm and a diameter of 4 inches (about 10 cm) was placed on a SiC stage having a built-in resistance heater and heated to 400°C.

[0169] In addition, an aluminum nozzle with an anodized surface was used for the mixed gas supply element and the exhaust element, and an aluminum plate with an anodized surface was used for the channel plate. In the temperature adjustment part of these nozzles and the channel plate, a glycol-based circulating fluid was circulated in a cooler as a heat medium to maintain the temperature of the bottom surface of each component at 20°C.

[0170] A gas cylinder filled with nitrogen gas was used for carrier gas supply. The gas cylinder and the atomizer were connected by a polyurethane resin pipe, and the atomizer and the nozzle unit were connected by a quartz pipe.

[0171] Next, nitrogen gas was added to the raw material container at a flow rate of 20 L / min, a mixture of mist and nitrogen gas was supplied to the nozzle unit, and exhaust was performed at an exhaust flow rate of 25 L / min. Furthermore, during this period, the distance between the channel plate and the surface of the substrate was maintained at 3 mm while the stage was transported horizontally, and film formation was performed for 20 minutes.

[0172] Immediately thereafter, the supply of nitrogen gas is stopped, and the supply of the mixed gas to the nozzle unit is stopped.

[0173] The produced film was analyzed and confirmed to be HfO2 by XPS measurement and polarization analysis measurement method.

[0174] After that, the thickness of the film was measured at nine points in the plane by polarization analysis, and the average value was calculated. In addition, the density of foreign matter (with a diameter of 0.3 μm or more) in the area other than the outer circumference width of 5 mm on the film formation surface was evaluated by a substrate inspection machine (KLA candela-CS10).

[0175] (Comparative Example 3)

[0176] Film formation was performed in the same manner as in Example 3 except that a film formation apparatus was used which did not include any temperature adjustment elements including the mixed gas supply nozzle, the channel plate, and the exhaust nozzle.

[0177] Next, XPS measurement was performed, and it was found that no film was formed on the substrate.

[0178] Furthermore, thereafter, the same film thickness measurement and foreign matter measurement as in Example 1 were performed.

[0179] (Example 4)

[0180] exist Figure 1 In the film forming device, use Figure 2 The film forming unit forms a silicon oxide film.

[0181] As a raw material solution, a solution containing 0.02 mol / L of polysilazane dissolved in ethylene glycol and 5% by volume of hydrogen peroxide was prepared and filled into an atomizer equipped with two ultrasonic vibration plates (frequency 2.4 MHz).

[0182] Next, the ultrasonic vibration plate propagates ultrasonic vibration through the water to the raw material solution in the atomizing device, thereby atomizing (misting) the raw material solution.

[0183] Next, a single crystal silicon wafer having a thickness of 0.35 mm and a diameter of 4 inches (about 10 cm) was placed on a SiC stage having a built-in resistance heater and heated to 250°C.

[0184] In addition, the mixed gas supply element and the exhaust element use an aluminum nozzle with an anodized surface, and the channel plate uses an aluminum plate with an anodized surface. In the temperature adjustment parts of these nozzles and the channel plate, water is circulated in a cooler as a heat medium to maintain the temperature of the bottom surface of each component at 35°C.

[0185] A gas cylinder filled with nitrogen gas was used for carrier gas supply. The gas cylinder and the atomizer were connected by a polyurethane resin pipe, and the atomizer and the nozzle unit were connected by a quartz pipe.

[0186] Next, nitrogen gas was added to the raw material container at a flow rate of 20 L / min, a mixture of mist and nitrogen gas was supplied to the nozzle unit, and exhaust was performed at an exhaust flow rate of 25 L / min. Furthermore, during this period, the substrate was horizontally transported while keeping the distance between the channel plate and the surface of the substrate at 3 mm, and film formation was performed for 5 minutes.

[0187] Immediately thereafter, the supply of nitrogen gas is stopped, and the supply of the mixed gas to the nozzle unit is stopped.

