Hard polyurethane / Mxene-coated HNT / gel flame-retardant material and preparation method thereof

By using Mxene@HNT and hydrogel layer-by-layer coating technology on the hard polyurethane surface, an organ-like structure is formed, which solves the problem of easy fall off and poor flame retardant effect, and achieves efficient flame retardant effect and safety promote.

CN119039656APending Publication Date: 2024-11-29WUHAN UNIV OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411185506.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The flame retardant in the rigid polyurethane flame retardant materials is prone to fall off, and the flame retardant effect is poor, resulting in the release of a large amount of heat and harmful gases during the combustion process, causing safety problems.

Method used

Using Mxene@HNT and hydrogel layer-by-layer coating technology, Mxene@HNT is coated onto the surface of the hard polyurethane to form an organ-like structure, enhance the flame retardant effect, and prevent the flame retardant from falling off through the hydrogel layer, and coordinate the resistance. Burn.

Benefits of technology

The flame retardant grade is significantly improved, from V1 to V0, which extends the production of residual carbon during combustion, enhances the smoke suppression effect, and improves the scratch resistance and durability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039656A_ABST
    Figure CN119039656A_ABST
Patent Text Reader

Abstract

The invention relates to a hard polyurethane / Mxene-coated HNT / gel flame-retardant material and a preparation method thereof.The preparation method comprises the following steps that Mxene and halloysite nanotubes are added into water and evenly dispersed to obtain a mixture A, and the mixture A is dried to obtain Mxene-coated HNT; adding the Mxene (at) HNT and calcium salt into an alcohol solvent, and uniformly dispersing to obtain a mixture B; coating the mixture B on the surface of hard polyurethane, and drying to obtain RPUF / M-H; and soaking the RPUF / M coated H into the hydrogel solution, carrying out gelation reaction, and after the reaction is finished, drying to obtain the polyurethane / Mxene coated HNT / gel flame-retardant material. The Mxene-coated HNT has an organ-shaped structure, so that heat and smoke diffusion paths are increased, and the flame-retardant effect of the flame-retardant material is enhanced; and then through coating of the hydrogel, the Mxene-coated HNT is prevented from falling off, and a synergistic flame-retardant effect can be achieved with the Mxene-coated HNT.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyurethane flame retardant materials, and specifically relates to a rigid polyurethane / Mxene@HNT / gel flame retardant material and a preparation method thereof. Background Art

[0002] Rigid polyurethane foam (RPUF) has the advantages of good thermal conductivity, low apparent density, high mechanical properties, and good hydrophobicity, and is widely used in building pipe insulation, transportation, and various industrial applications. However, the dependence of RPUF production on petroleum resources, coupled with the gradual depletion of petroleum resources, has prompted the need for cleaner and more environmentally friendly alternatives to mitigate environmental pollution. Therefore, more attention is currently paid to the use of plant sources, such as castor, bamboo, soybean, etc., to develop vegetable oil-based polyols as alternatives to petroleum-based polyols. Despite these advantages, the loose and porous internal structure of rigid polyurethane leads to a low limiting oxygen index (LOI), a low UL-94 flame retardant rating, and other combustion-related problems, which in turn leads to the release of a large amount of heat and harmful gases such as CO during combustion, causing serious safety issues. Therefore, there is an urgent need to design and produce environmentally friendly rigid polyurethane flame retardant systems with good flame retardant effects.

[0003] In flame-retardant RPUFs, the surface area may partially burn while the interior remains intact, indicating that flame retardancy is mainly manifested by the formation of a protective carbon layer on the surface. However, this interior usually lacks an effective flame retardant barrier, rendering most of the internal flame retardants ineffective and potentially compromising the original properties of the polyurethane. Therefore, surface coating treatments offer a promising approach to impart excellent flame retardancy to RPUFs while maintaining their original mechanical properties, making it a viable design solution. However, flame retardant materials generally have poor adhesion to rigid polyurethane surfaces, leading to a series of problems such as easy detachment of the flame retardant, poor flame retardant effect, and poor durability. Summary of the invention

[0004] The purpose of the present invention is to overcome the above technical deficiencies, provide a rigid polyurethane / Mxene@HNT / gel flame retardant material and a preparation method thereof, and solve the technical problems in the prior art that the flame retardant in the polyurethane flame retardant material is easy to fall off and the flame retardant effect is poor.

