Casting process of aluminum alloy end cover for lightweight motor

By adopting specific mold structures and process flows in motor end cap casting, using inert gas pressurization and alternating pressure reduction, combined with the use of refining agents and mold release agents, the difficulty of metal filling and gas discharge problems during casting is solved. , realizes high-quality and lightweight aluminum alloy end caps, improving the mechanical properties and service life of the motor.

CN119035462APending Publication Date: 2024-11-29JIANGSU YOUGEMAN AVIATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411109931.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During the casting process, the existing motor end covers are designed with many cavity, which makes it difficult to fill the metal liquid and the internal gas difficult to discharge, resulting in defects and affecting the mechanical properties and service life.

Method used

Using a casting process for aluminum alloy end caps for lightweight motors, by setting a specific cavity structure and casting method in the mold, pressurization and alternating pressure reduction are used to ensure that the metal liquid is fully filled and discharged from the internal gas, combined with refining The use of agent and release agent is carried out in solid solution and aging treatment, and finally achieves a high-quality end cap finished product.

Benefits of technology

The prepared end cap is light in weight, has no pores or slag inclusions inside, has uniform structure, small grains, excellent mechanical properties, and effectively improves service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035462A_ABST
    Figure CN119035462A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of cast aluminum alloy, in particular to a casting process of an aluminum alloy end cover for a lightweight motor. Comprising the following steps that S1, smelting is conducted, specifically, raw materials are put into a smelting furnace, after the raw materials are completely smelted, a refining agent is added for refining, and molten metal is obtained; s2, molten metal is poured into the mold, and an end cover blank is manufactured; s3, heat treatment is conducted, specifically, solution treatment and aging treatment are conducted on the end cover blank in sequence; and S4, finish machining is conducted, specifically, the end cover blank subjected to heat treatment is subjected to finish machining, and an end cover finished product is obtained. The end cover prepared through the casting technology is light in weight, free of defects such as air holes and slag inclusion inside during casting, uniform in internal structure, small in crystal grain and excellent in mechanical property, and the service life of the end cover can be effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cast aluminum alloys, and in particular to a casting process for an aluminum alloy end cover for a lightweight motor. Background Art

[0002] In recent years, new energy vehicles have developed rapidly due to their advantages of environmental protection, low carbon and high efficiency. New energy vehicles refer to vehicles that use non-traditional fuels or energy, mainly including pure electric vehicles, plug-in hybrid vehicles and fuel cell vehicles, etc. These vehicles use batteries, electric motors, supercapacitors, fuel cells, etc. as power sources to replace traditional fuel engines.

[0003] The stable operation of new energy vehicles is closely related to the performance of the motor. The motor is mainly composed of a housing, an end cover, and an internal stator and rotor. The main function of the end cover is to seal the inside of the motor and fix the rotor. In order to reduce the weight, the existing motor end cover is often designed with more cavities, which makes it difficult to fill the mold with molten metal during casting, and it is difficult to discharge the internal gas when the molten metal solidifies. There are many defects inside the end cover, which affects the mechanical properties of the end cover and affects the service life of the motor. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a casting process for an aluminum alloy end cover for a lightweight motor.

[0005] The technical solution of the present invention is: a casting process of aluminum alloy end cover for lightweight motor, comprising the following steps:

[0006] S1. Melting

[0007] Put the raw materials into a smelting furnace and heat them to 750-800°C until all the raw materials are melted, then add a refining agent for refining to obtain molten metal;

[0008] S2, pouring the molten metal into the mold to obtain an end cover blank;

[0009] The mold comprises an upper mold and a lower mold, a columnar core is provided at the center of the lower mold, and an inner annular partition and an outer annular partition are arranged concentrically with the columnar core, a first cavity is formed between the inner annular partition and the columnar core, a second cavity is formed between the outer annular partition and the inner annular partition, a first pouring port for adding molten metal into the first cavity and a second pouring port for adding molten metal into the second cavity are provided on the upper mold, a first annular core is provided on the upper mold located in the first cavity, a second annular core is provided on the upper mold located in the second cavity, and a partition core for controlling the connection or closure between the first cavity and the second cavity is slidably provided between the first annular core and the second annular core;