[0188] The produced film was found to be SiO2 based on the infrared absorption spectrum.

[0189] After that, the thickness of the film was measured at nine points in the plane by polarization analysis, and the average value was calculated. In addition, the density of foreign matter (with a diameter of 0.3 μm or more) in the area other than the outer circumference width of 5 mm on the film formation surface was evaluated by a substrate inspection machine (KLA candela-CS10).

[0190] (Comparative Example 4)

[0191] The film formation was carried out in the same manner as in Example 4 except that a film forming apparatus was used which did not include any temperature adjustment elements including the mixed gas supply nozzle, the channel plate, and the exhaust nozzle.

[0192] Thereafter, the film was evaluated in the same manner as in Example 4.

[0193] The produced film was found to be SiO2 based on the infrared absorption spectrum.

[0194] Thereafter, the film thickness measurement and foreign matter measurement were performed in the same manner as in Example 1.

[0195] [Table 1]

[0196]

[0197] Table 1 shows the evaluation results of Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, 4.

[0198] The film produced by the film forming method of the present invention can achieve stable film growth and suppress the foreign matter density to a low level. In contrast, in the film forming method of the prior art, the film thickness decreases and the foreign matter density increases significantly. It is believed that this is the result of excessive heating of the raw material mist, which causes the solid components in the mist to precipitate, thereby preferentially forming powders and reducing the benefits of film formation.

[0199] As can be seen from the above results, according to the present invention, it is possible to provide a film forming apparatus capable of manufacturing a film of higher quality than the conventional art with high productivity.

[0200] This manual contains the following methods.

[0201] [1]: A film forming method comprising:

[0202] A step of atomizing the raw material solution to form raw material mist;

[0203] The step of mixing the raw material mist with a carrier gas to form a mixed gas;

[0204] The step of placing a substrate on a stage;

[0205] a film forming step of supplying the mixed gas from a mixed gas supplying means to the substrate and forming a film on the substrate by a thermal reaction; and

[0206] an exhaust step of exhausting the mixed gas after film formation by using an exhaust element,

[0207] The film forming method is characterized in that

[0208] A channel plate is disposed on the substrate so as to face the substrate with a space therebetween.

[0209] In the space on the substrate, a mixed gas flow is formed so as to flow linearly from the mixed gas supply element toward the exhaust element in a manner such that the mixed gas flows along at least a portion of the main surface of the substrate,

[0210] In the film forming step and the exhaust step, at least the temperature T1 of the mixed gas supplying element and the temperature T2 of the channel plate are controlled.

[0211] [2]: In the film forming method of the above-mentioned [1], it is characterized by further controlling the temperature T3 of the exhaust element.

[0212] [3]: A film forming method comprising:

[0213] A step of atomizing the raw material solution to form raw material mist;

[0214] The step of mixing the raw material mist with a carrier gas to form a mixed gas;

[0215] The step of placing a substrate on a stage;

[0216] a film forming step of supplying the mixed gas from a mixed gas supplying means to the substrate and forming a film on the substrate by a thermal reaction; and

[0217] an exhaust step of exhausting the mixed gas after film formation by using an exhaust element,

[0218] The film forming method is characterized in that

[0219] A channel plate is disposed on the substrate so as to face the substrate with a space therebetween.

[0220] In the space on the substrate, a mixed gas flow is formed so as to flow linearly from the mixed gas supply element toward the exhaust element in a manner such that the mixed gas flows along at least a portion of the main surface of the substrate,

[0221] In the film forming step and the exhaust step, at least the temperature T2 of the channel plate is controlled.

[0222] [4]: In the film forming method of the above-mentioned [3], it is characterized in that the temperature T3 of the exhaust element is further controlled.

[0223] [5]: A film forming device, characterized in that it comprises:

[0224] an atomizing element, which atomizes the raw material solution to form a raw material mist;

[0225] a carrier gas supply element for conveying the raw material mist;

[0226] A mixed gas supply element supplies a mixed gas formed by mixing the raw material mist and a carrier gas to the surface of the substrate;

[0227] a table on which the substrate is placed;

[0228] an exhaust element for exhausting the mixed gas;

[0229] a channel plate disposed on the base body so as to face the base body with a space therebetween; and

[0230] A temperature control element controls at least the temperature T1 of the mixed gas supply element and the temperature T2 of the channel plate.