[0005] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a method for preparing a rigid polyurethane / Mxene@HNT / gel flame retardant material, comprising the following steps: S1, adding Mxene and halloysite nanotubes to water, dispersing them evenly to obtain a mixture A, and drying them to obtain Mxene@HNT; S2, adding Mxene@HNT and calcium salt to an alcohol solvent, dispersing them evenly to obtain a mixture B; S3, coating the mixture B on the surface of a rigid polyurethane, and drying them to obtain RPUF / M@H; S4, immersing RPUF / M@H in a hydrogel solution to perform a gelation reaction, and drying them after the reaction to obtain a polyurethane / Mxene@HNT / gel flame retardant material.

[0006] In a second aspect, the present invention provides a rigid polyurethane / Mxene@HNT / gel flame retardant material prepared by the above preparation method.

[0007] Compared with the prior art, the beneficial effects of the present invention include: The present invention first prepares Mxene@HNT, and then uses hydrogel to coat Mxene@HNT on the surface of rigid polyurethane (RPUF) in a layer-by-layer coating manner, thereby forming a rigid polyurethane / Mxene@HNT / gel flame retardant material; wherein, halloysite nanotubes (HNT) and Mxene are substances with good flame retardant properties, and the prepared Mxene@HNT has an accordion-like structure, which increases the path for heat and smoke diffusion and enhances the flame retardant effect of the flame retardant material; and then through the coating of hydrogel, the problems of easy leakage of flame retardant materials and short effective time in the flame retardant of the surface coating are effectively solved, the Mxene@HNT is prevented from falling off, and the Mxene@HNT can have a synergistic flame retardant effect, and the flame retardant grade is between V1 and V0. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 This is a scanning electron microscope (SEM) image of the Mxene@HNT prepared in Example 1; wherein the scale bar in (a) is 4 μm, and the scale bar in (b) is 1 μm; Figure 2 This is the energy spectrum analysis (EDS) of Mxene@HNT prepared in Example 1; wherein (a) is Ti, Al, and Si, (b) is Al, (c) is Si, and (d) is Ti; Figure 3 The vertical combustion pictures of the RPUF / Mxene@HNT-3 / DH flame retardant material prepared in Example 3 and the original rigid polyurethane (RPUF) in Comparative Example 1; wherein, group (a) is Comparative Example 1, and group (b) is Example 3; Figure 4It is a cross-sectional view of the RPUF / Mxene@HNT-3 / DH flame retardant material prepared in Example 3 and the original rigid polyurethane (RPUF) in Comparative Example 1 after vertical combustion; Figure 5 The physical images (a1, b1), scanning electron microscope images (a2, b2) and Raman spectra (a3, b3) of the corresponding residues after combustion of the samples obtained in Comparative Example 1 and Comparative Example 2; wherein a represents Comparative Example 1 and b represents Comparative Example 2; Figure 6 The actual pictures (c1, d1), scanning electron microscope pictures (c2, d2) and Raman spectra (c3, d3) of the corresponding residues after combustion of the samples obtained in Comparative Example 3 and Example 3; wherein c represents Comparative Example 3 and d represents Example 3. DETAILED DESCRIPTION

[0009] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0010] The present invention provides a rigid polyurethane / Mxene@HNT / gel flame retardant material and a preparation method thereof. Mxene@HNT is first prepared, and then a double hydrogel is used to coat the Mxene@HNT on the surface of a rigid polyurethane (RPUF) by layer-by-layer coating, thereby forming a RPUF / Mxene@HNT / DH flame retardant system.