[0010] The specific casting method is:

[0011] S2-1, spraying a release agent on the upper mold and the lower mold surface, and after the release agent is sprayed, pouring the molten metal into the first cavity and the second cavity through the first pouring gate and the second pouring gate respectively;

[0012] S2-2, filling the first cavity and the second cavity with inert gas to pressurize them, the filling pressure is 0.3-0.5 MPa, the pressurization time is 10-20 seconds, then releasing the pressure and moving the partition core upward to connect the first cavity with the second cavity, and after standing for 15-30 seconds, replenishing the molten metal into the mold through the third pouring port;

[0013] S2-3. After the metal liquid is replenished, the first cavity and the second cavity are pressurized with inert gas at the same time. The pressure is 0.4-0.6MPa. After 10-20s of pressurization, the pressure in the first cavity and the second cavity is reduced alternately. The single pressure reduction in the first cavity is n, and the single pressure reduction in the second cavity is 2n. After each pressure reduction, it is maintained for 10-15s. The value of n is 0.05-0.15MPa.

[0014] S2-4, until the pressure in the first cavity and the second cavity drops to normal pressure, cooling for 6 to 8 hours to obtain the end cover blank;

[0015] S3. Heat treatment

[0016] The end cap blank is subjected to solution treatment and aging treatment in sequence to obtain a heat-treated end cap blank;

[0017] S4, finishing

[0018] After the heat treatment, the end cover blank is finely processed to remove burrs to obtain the end cover finished product.

[0019] Description: In the above casting process, the first cavity and the second cavity are firstly closed and poured to ensure that the molten metal can be fully filled, and then the first cavity and the second cavity are connected so that the internal gas can be fully discharged through the third pouring port. The pressure in the first cavity and the second cavity is alternately reduced to ensure that the cavity space can be completely filled. The end cover finally prepared is light in weight, free of defects such as pores and slag inclusions, has uniform structure, small grains, and excellent mechanical properties, which can effectively improve the service life of the end cover.

[0020] Furthermore, the raw material comprises the following components by mass percentage: Mg 2.5-3.4%, Mn 2.2-3.2%, Cu 1.2-1.8%, Si 5.0-8.0%, Fe 0.1-0.3%, Cr 0.1-0.2%, and the balance is Al.

[0021] Note: The raw materials of the above components have good fluidity after melting, and can completely fill the cavity to avoid casting defects. The upper layer of molten metal can effectively compensate for shrinkage and avoid defects such as pores inside.

[0022] Furthermore, the refining agent comprises, by weight: 10 to 20 parts of NaOH, 8 to 12 parts of Na3AlF, 3 to 8 parts of CaF2, 30 to 40 parts of KCl, and 1 to 2 parts of rare earth.

[0023] Note: The above refining agent can effectively remove the gas in the molten metal and reduce the bubbles in the molten metal. The refining agent can also remove impurities in the molten metal and avoid slag inclusion in the end cover.

[0024] Furthermore, the refining step is: adding a refining agent accounting for 0.3-0.4% of the total mass of the raw material, stirring for 4-6 minutes, then scraping off the surface scum, adjusting the temperature of the smelting furnace to 720-730°C, adding a refining agent accounting for 0.1-0.2% of the mass of the raw material again, and after standing for 2-3 minutes, the refining is completed.

[0025] Note: The above refining steps can release the refining agent evenly into the molten metal, so that the gas in the molten metal can be effectively discharged.

[0026] Furthermore, the release agent comprises, by weight, 12 to 18 parts of polydimethylsiloxane, 4 to 6 parts of sodium tetraborate, 3 to 5 parts of triethanolamine, 10 to 15 parts of trichlorosilane, and 25 to 35 parts of oleyl glyceride.

