Epoxy casting resin for 110kV dry-type transformer, preparation method of epoxy casting resin and transformer

By combining modified epoxy resin and anhydride curing agent, combined with two-particle-size composite inorganic filler and environmentally friendly flame retardant, the problem of insufficient thermal conductivity and flame retardant of epoxy cast resin is solved, and 110kV drying is significantly improved The heat dissipation and crack resistance of the type transformer extends the service life and improves the stability of high-temperature operation.

CN119039737APending Publication Date: 2024-11-29NANTONG GAOMENG NEW MATERIAL
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411318456.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The epoxy cast resin of the existing 110kV dry transformer has poor thermal conductivity, resulting in poor heat dissipation, which shortens the service life of the equipment. At the same time, its flame retardant and crack resistance are insufficient, making it difficult to meet the stability requirements of high-temperature operation.

Method used

Using modified epoxy resin and modified anhydride curing agent, the resin is improved by combining inorganic fillers and environmentally friendly flame retardants by two-particle size, and the resin is enhanced through specific formulations and processes. Viscosity and filling effect improve crack resistance.

Benefits of technology

It significantly improves the heat dissipation effect and crack resistance of the dry transformer, extends the service life, meets the stability and flame retardant requirements of high-temperature operation, and improves the heat resistance and mechanical properties of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005052888060000141
    Figure BDA0005052888060000141
  • Figure BDA0005052888060000142
    Figure BDA0005052888060000142
  • Figure BDA0005052888060000151
    Figure BDA0005052888060000151
Patent Text Reader

Abstract

The invention discloses epoxy casting resin for a 110kV dry-type transformer, a preparation method of the epoxy casting resin and the transformer. The resin comprises modified epoxy resin and a modified anhydride curing agent in a mass ratio of 100: 100, the modified epoxy resin comprises the following components in parts by mass: 100 parts of epoxy resin, 5-15 parts of a toughening agent, 0.2 part of a dispersing agent, 0.05 part of a defoaming agent, 7-25 parts of an environment-friendly flame retardant and 190-210 parts of a first double-particle-size compound inorganic filler; the modified anhydride curing agent comprises the following components in parts by mass: 100 parts of anhydride, 5-10 parts of a toughening agent, 0.1-0.5 part of a curing accelerator and 225-265 parts of second double-particle-size compound inorganic filler. The epoxy casting resin is low in viscosity, high in filling and long in operable time, a transformer cast by using the epoxy casting resin has excellent heat resistance, heat dissipation performance, cracking resistance, mechanical performance and flame retardant performance, the high-temperature operation reliability of the dry type transformer is improved, and the service life of the dry type transformer is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of epoxy casting resins, and in particular to an epoxy casting resin for a 110kV dry-type transformer and a preparation method thereof. Background Art

[0002] With the rapid development of China's economy, the scale of urbanization is getting larger and larger, and the power consumption of industrial production and residents has also increased sharply. The demand for 110kV substations for nearby power supply and transformation has increased. However, at present, transformers of this level are still mainly oil-immersed, but the mineral oil used in oil-immersed transformers is flammable, which limits its use in places with higher fire protection levels. In addition, it needs to be equipped with large and complete fire prevention and fire extinguishing facilities, and its ability to resist external short-circuit faults is poor; therefore, the demand for oil-free substations has increased significantly. The key basis for oil-free 110kV power stations is to change oil transformers to dry transformers. At present, there are three options for insulation structures that can be used for 110kV dry transformers, namely epoxy cast transformers, SF6 gas insulated transformers and cable transformers. 110kV SF6 gas transformers are used in small quantities in first-tier cities, but they are expensive, complex in structure, poor in heat dissipation capacity, and cumbersome in maintenance. At the same time, although SF6 gas is a low-toxic gas, if leaked, the colorless and odorless SF6 will suffocate the human body, and there are environmental protection and safety issues, which also limits its development. In addition, since dry-type transformers are oil-free, they require fewer accessories, no oil storage cabinets, safety airways, throttles and other components, and no sealing problems, so the workload of dry-type transformer maintenance and overhaul is very small. Due to the above advantages of dry-type transformers, the demand has increased rapidly. In industrially developed countries such as the United States, Japan and Germany, dry-type transformers have accounted for more than 20% of the output of distribution transformers, and some countries even account for about 50%. The output of dry-type transformers in my country has accounted for more than 10% of distribution transformers. It can be foreseen that with the increase in the demand for fire protection in today's society, dry-type transformers will still have a lot of room for development. Comprehensively comparing the advantages and disadvantages of the three dry-type transformers, for my country, the epoxy resin cast dry-type transformer is undoubtedly the best.

[0003] Dry-type transformers can be divided into impregnated dry-type transformers and epoxy resin dry-type transformers according to the manufacturing process. Resin dry-type transformers are further divided into wrapped resin dry-type transformers and cast resin dry-type transformers. Impregnated dry-type transformers appeared earlier, but due to their low insulation level, poor short-circuit resistance, and poor moisture and dust resistance of the windings, they have gradually withdrawn from the market. Wrapped resin dry-type transformers have poor reliability and large size, and their application occasions are greatly limited. At present, the products on the market are mainly cast resin dry-type transformers, which are widely used in substations and some places with high fire protection requirements due to their good insulation level, fire and moisture resistance, and small size.