[0011] Among them, halloysite nanotubes (HNTs) are a natural tubular clay known for their high aspect ratio, high specific surface area, cavity structure, rich surface hydroxyl groups and environmental friendliness. HNTs are characterized by aluminum oxide octahedral sheets (Al-OH) inside and silicon oxide tetrahedral sheets (Si-O-Si) outside, which produce Al2O3 and SiO2 during thermal degradation and release a large amount of water, thereby extending the ignition time, increasing the residual carbon generation during combustion, and helping to achieve excellent flame retardant properties.

[0012] Mxene is a new type of three-dimensional nanomaterial with a high specific surface area and excellent thermal stability due to its stable and compact multilayer structure. This property allows Mxene to establish a dense flame retardant barrier at high temperatures, produce a "maze effect", extend the smoke flow path within the matrix, and thus provide effective smoke suppression. At the same time, Mxene undergoes thermal decomposition and is converted into TiO2 nanoparticles, which act as a catalyst to catalyze the carbon source to generate a dense carbon layer. Due to its special multilayer structure, wide surface area and excellent flame retardant properties, the present invention uses Mxene nanosheets as a three-dimensional porous flame retardant carrier to prepare an accordion-shaped structure Mxene@HNT as a flame retardant.

[0013] In the present invention, soybean oil-based polyol is used to prepare rigid polyurethane. The soybean oil-based polyol is prepared from soybean oil produced on the market. Compared with traditional petroleum-based polyols, it has a green protection effect on the environment. Specifically, the soybean oil-based polyol is prepared by ring-opening reaction of epoxidized soybean oil and distilled water. The specific preparation steps can refer to patent CN117384343A.

[0014] In a first aspect, the present invention provides a method for preparing a rigid polyurethane / Mxene@HNT / gel flame retardant material, comprising the following steps: S1, adding Mxene and halloysite nanotubes into water, dispersing them evenly to obtain a mixture A, and drying to obtain Mxene@HNT; S2, adding Mxene@HNT and calcium salt into an alcohol solvent and dispersing them evenly to obtain a mixture B; S3, coating the mixture B on the surface of the rigid polyurethane and drying to obtain RPUF / M@H; S4, immersing RPUF / M@H into a hydrogel solution to perform a gelation reaction, and after the reaction is completed, drying is performed to obtain a polyurethane / Mxene@HNT / gel flame retardant material.

[0015] Preferably, in step S1, the mass ratio of Mxene to halloysite nanotubes is (1.5-2.5):1.

[0016] Preferably, in step S1, deionized water is used; the ratio of Mxene to water is (0.4-0.6) g:10 mL.

[0017] Preferably, in step S1, the length of the halloysite nanotube (HNT) is 200 nm to 1000 nm; the size of the Mxene is 2 um to 5 um; the above sizes are combined to be more conducive to the preparation of a micro flame retardant material with an organ structure.

[0018] Preferably, in step S1, uniform dispersion is achieved by ultrasonic treatment and water bath stirring, and the ultrasonic treatment and water bath stirring are performed alternately and repeated 2 to 4 times; the ultrasonic treatment is performed under ice bath conditions, the power of the ultrasonic treatment is 50 to 150 W, and the time is 20 to 40 min; the temperature of the water bath stirring is 60 to 70° C., and the stirring time is 1.5 to 2.5 h.

[0019] Preferably, in step S1, the drying is performed by freeze drying.

[0020] Preferably, in step S1, the preparation step of Mxene includes: adding Ti3AlC2 powder to concentrated hydrochloric acid of LiF for etching, and then washing and freeze-drying to obtain Mxene; wherein the mass fraction of concentrated hydrochloric acid is 37%, and the ratio of Ti3AlC2, LiF and concentrated hydrochloric acid is (0.3-0.7) g: (0.5-1) g: 10 mL; the etching time is 30-40 h; washing is performed with distilled water until pH is ≥ 6. The present invention finally obtains multilayer Mxene after centrifugal peeling by freeze-drying, which has an accordion-like structure.

[0021] Preferably, in step S2, the mass ratio of Mxene@HNT to calcium salt is (1.5-2.5):1.

[0022] Preferably, in step S2, the alcohol solvent includes ethanol; the ratio of Mxene@HNT to the alcohol solvent is (0.08-0.12) g:5 mL.