[0027] Description: The above-mentioned release agent has good demoulding performance, which can ensure the effective separation of the end cap blank from the mold and the surface quality of the end cap blank. The trichlorosilane in the release agent can react with hydrogen and oxygen during the flow of the molten metal, reduce the gas inclusions in the molten metal, and add silicon to the molten metal. At the same time, the sodium hydroxide in the refining agent can react with the generated hydrochloric acid to release heat, slow down the solidification speed of the molten metal, and enable the gas in the molten metal to be fully discharged, thereby ensuring the casting quality of the end cap.

[0028] Furthermore, in step S2-1, the spraying amount of the release agent is 5 to 6 g / cm 2 .

[0029] Note: Limiting the spraying amount of molten metal can ensure the demoulding effect and the gas removal effect in the molten metal.

[0030] Furthermore, in step S2-4, an ultrasonic field is applied to the mold for 30 to 45 minutes during cooling, the ultrasonic frequency is 30 to 40 kHz, and the ultrasonic power is 1000 to 1500 W.

[0031] Note: The ultrasonic field can disturb the molten metal, so that the elements in the molten metal can be evenly distributed, avoiding excessive concentration of doped elements inside the molten metal.

[0032] Furthermore, the solution treatment method is: keeping the end cover blank at 500-520° C. for 2-3 hours, and then taking it out of the furnace and water cooling it.

[0033] Note: The above-mentioned solid solution treatment can dissolve other metal elements into the aluminum matrix to form a solid solution, refine the grains, and improve the plasticity and toughness of the end cover blank.

[0034] Furthermore, the aging treatment method is: keeping the end cover blank at 180-220° C. for 6-8 hours, and then taking it out of the furnace and air cooling it.

[0035] Description: Aging treatment can make the structure of the end cover blank more uniform, the grain boundary structure more dense, and improve the strength and hardness of the end cover blank.

[0036] The beneficial effects of the present invention are:

[0037] (1) The end cap prepared by the casting process of the present invention is light in weight, has no internal defects such as pores and slag inclusions during casting, has uniform internal structure, small grains, and excellent mechanical properties, which can effectively improve the service life of the end cap.

[0038] (2) The demolding agent of the present invention has good demolding performance, which can ensure that the end cover blank is effectively separated from the mold, and silicon trichloride can react with hydrogen and oxygen at high temperature to reduce gas inclusions in the molten metal and add silicon to the molten metal. At the same time, the sodium hydroxide in the refining agent can react with the generated hydrochloric acid to release heat, slow down the solidification rate of the molten metal, and enable the gas in the molten metal to be fully discharged, thereby ensuring the casting quality of the end cover. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a schematic diagram of the internal structure of the mold of the present invention;

[0040] Figure 2 It is a schematic diagram of the end cover structure of the present invention;

[0041] Among them, 1-upper mold, 11-first annular core, 12-second annular core, 2-lower mold, 21-columnar core, 22-inner annular partition, 23-outer annular partition, 3-first cavity, 4-second cavity, 5-partition core, 6-first pouring gate, 7-second pouring gate, 8-third pouring gate. DETAILED DESCRIPTION

[0042] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.

[0043] Embodiment 1: A casting process for an aluminum alloy end cover for a lightweight motor, comprising the following steps:

[0044] S1. Melting

[0045] Put the raw materials into a smelting furnace and heat them to 780°C until all the raw materials are melted, then add a refining agent for refining to obtain molten metal;

[0046] The raw materials include the following components by mass percentage: Mg 3.0%, Mn 2.7%, Cu 1.6%, Si 6.5%, Fe0.2%, Cr 0.15%, and the balance is Al;

[0047] The refining agent includes, by weight: 15 parts of NaOH, 10 parts of Na3AlF, 5 parts of CaF2, 35 parts of KCl, and 1.5 parts of rare earth; wherein the rare earth is lanthanum;