[0231] [6]: In the film forming device of the above-mentioned [5], it is characterized in that the film forming device further includes a temperature control element for controlling the temperature T3 of the exhaust element.

[0232] [7]: A laminate comprising:

[0233] a crystalline substrate; and

[0234] a crystalline film formed by epitaxial growth on the crystalline substrate,

[0235] The laminate is characterized in that

[0236] The density of foreign matter with a diameter of 0.3 μm or more on the surface of the crystal film is 1 cm -2 the following.

[0237] [8]: In the laminated body of [7] above, the film thickness of the crystal film is 0.3 μm or more.

[0238] The present invention is not limited to the above-described embodiments. The above-described embodiments are illustrative, and any scheme having substantially the same structure and achieving the same function and effect as the technical concept described in the claims of the present invention is included in the technical scope of the present invention.

Claims

1. A film forming method comprising: A step of atomizing the raw material solution to form raw material mist; The step of mixing the raw material mist with a carrier gas to form a mixed gas; The step of placing a substrate on a stage; a film forming step of supplying the mixed gas from a mixed gas supplying means to the substrate and forming a film on the substrate by a thermal reaction; and an exhaust step of exhausting the mixed gas after film formation by using an exhaust element, The film forming method is characterized in that A channel plate is disposed on the substrate so as to face the substrate with a space therebetween. In the space on the substrate, a mixed gas flow is formed so as to flow linearly from the mixed gas supply element toward the exhaust element in a manner such that the mixed gas flows along at least a portion of the main surface of the substrate, In the film forming step and the exhaust step, at least the temperature T1 of the mixed gas supplying element and the temperature T2 of the channel plate are controlled.

2. The film forming method according to claim 1, It is characterized in that The temperature T3 of the exhaust element is further controlled.

3. A film forming method comprising: A step of atomizing the raw material solution to form raw material mist; The step of mixing the raw material mist with a carrier gas to form a mixed gas; The step of placing a substrate on a stage; a film forming step of supplying the mixed gas from a mixed gas supplying means to the substrate and forming a film on the substrate by a thermal reaction; and an exhaust step of exhausting the mixed gas after film formation by using an exhaust element, The film forming method is characterized in that A channel plate is disposed on the substrate so as to face the substrate with a space therebetween. In the space on the substrate, a mixed gas flow is formed so as to flow linearly from the mixed gas supply element toward the exhaust element in a manner such that the mixed gas flows along at least a portion of the main surface of the substrate, In the film forming step and the exhaust step, at least the temperature T2 of the channel plate is controlled.

4. The film forming method according to claim 3, It is characterized in that The temperature T3 of the exhaust element is further controlled.

5. A film forming device, It is characterized in that have: an atomizing element, which atomizes the raw material solution to form a raw material mist; a carrier gas supply element for conveying the raw material mist; A mixed gas supply element supplies a mixed gas formed by mixing the raw material mist and a carrier gas to the surface of the substrate; a table on which the substrate is placed; an exhaust element for exhausting the mixed gas; a channel plate disposed on the base body so as to face the base body with a space therebetween; and A temperature control element controls at least the temperature T1 of the mixed gas supply element and the temperature T2 of the channel plate.

6. The film forming device according to claim 5, It is characterized in that The film forming apparatus further includes a temperature control element for controlling a temperature T3 of the exhaust element.

7. A laminate comprising: a crystalline substrate; and a crystalline film formed by epitaxial growth on the crystalline substrate, The laminate is characterized in that The density of foreign matter with a diameter of 0.3 μm or more on the surface of the crystal film is 1 cm -2 the following.

8. The laminate according to claim 7, It is characterized in that The film thickness of the crystal film is 0.3 μm or more.