[0023] Preferably, in step S2, uniform dispersion is achieved by ultrasound for 8 to 12 minutes.

[0024] Preferably, in step S3, the mixture B is coated on the surface of the rigid polyurethane for 1 to 3 times; the total coating amount of the mixture B on the surface of the rigid polyurethane is 5 to 20 mg / cm 2 .

[0025] Preferably, in step S3, the preparation step of the rigid polyurethane comprises: by weight, mixing 100 parts of soybean oil-based polyol (HSBP) with 0.5-1 parts of catalyst, 2-3 parts of stabilizer and 1-2 parts of deionized water to prepare a first mixture; then adding 125-135 parts of isocyanate and stirring evenly to obtain a second mixture; transferring the second mixture to a mold for foaming to obtain a rigid polyurethane. The RPUF of the present invention is obtained by the free rise method.

[0026] Further preferably, the catalyst includes stannous octoate or dibutyltin dilaurate; the stabilizer includes a silicone oil stabilizer, specifically AK-8805; the isocyanate is PMDI, and n(-NCO) / n(-OH) in PMDI = 1.1.

[0027] More preferably, after adding the isocyanate, stirring is performed at a speed of 800 to 1200 r / min for 8 to 12 s; during the foaming process, the temperature is 75 to 85° C. and the time is 18 to 24 h.

[0028] Preferably, in step S4, the hydrogel solution is a double hydrogel solution formed by dissolving sodium alginate and chitosan quaternary ammonium salt in acetic acid solution; in the hydrogel solution, the concentrations of sodium alginate and chitosan quaternary ammonium salt are 5-15 mg / mL respectively; the mass concentration of the acetic acid solution is 1.5-2.5%. In the present invention, the thickness of the gel layer is regulated by controlling the concentrations of sodium alginate and chitosan quaternary ammonium salt in the hydrogel solution; the chitosan quaternary ammonium salt used in the present invention has better water solubility, which is conducive to the formation of a hydrogel cross-linked network; the hydrogel cross-linked network of the present invention is a physical hydrogel, in which there are only ionic bonds and intermolecular hydrogen bonds in the network space, and there are no chemical bonds, which is conducive to improving the safety of the system.

[0029] Further preferably, the preparation step of the double hydrogel solution includes: adding sodium alginate to an acetic acid solution, stirring in a water bath at 80-90° C. for 8-12 min, then adding chitosan quaternary ammonium salt, and continuing to stir for 8-12 min to obtain a double hydrogel solution.

[0030] Preferably, in step S4, the gelation reaction time, i.e., the immersion time, is 3 to 8 minutes. The present invention controls the immersion time to ensure that the sodium alginate and Ca 2+ Full response.

[0031] In a second aspect, the present invention provides a rigid polyurethane / Mxene@HNT / gel flame retardant material obtained by the above preparation method, comprising a polyurethane, a solid flame retardant layer and a gel flame retardant layer arranged in sequence from the inside to the outside, wherein the solid flame retardant layer comprises Mxene@HNT.

[0032] The present invention provides two flame retardant layers, and the inner accordion-shaped flame retardant material Mxene@HNT and the outer double hydrogel have a synergistic effect, and compared with using them alone, they have better flame retardant effect after being prepared at the same time. The hydrogel layer is located on the outside, and while enhancing the flame retardant effect, the inner Mxene@HNT is wrapped on the polyurethane surface, making it difficult to fall off.

[0033] Preferably, the thickness of the gel flame retardant layer is 0.5 to 2 mm, and more preferably 1 mm. In the present invention, by providing the gel flame retardant layer, the final material has both good flame retardant properties and scratch resistance.

[0034] The present invention is further described in detail below through specific examples and comparative examples.

[0035] Example 1 (Rigid polyurethane flame retardant system RPUF / Mxene@HNT-1 / DH) The steps for preparing the soybean oil-based rigid polyurethane used in this embodiment include: A mixture was prepared by stirring 10 g of soybean oil-based polyol with 0.1 g of dibutyltin dilaurate, 0.3 g of AK-8805, and 0.15 g of deionized water. Subsequently, 12.5 g of PMDI [n(-NCO) / n(-OH) = 1.1] was quickly added and then stirred at 1000 r / min for 10 s. Finally, the mixture was quickly transferred to a mold and foamed in an oven at 85 °C for 18 h.