[0048] The refining steps are as follows: add a refining agent accounting for 0.35% of the total weight of the raw material, stir for 5 minutes, then scrape off the surface scum, adjust the temperature of the smelting furnace to 725°C, add a refining agent accounting for 0.15% of the weight of the raw material again, and after standing for 2.5 minutes, the refining is completed;

[0049] S2, pouring molten metal into the mold to obtain an end cover blank;

[0050] like Figure 1 As shown, the mold includes an upper mold 1 and a lower mold 2, a columnar core 21 is provided at the center of the lower mold 2, and an inner annular partition 22 and an outer annular partition 23 are arranged concentrically with the columnar core, a first cavity 3 is formed between the inner annular partition 22 and the columnar core 21, and a second cavity 4 is formed between the outer annular partition 23 and the inner annular partition 22, a first pouring port 6 for adding molten metal into the first cavity 3, and a second pouring port 7 for adding molten metal into the second cavity 4 are provided on the upper mold 1, a first annular core 11 is provided on the upper mold 1 located in the first cavity 3, and a second annular core 12 is provided on the upper mold 1 located in the second cavity 4, and a partition core 5 for controlling the connection or closure between the first cavity 3 and the second cavity 4 is slidably provided between the first annular core 11 and the second annular core 12;

[0051] The specific casting method is:

[0052] S2-1, spraying a release agent on the surface of the upper mold 1 and the lower mold 2, and after the release agent is sprayed, pouring the molten metal into the first cavity 3 and the second cavity 4 through the first pouring port 6 and the second pouring port 7 respectively;

[0053] S2-2, inert gas is filled into the first cavity 3 and the second cavity 4 for pressurization, the filling pressure is 0.4 MPa, the pressurization time is 15 seconds, and then the pressure is released and the partition core 5 is moved upward to connect the first cavity 3 with the second cavity 4. After standing for 22 seconds, the metal liquid is added into the mold through the third pouring port 8;

[0054] S2-3, after the metal liquid is replenished, the first cavity 3 and the second cavity 4 are pressurized with inert gas at the same time, and the pressure is 0.5MPa. After 15s of pressurization, the pressure in the first cavity 3 and the second cavity 4 are alternately reduced in turn. The single pressure reduction amount in the first cavity 3 is n, and the single pressure reduction amount in the second cavity 4 is 2n. After each pressure reduction, it is maintained for 10 to 15s; the value of n is 0.1MPa;

[0055] S2-4, until the pressure in the first cavity 3 and the second cavity 4 drops to normal pressure, cooling for 7 hours to obtain the end cover blank;

[0056] The release agent is calculated by weight and includes: 16 parts of polydimethylsiloxane, 5 parts of sodium tetraborate, 4 parts of triethanolamine, 12 parts of trichlorosilane, and 30 parts of oleyl glycerol; the spraying amount of the release agent is 5.5g / cm 2 ;

[0057] During cooling, an ultrasonic generator was used to apply an ultrasonic field to the mold for 40 min, with an ultrasonic frequency of 35 kHz and an ultrasonic power of 1200 W;

[0058] S3. Heat treatment

[0059] The end cap blank is subjected to solution treatment and aging treatment in sequence to obtain a heat-treated end cap blank; the solution treatment method is: the end cap blank is kept at 510°C for 2.5 hours, and then taken out of the furnace for water cooling; the aging treatment method is: the end cap blank is kept at 200°C for 7 hours, and then taken out of the furnace for air cooling;

[0060] S4, finishing

[0061] After heat treatment, the end cap blank is finely processed to remove burrs to obtain the end cap finished product, such as Figure 2 shown.

[0062] Example 2: This example is basically the same as Example 1, except that the raw materials include the following components by weight: Mg 2.5%, Mn 2.2%, Cu 1.2%, Si 5.0%, Fe 0.1%, Cr 0.1%, and the balance is Al.

[0063] Example 3: This example is basically the same as Example 1, except that the raw materials include the following components by weight: Mg 3.4%, Mn 3.2%, Cu 1.8%, Si 8.0%, Fe 0.3%, Cr 0.2%, and the balance is Al.