[0036] The preparation steps of Mxene used in this embodiment include: 0.5 g of Ti3AlC2 powder was gradually added to a centrifuge tube containing 0.78 g of LiF and 10 mL of hydrochloric acid, and then stirred for 36 h to obtain an etched product, which was thoroughly rinsed with distilled water at 40 °C until pH ≥ 6. Finally, multilayer Mxene after centrifugal exfoliation was obtained by freeze drying.

[0037] This embodiment provides a method for preparing a rigid polyurethane / Mxene@HNT / gel flame retardant material, comprising the following steps: S1, 1 g of Mxene and 0.5 g of halloysite nanotubes (HNT) were added to 10 mL of deionized water under ice bath conditions, and ultrasonicated at 100 W for 30 min; then stirred in a 65 ° C water bath for 2 h, and the above ultrasonic and water bath stirring steps were repeated 3 times and alternated to obtain a uniformly dispersed mixture A, which was freeze-dried to obtain Mxene@HNT; S2, 0.1 g of Mxene@HNT and 0.05 g of anhydrous calcium chloride powder were added to 5 mL of ethanol and ultrasonicated for 10 min to obtain mixture B; S3, coating the mixture B on the surface of a 12 cm × 1.3 cm × 1.2 cm rigid polyurethane (RPUF) surface, the coating amount of the mixture B on the rigid polyurethane surface is 5 mg / cm 2 , and then dried in an oven at 75 °C for 30 min to obtain RPUF / M@H; S4, preparation of double network hydrogel solution (DH): 1 g sodium alginate (SA) was added to 100 mL of 2% acetic acid solution, stirred in a water bath at 85 °C for 10 min, and then 1 g chitosan quaternary ammonium salt (QCS) was added, and stirring was continued for 10 min to obtain a hydrogel solution; RPUF / M@H was immersed in the hydrogel solution for 5 min to perform gelation reaction to ensure that the sodium alginate on the surface of RPUF and Ca 2+ After the reaction was complete, the composite material was extracted and placed in an oven at 65°C for 30 minutes to obtain a polyurethane / Mxene@HNT / gel flame retardant material, in which the gel flame retardant layer formed was about 1 mm thick, recorded as RPUF / Mxene@HNT-1 / DH.

[0038] Example 2 The only difference from Example 1 is that step S3 is adjusted to repeat the steps of coating and drying the mixture B once more, and the total coating amount of the mixture B on the hard polyurethane surface is 10 mg / cm 2 , other steps and conditions are the same as those in Example 1; the obtained polyurethane / Mxene@HNT / gel flame retardant material is recorded as RPUF / Mxene@HNT-2 / DH.

[0039] Example 3 The only difference from Example 1 is that step S3 is adjusted to repeat the steps of coating and drying the mixture B twice, and the total coating amount of the mixture B on the hard polyurethane surface is 15 mg / cm 2 , other steps and conditions are the same as those in Example 1; the obtained polyurethane / Mxene@HNT / gel flame retardant material is recorded as RPUF / Mxene@HNT-3 / DH.

[0040] Comparative Example 1 Blank control group: soybean oil-based rigid polyurethane prepared in Example 1.

[0041] Comparative Example 2 (Hard polyurethane loaded dual hydrogel DH) The difference from Example 1 is that: Mxene@HNT is removed to obtain a rigid polyurethane-loaded dual hydrogel DH material, which is denoted as RPUF / DH. The specific preparation steps include: The RPUF was immersed in 10 mg / mL calcium chloride ethanol solution and the hydrogel solution prepared in Example 1 for 5 min in turn to ensure that the sodium alginate on the surface of the RPUF was 2+ Finally, the composite material was extracted and placed in an oven at 65°C for 30 minutes to obtain RPUF / DH, with a DH thickness of about 1 mm.

[0042] Comparative Example 3 (Hard Polyurethane Loaded with Mxene@HNT-3) The only difference from Example 3 is that no anhydrous calcium chloride powder is added to mixture B (i.e., 0.1 g of Mxene@HNT is mixed with 5 mL of ethanol and ultrasonicated for 10 min to obtain mixture B), and step S4 is removed. The other steps and conditions are the same as those in Example 3 to obtain RPUF / Mxene@HNT-3.

[0043] Performance Testing 1. Scanning the Mxene@HNT obtained in Example 1 by electron microscope, the results are as follows Figure 1 As shown, Mxene has an accordion-like structure, and HNT nanoparticles are embedded between the layers and on the surface of the accordion-like structure.

[0044] pass Figure 1 Scanning electron microscope photos, combined with Figure 2 The energy spectrum scan confirmed that the Mxene@HNT structure was successfully prepared and the HNT was successfully embedded in the Mxene interlayer.

[0045] 2. Limiting oxygen index test (LOI): Different samples were tested using a limiting oxygen index tester (FTT0077, UK). All tests were based on ASTM D2863-97.

[0046] Vertical burning test: UL-94 vertical burning test was performed on different samples using a vertical burning apparatus (model CFZ-2, Jiangning, China). The sample size was 125 × 13 × 10 mm. 3 , 5 parallel samples were tested in each group to obtain the average data.

[0047] Microstructure characterization: Infrared spectroscopy (Thermo Scientific Nicolet iS20, USA) was used in the wave number range of 4000 to 500 cm -1 FTIR spectra of the samples were recorded in KBr slices.

[0048] Carbonization degree test: A laser confocal Raman spectrometer (Horiba LabRAM HR Evolution, Japan) was used to obtain the Raman spectrum of the residual carbon after combustion, with a wave number range of 1800-500 cm -1 , the excitation wavelength is 514 nm.

[0049] The performance tests were performed on the products obtained in the above Examples 1-3 and Comparative Examples 1-3, and the results are shown in Table 1 below.

[0050] Table 1 Flame retardant properties of different embodiments:

[0051] in, a t1 and a t2: autonomous combustion time after the fire source is removed 10s after the first and second combustion; b BC: burn to clamp; c NR: Not Rated.

[0052] As can be seen from Table 1, the LOI of Comparative Example 1 is relatively low, at 18.6%, indicating that its flame retardancy is poor and needs to be further enhanced. Compared with Comparative Example 1, Comparative Example 2 can improve the flame retardancy by adding DH only to the outer layer, and the LOI increases to 21.9%.

[0053] In addition, it can be seen from the comparison between Comparative Example 2, Comparative Example 3 and Example 3 that as the number of inner M@H coating layers increases from 0 to 3, and a double hydrogel layer is set on the outer layer, the LOI of the rigid polyurethane / Mxene@HNT / gel flame retardant material obtained by the present invention gradually increases from 21.9% in Comparative Example 2 to 30.5%, indicating that the synergistic flame retardant effect of the inner and outer flame retardant layers is good. Although Comparative Example 3 also achieves a relatively excellent flame retardant effect, the solid flame retardant layer on its surface is easy to fall off, so the present invention needs to wrap another gel layer on the outermost layer to prevent the solid flame retardant layer from falling off, while achieving a synergistic flame retardant effect.

[0054] In addition, the actual picture of UL-94 test is as follows Figure 3 As shown, group (a) is comparative example 1, and group (b) is example 3; comparative example 1 was ignited within 2 seconds after exposure, the flame spread rapidly, and a large amount of black smoke appeared. The entire combustion process lasted for 21 seconds, resulting in complete combustion of the sponge and structural deformation. In contrast, after the flame approached, example 3 showed delayed ignition within 10 seconds, and even if ignited, only a small amount of black smoke was emitted, which was quickly extinguished after the flame was removed. In addition, the flammability level of example 3 transitioned from "no level" of comparative example 1 to V0 (the highest flammability level).