[0064] Example 4: This example is basically the same as Example 1, except that the refining agent comprises, by weight: 10 parts of NaOH, 8 parts of Na3AlF, 3 parts of CaF2, 30 parts of KCl, and 1 part of rare earth.

[0065] Example 5: This example is basically the same as Example 1, except that the refining agent comprises, by weight: 20 parts of NaOH, 12 parts of Na3AlF, 8 parts of CaF2, 40 parts of KCl, and 2 parts of rare earth.

[0066] Example 6: This example is basically the same as Example 1, except that 0.3% of the total mass of the refining agent is added to the raw material, stirred for 5 minutes, then the surface scum is scraped off, the temperature of the smelting furnace is adjusted to 725°C, and 0.1% of the mass of the raw material is added again.

[0067] Example 7: This example is basically the same as Example 1, except that 0.4% of the total mass of the refining agent is added to the raw material, stirred for 5 minutes, then the surface scum is scraped off, the temperature of the smelting furnace is adjusted to 725°C, and 0.2% of the mass of the raw material is added again.

[0068] Example 8: This example is basically the same as Example 1, except that the release agent is calculated by weight: 12 parts of polydimethylsiloxane, 4 parts of sodium tetraborate, 3 parts of triethanolamine, 10 parts of trichlorosilane, and 25 parts of oleyl glycerol.

[0069] Example 9: This example is basically the same as Example 1, except that the release agent is calculated by weight: 18 parts of polydimethylsiloxane, 6 parts of sodium tetraborate, 5 parts of triethanolamine, 15 parts of trichlorosilane, and 35 parts of oleyl glycerol.

[0070] Example 10: This example is basically the same as Example 1, except that the spraying amount of the release agent is 5 g / cm 2 .

[0071] Example 11: This example is basically the same as Example 1, except that the spraying amount of the release agent is 6 g / cm 2 .

[0072] Example 12: This example is basically the same as Example 1, except that, in step S2-3, after the metal liquid is replenished, an inert gas is used to pressurize the first cavity 3 and the second cavity 4 at the same time, and the charging pressure is 0.4 MPa.

[0073] Example 13: This example is basically the same as Example 1, except that, in step S2-3, after the metal liquid is replenished, an inert gas is used to pressurize the first cavity 3 and the second cavity 4 at the same time, and the charging pressure is 0.6 MPa.

[0074] Example 14: This example is basically the same as Example 1, except that in step S2-3, the value of n is 0.05 MPa.

[0075] Example 15: This example is basically the same as Example 1, except that in step S2-3, the value of n is 0.15 MPa.

[0076] Example 16: This example is basically the same as Example 1, except that the ultrasonic frequency is 30kHz.

[0077] Example 17: This example is basically the same as Example 1, except that the ultrasonic frequency is 40kHz.

[0078] Example 18: This example is basically the same as Example 1, except that the ultrasonic power is 1000W.

[0079] Example 19: This example is basically the same as Example 1, except that the ultrasonic power is 1500W.

[0080] Example 20: This example is basically the same as Example 1, except that the solution treatment method is: keeping the end cover blank at 500°C for 2 hours, and then taking it out of the furnace and cooling it with water.

[0081] Example 21: This example is basically the same as Example 1, except that the solution treatment method is: keeping the end cover blank at 520°C for 3 hours, and then taking it out of the furnace and cooling it with water.

[0082] Example 22: This example is basically the same as Example 1, except that the aging treatment method is: keeping the end cover blank at 180°C for 6 hours, and then taking it out of the furnace and air cooling it.

[0083] Example 23: This example is basically the same as Example 1, except that the aging treatment method is: keeping the end cover blank at 220°C for 8 hours, and then taking it out of the furnace and air cooling it.

[0084] Comparative Example 1: Using Example 1 as a reference, the sodium hydroxide in the refining agent was removed.