[0055] The material cross-section analysis after burning for 10 seconds in the UL-94 test is as follows: Figure 4 As shown, the internal combustion and carbonization of Comparative Example 1 are obvious, resulting in severe collapse and deformation. In contrast, the surface layer of Example 3 presents a carbon protective layer, while the internal structure is not affected, indicating that the surface layer has effective flame retardancy and provides strong internal protection.

[0056] Cone calorimeter was used to test the safety and fire resistance of each embodiment and comparative example. The flame degree further simulated the real fire situation, and the gas generation and heat release were further analyzed. The residuals of each representative sample after burning for 400 seconds were analyzed by scanning electron microscopy and Raman spectroscopy. The results are as follows: Figure 5 and Figure 6As shown, a1 represents the actual image of the residue after burning of comparative example 1, a2 is the scanning electron microscope image of the residue after burning of comparative example 1, and a3 is the Raman spectrum of the residue after burning of comparative example 1; the other figures are similar, b represents comparative example 2, c represents comparative example 3, and d represents example 3. It can be seen that the flame retardant system is gradually improved in the process from comparative example 1-3 to example 3, and the flame retardant effect exhibited is also gradually improved. The surface of the rigid polyurethane residue changes from a small amount of carbon residue and a thin carbon layer with many cracks in comparative example 1 (not enough to hinder the transfer of heat and smoke) to a crack-free, smooth, and dense carbon residue surface in example 3, and the flame retardant effect is further improved. Raman spectroscopy is then used to evaluate the degree of graphitization of the residual carbon layer after CCT (cone calorimeter). The ratio of the D peak area to the G peak area (I D / I G ) is an important indicator of graphitization strength, I D / I G The lower the value, the higher the degree of graphitization, indicating that the heat and smoke protection effect is better. D / I G The values ​​are 3.224, 3.028, 2.580, and 1.620, respectively. It is worth noting that the scaffold of Example 3 exhibits the lowest I D / I G ratio and the highest degree of graphitization.

[0057] In summary, the present invention provides a rigid polyurethane / Mxene@HNT / gel flame retardant material and a preparation method thereof. The present invention uses vegetable oil as a polyol to prepare a rigid polyurethane foam (RPUF), which meets the requirements of green environmental protection. However, improving its flame retardancy is crucial to solving the safety issues of its widespread application in various commercial sectors. The present invention successfully prepares Mxene@HNT, and then uses a double hydrogel to coat Mxene@HNT on the surface of rigid polyurethane (RPUF) by layer-by-layer coating, thereby forming a RPUF / Mxene@HNT / gel flame retardant material; the double hydrogel in the present invention is cross-linked by sodium alginate and chitosan quaternary ammonium salt, and sodium alginate and chitosan quaternary ammonium salt are natural biopolymers with environmental friendliness and cost-effectiveness. Halloysite nanotubes (HNT) and Mxene are substances with good flame retardant properties. In the present invention, Mxene@HNT with an accordion-like structure is prepared, which increases the path for heat and smoke diffusion and enhances the flame retardant effect of the system; the double network in the double hydrogel in the present invention refers to sodium alginate and Ca 2+The metal ion network formed by cross-linking is formed by the physical cross-linking network of positive and negative ions formed by sodium alginate and chitosan quaternary ammonium salt in aqueous solution. The double hydrogel coating effectively solves the problems of easy leakage of flame retardant materials and short effective time in surface coating flame retardancy, providing a new idea for the green production and surface flame retardancy of rigid polyurethane.

[0058] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a rigid polyurethane / Mxene@HNT / gel flame retardant material, It is characterized in that The following steps are involved: S1, adding Mxene and halloysite nanotubes into water, dispersing them evenly to obtain a mixture A, and drying to obtain Mxene@HNT; S2, adding Mxene@HNT and calcium salt into an alcohol solvent and dispersing them evenly to obtain a mixture B; S3, coating the mixture B on the surface of the rigid polyurethane and drying to obtain RPUF / M@H; S4, immersing RPUF / M@H into a hydrogel solution to perform a gelation reaction, and after the reaction is completed, drying is performed to obtain a polyurethane / Mxene@HNT / gel flame retardant material.

2. The method for preparing the rigid polyurethane / Mxene@HNT / gel flame retardant material according to claim 1, It is characterized in that In step S1, the mass ratio of the Mxene to the halloysite nanotubes is (1.5-2.5):

1.

3. The preparation method of the rigid polyurethane / Mxene@HNT / gel flame retardant material according to claim 1, It is characterized in that In step S1, the length of the halloysite nanotubes is 200 nm to 1000 nm; the size of the Mxene is 2 um to 5 um; The uniform dispersion in step S1 is achieved by ultrasonic treatment and water bath stirring, and the ultrasonic treatment and water bath stirring are performed alternately and repeated 2 to 4 times; the ultrasonic treatment is performed under ice bath conditions, the power of the ultrasonic treatment is 50 to 150 W, and the time is 20 to 40 minutes; the temperature of the water bath stirring is 60 to 70° C., and the stirring time is 1.5 to 2.5 hours.

4. The method for preparing the rigid polyurethane / Mxene@HNT / gel flame retardant material according to claim 1, It is characterized in that In step S1, the preparation steps of Mxene include: 3 AlC 2 The powder was added to LiF concentrated hydrochloric acid for etching, and then washed and freeze-dried to obtain Mxene; the mass fraction of concentrated hydrochloric acid was 37%, Ti 3 AlC 2 , LiF and concentrated hydrochloric acid ratio is (0.3 ~ 0.7) g: (0.5 ~ 1) g: 10mL; etching time is 30 ~ 40h.

5. The method for preparing the rigid polyurethane / Mxene@HNT / gel flame retardant material according to claim 1, It is characterized in that In step S2, the mass ratio of Mxene@HNT to calcium salt is (1.5-2.5):1; The alcohol solvent includes ethanol; the ratio of Mxene@HNT to the alcohol solvent is (0.08-0.12) g:5 mL.

6. The method for preparing the rigid polyurethane / Mxene@HNT / gel flame retardant material according to claim 1, It is characterized in that In step S3, the mixture B is coated on the surface of the rigid polyurethane for 1 to 3 times; the total coating amount of the mixture B on the surface of the rigid polyurethane is 5 to 20 mg / cm 2 .

7. The method for preparing the rigid polyurethane / Mxene@HNT / gel flame retardant material according to claim 1, It is characterized in that In step S3, the preparation steps of rigid polyurethane include: mixing 100 parts of soybean oil-based polyol (HSBP) with 0.5-1 parts of catalyst, 2-3 parts of stabilizer and 1-2 parts of deionized water by mass to prepare a first mixture; then adding 125-135 parts of isocyanate and stirring evenly to obtain a second mixture; transferring the second mixture to a mold for foaming to obtain rigid polyurethane.

8. The method for preparing the rigid polyurethane / Mxene@HNT / gel flame retardant material according to claim 7, It is characterized in that The catalyst includes stannous octoate or dibutyltin dilaurate; the stabilizer includes a silicone oil stabilizer, specifically AK-8805; the isocyanate uses PMDI; The stirring is performed at a speed of 800 to 1200 r / min for 8 to 12 seconds; The foaming temperature is 75-85° C. and the foaming time is 18-24 h.

9. The method for preparing the rigid polyurethane / Mxene@HNT / gel flame retardant material according to claim 1, It is characterized in that In step S4, the hydrogel solution is a double hydrogel solution formed by dissolving sodium alginate and chitosan quaternary ammonium salt in acetic acid solution; in the hydrogel solution, the concentrations of sodium alginate and chitosan quaternary ammonium salt are 5-15 mg / mL respectively; the mass concentration of the acetic acid solution is 1.5-2.5%; The gelation reaction time is 3 to 8 minutes.

10. The rigid polyurethane / Mxene@HNT / gel flame retardant material prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Mxene nano hybrid material and application thereof in flame-retardant foaming material

    CN119978549A

  • A type of Mxene nanohybrid material and its application in flame-retardant foam materials

    CN119978549B