[0085] Comparative Example 2: Taking Example 1 as a reference, the refining agent was added all at once.

[0086] Comparative Example 3: Using Example 1 as a reference, trichlorosilane in the release agent was removed.

[0087] Comparative Example 4: With reference to Example 1, the pressure in the first cavity 3 and the second cavity 4 was maintained at 0.5 MPa without any change.

[0088] Comparative Example 5: Using Example 1 as a reference, no ultrasonic field was applied during cooling.

[0089] Experimental Example: The end caps prepared in various embodiments were subjected to performance tests to explore the influence of the parameters of each embodiment on the performance of the end caps. The specific exploration is as follows:

[0090] Experimental Example 1: Investigating the influence of raw material composition on end cap performance

[0091] Using Examples 1 to 3 as experimental comparison, the end cap performances under different raw material compositions are shown in Table 1 below:

[0092] Table 1 Effect of raw material composition on end cap performance

[0093] Group Tensile strength / MPa Hardness / HV Example 1 512 456 Example 2 520 422 Example 3 479 464

[0094] It can be seen from the data in Table 1 that although the tensile strength of the end cap of Example 2 is improved, the hardness is greatly reduced, and although the hardness of the end cap of Example 3 is improved, the tensile strength is greatly reduced. Therefore, the end cap of Example 1 has the best comprehensive performance, and the raw material composition selected in Example 1 is optimal.

[0095] Experimental Example 2: Investigating the effects of refining agent composition and addition amount on end cap performance

[0096] Using Example 1, Examples 4 to 7 and Comparative Examples 1 to 2 as experimental comparisons, the end cap performances under different components and addition amounts of the refining agent are shown in Table 2 below:

[0097] Table 2 Effect of refining agent composition and addition amount on end cap performance

[0098] Group Tensile strength / MPa Hardness / HB Example 1 512 456 Example 4 478 429 Example 5 469 433 Example 6 484 438 Example 7 473 431 Comparative Example 1 435 416 Comparative Example 2 453 430

[0099] From the data in Table 2, it can be seen that compared with Examples 4 to 7, the composition of the refining agent and the amount of the refining agent added in Example 1 will affect the performance of the end cap, among which the tensile strength and hardness of the end cap in Example 1 are the highest, so the composition of the refining agent and the amount of the refining agent added in Example 1 are the best;

[0100] In Example 1, compared with Comparative Examples 1 to 2, the performance of the end cap decreased after the sodium hydroxide in the refining agent was removed. This may be because the hydrochloric acid gas generated by the release agent reaction could not be neutralized after the sodium hydroxide was removed, and the cooling rate of the molten metal was too fast, resulting in part of the gas being unable to be discharged, causing defects in the end cap structure; after the refining agent was added all at once, the performance of the end cap decreased, which may be because the components in the refining agent were not evenly distributed in the molten metal.

[0101] Experimental Example 3: Investigating the effects of release agent composition and addition amount on end cap performance

[0102] Using Example 1, Examples 8 to 11 and Comparative Examples 3 to 4 as experimental comparisons, the end cap performances with different components and different addition amounts of the release agent are shown in Table 3 below:

[0103] Table 3 Effect of release agent composition and addition amount on end cap performance

[0104] Group Tensile strength / MPa Hardness / HB Example 1 512 456 Example 8 504 448 Example 9 493 442 Example 10 482 438 Embodiment 11 487 440 Comparative Example 3 406 416

[0105] It can be seen from the data in Table 3 that compared with Examples 8 to 11, the release agent components and addition amount of Example 1 will affect the performance of the end cap, among which the end cap of Example 1 has the highest tensile strength and hardness, so the release agent components and addition amount selected in Example 1 are the best;

[0106] Compared with Comparative Example 3, after removing trichlorosilane from the release agent, the performance of the end cap decreased in Example 1. This may be because after removing trichlorosilane, more hydrogen and oxygen existed in the molten metal, resulting in more defects in the end cap structure.

[0107] Experimental Example 4: Investigating the influence of charging pressure and pressure variation on the performance of the end cap

[0108] Using Example 1 and Examples 12 to 15 as experimental comparisons, the end cap performances under different charging pressures and different pressure changes are shown in Table 4 below:

[0109] Table 4 Effects of charging pressure and pressure variation on end cap performance

[0110]

[0111]

[0112] It can be seen from the data in Table 4 that compared with Examples 1 to 15, the charging pressure and pressure variation of Example 1 have an impact on the performance of the end cap, among which the end cap of Example 1 has the highest tensile strength and hardness, so the charging pressure and pressure variation selected in Example 1 are both optimal;

[0113] Compared with comparative example 4, in embodiment 1, the performance of the end cover was reduced after the pressure in the first cavity 3 and the second cavity 4 did not change. This may be because the molten metal failed to effectively fill the cavity, resulting in more defects inside the end cover.

[0114] Experimental Example 5: Investigating the influence of ultrasonic field parameters on the performance of the end cap

[0115] Using Example 1, Examples 16 to 19 and Comparative Example 5 as experimental comparisons, the end cap performance under different ultrasonic field parameters is shown in Table 5 below:

[0116] Table 5 Effect of ultrasonic field parameters on end cap performance

[0117] Group Tensile strength / MPa Hardness / HB Example 1 512 456 Example 16 505 451 Embodiment 17 495 448 Embodiment 18 493 445 Embodiment 19 497 450 Comparative Example 5 468 431

[0118] It can be seen from the data in Table 5 that, compared with Examples 16 to 17, the ultrasonic frequency and power of Example 1 will affect the performance of the end cap, among which the end cap of Example 1 has the highest tensile strength and hardness, so the ultrasonic parameters selected in Example 1 are the best;

[0119] Compared with comparative example 5, the performance of the end cap in Example 1 was reduced after the ultrasonic field was not applied. This may be because the silicon element generated by the reaction of trichlorosilane could not diffuse into the interior of the molten metal after the ultrasonic field was not applied.

[0120] Experimental Example 6: Investigating the influence of heat treatment parameters on the performance of end caps

[0121] Using Example 1 and Examples 20 to 23 as experimental comparisons, the end cap performance under different heat treatment parameters is shown in Table 6 below:

[0122] Table 6 Effect of heat treatment parameters on end cap performance

[0123]

[0124]

[0125] It can be seen from the data in Table 6 that, compared with Examples 20 to 23, both the solution treatment and aging treatment parameters of Example 1 will affect the performance of the end cap, among which the end cap of Example 1 has the highest tensile strength and hardness, so the heat treatment parameters selected in Example 1 are optimal.

Claims

1. A casting process for an aluminum alloy end cover for a lightweight motor, characterized in that: The following steps are involved: S1. Melting Put the raw materials into a smelting furnace and heat them to 750-800°C until all the raw materials are melted, then add a refining agent for refining to obtain molten metal; S2, pouring the molten metal into the mold to obtain an end cover blank; The mold comprises an upper mold (1) and a lower mold (2); a columnar core (21) is provided at the center of the lower mold (2), and an inner annular partition (22) and an outer annular partition (23) are arranged concentrically with the columnar core; a first mold cavity (3) is formed between the inner annular partition (22) and the columnar core (21); a second mold cavity (4) is formed between the outer annular partition (23) and the inner annular partition (22); and a tool for adding molten metal into the first mold cavity (3) is provided on the upper mold (1). A first pouring port (6) and a second pouring port (7) for adding molten metal into the second cavity (4); a first annular core (11) is provided on the upper mold (1) located in the first cavity (3); a second annular core (12) is provided on the upper mold (1) located in the second cavity (4); a partition core (5) is slidably provided between the first annular core (11) and the second annular core (12) for controlling the connection or closure between the first cavity (3) and the second cavity (4); The specific casting method is: S2-1, spraying a mold release agent on the surface of the upper mold (1) and the lower mold (2), and after the mold release agent is sprayed, pouring the molten metal into the first mold cavity (3) and the second mold cavity (4) through the first pouring port (6) and the second pouring port (7) respectively; S2-2, filling the first cavity (3) and the second cavity (4) with an inert gas to pressurize them, the filling pressure being 0.3 to 0.5 MPa, the pressurization time being 10 to 20 seconds, then releasing the pressure and moving the partition core (5) upwards to connect the first cavity (3) and the second cavity (4), and after standing for 15 to 30 seconds, replenishing the molten metal into the mold through the third pouring port (8); S2-3, after the metal liquid is replenished, the first cavity (3) and the second cavity (4) are pressurized simultaneously with an inert gas, the pressure of which is 0.4 to 0.6 MPa. After 10 to 20 seconds of pressurization, the pressure in the first cavity (3) and the second cavity (4) are alternately reduced in turn, the pressure reduction amount in the first cavity (3) is n, and the pressure reduction amount in the second cavity (4) is 2n, and the pressure is maintained for 10 to 15 seconds after each pressure reduction; the value of n is 0.05 to 0.15 MPa; S2-4, until the pressure in the first cavity (3) and the second cavity (4) drops to normal pressure, cooling for 6 to 8 hours to obtain an end cap blank; S3. Heat treatment The end cap blank is subjected to solution treatment and aging treatment in sequence to obtain a heat-treated end cap blank; S4, finishing After the heat treatment, the end cover blank is finely processed to remove burrs to obtain the end cover finished product.

2. The casting process of aluminum alloy end cover for lightweight motor according to claim 1, characterized in that: The raw material comprises the following components by mass percentage: Mg 2.5-3.4%, Mn 2.2-3.2%, Cu 1.2-1.8%, Si 5.0-8.0%, Fe 0.1-0.3%, Cr 0.1-0.2%, and the balance is Al.

3. The casting process of aluminum alloy end cover for lightweight motor according to claim 1, characterized in that: The refining agent comprises, by weight: 10 to 20 parts of NaOH, 8 to 12 parts of Na3AlF, 3 to 8 parts of CaF2, 30 to 40 parts of KCl, and 1 to 2 parts of rare earth.

4. The casting process of aluminum alloy end cover for lightweight motor according to claim 3 is characterized in that: The refining step is: adding a refining agent accounting for 0.3-0.4% of the total mass of the raw material, stirring for 4-6 minutes, then scraping off the surface scum, adjusting the temperature of the smelting furnace to 720-730°C, adding a refining agent accounting for 0.1-0.2% of the mass of the raw material again, and standing for 2-3 minutes to complete the refining.

5. The casting process of aluminum alloy end cover for lightweight motor according to claim 1, characterized in that: The release agent comprises, by weight, 12 to 18 parts of polydimethylsiloxane, 4 to 6 parts of sodium tetraborate, 3 to 5 parts of triethanolamine, 10 to 15 parts of trichlorosilane, and 25 to 35 parts of oleic acid glyceride.

6. The casting process of aluminum alloy end cover for lightweight motor according to claim 5, characterized in that: In step S2-1, the spraying amount of the release agent is 5 to 6 g / cm 2 .

7. The casting process of aluminum alloy end cover for lightweight motor according to claim 1, characterized in that: In step S2-4, an ultrasonic field is applied to the mold for 30 to 45 minutes during cooling, the ultrasonic frequency is 30 to 40 kHz, and the ultrasonic power is 1000 to 1500 W.

8. The casting process of aluminum alloy end cover for lightweight motor according to claim 1, characterized in that: The solution treatment method is: keeping the end cover blank at 500-520° C. for 2-3 hours, and then taking it out of the furnace and cooling it with water.

9. The casting process of aluminum alloy end cover for lightweight motor according to claim 1, characterized in that: The aging treatment method is: keeping the end cover blank at 180-220° C. for 6-8 hours, and then taking it out of the furnace and air cooling it.