[0004] With the continuous increase in the capacity of dry-type transformers, the capacity has increased from 35kV to 110kV, and the heat dissipation problem has become prominent. Overheating of the transformer winding will accelerate the aging of the insulation, thereby shortening the service life of the dry-type transformer. Data show that for every 7°C increase in the winding temperature of power equipment such as transformers and motors, their expected life will be shortened by half. However, the thermal conductivity of the epoxy resin body is poor, which seriously restricts the improvement of the heat dissipation capacity of the dry-type transformer; at the same time, the epoxy casting resin used in the dry-type transformer will not extinguish itself after the high temperature causes a fire during operation, so it is very necessary to improve the flame retardant properties of the epoxy casting resin while improving its thermal conductivity. This puts higher requirements on the heat resistance, thermal conductivity, flame retardant properties and crack resistance of the casting resin of the 110kV dry-type transformer.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to provide an epoxy casting resin for a 110kV dry-type transformer, a preparation method thereof and a transformer, which has the characteristics of high filling, low viscosity, long operability time, good thermal conductivity and flame retardancy, thereby solving the above-mentioned technical problems existing in the prior art.

[0007] The objective of the present invention is achieved through the following technical solutions:

[0008] An epoxy casting resin for a 110kV dry-type transformer comprises: a modified epoxy resin and a modified anhydride curing agent in a mass ratio of 100:100; wherein:

[0009] The modified epoxy resin is prepared from the following components in parts by mass, including: 100 parts of epoxy resin, 5 to 15 parts of a first toughening agent, 0.2 parts of a dispersant, 0.05 parts of a defoaming agent, 7 to 25 parts of an environmentally friendly flame retardant, and 190 to 210 parts of a first double-particle-size composite inorganic filler;

[0010] The modified acid anhydride curing agent is prepared from the following components in parts by mass, including: 100 parts of acid anhydride, 5 to 10 parts of a second toughening agent, 0.1 to 0.5 parts of a curing accelerator and 225 to 265 parts of a second double-particle-size composite inorganic filler.

[0011] Preferably, in the above resin, the first double-particle size composite inorganic filler and the second double-particle size composite inorganic filler are both composed of a large-particle size filler treated with a silane coupling agent for surface activation and a small-particle size filler treated with a silane coupling agent for surface activation, which are compounded in a mass ratio of 100:5 to 11, wherein the average particle size D50 of the large-particle size filler is 20 to 30 μm, and the average particle size D50 of the small-particle size filler is 2 to 5 μm.

[0012] Preferably, in the above resin, the large particle size filler is an inorganic filler in an angular shape or an inorganic filler in a spherical shape;

[0013] The small particle size filler is an inorganic filler in an angular shape or an inorganic filler in a spherical shape.

[0014] Preferably, in the above resin, in the first double-particle size composite inorganic filler and the second double-particle size composite inorganic filler, the large-particle size filler and the small-particle size filler are any one or more of silicon dioxide, aluminum oxide, magnesium oxide, zinc oxide, boron nitride, and aluminum nitride.

[0015] Preferably, in the above resin, in the modified epoxy resin, the epoxy resin is any one or more of bisphenol epoxy resin, novolac epoxy resin, and alicyclic epoxy resin;

[0016] The dispersant and defoamer are both silicone defoamers;

[0017] The first toughening agent is any one or more of CTBN-modified epoxy resin, NBR-modified epoxy resin, silicon-modified epoxy resin, and core-shell structure toughening agent.

[0018] The environmentally friendly flame retardant is a non-halogen organic flame retardant containing flame retardant elements such as phosphorus, nitrogen, and silicon;

[0019] Preferably, in the above resin, the environmentally friendly flame retardant is any one or more of diethyl aluminum phosphinate, 1,3-phenylene (2,6-xylyl) tetraphosphate, hexaphenoxy cyclotriphosphazene, ammonium polyphosphate, melamine cyanurate, triphenyl phosphate, tricresyl phosphate, toluene diphenyl phosphate, and modified cage-type polysilsesquioxane;

[0020] Preferably, among the above resins, the bisphenol epoxy resin is at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, and hydrogenated bisphenol A epoxy resin;

[0021] The novolac epoxy resin is at least one of phenol novolac epoxy resin, o-cresol novolac epoxy resin, dicyclopentadiene phenol epoxy resin, biphenyl phenol epoxy resin, trifunctional novolac epoxy resin, and tetrafunctional novolac epoxy resin;

[0022] The alicyclic epoxy resin is at least one of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, bis((3,4-epoxycyclohexyl)methyl)adipate, 4-vinyl-1-cyclohexene diepoxide, 1,4-cyclohexanedimethanol bis(3,4-epoxycyclohexanecarboxylate), (3,4,3',4'-diepoxy)dicyclohexane, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, 4,5-epoxytetrahydrophthalic acid diglycidyl ester, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.

[0023] Preferably, in the above resin, in the modified acid anhydride curing agent, the acid anhydride is any one or more of tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, nadic anhydride, and methylnadic anhydride;

[0024] The curing accelerator is a tertiary amine accelerator;

[0025] The second toughening agent is any one or more of CTBN-modified epoxy resin, NBR-modified epoxy resin, silicon-modified epoxy resin, and core-shell structure toughening agent.

[0026] A method for preparing the epoxy casting resin for the 110kV dry-type transformer of the present invention comprises the following steps:

[0027] The modified epoxy resin and the modified anhydride curing agent are prepared respectively, wherein:

[0028] The modified epoxy resin is prepared, comprising: taking raw materials according to the formula of the modified epoxy resin of the present invention, adding the epoxy resin and the first toughening agent in the raw materials into a stirring container, stirring at a temperature of 60 to 80° C. for 20 minutes, then adding a dispersant and a defoamer, stirring for 5 minutes, then adding an environmentally friendly flame retardant and a first double-particle-size composite inorganic filler in sequence under stirring, raising the temperature to 90 to 100° C., stirring for 30 to 60 minutes, starting a thin film vacuum degassing under stirring, stirring for 90 to 120 minutes under the condition of a vacuum degree of less than 133 Pa, stopping stirring after completion and maintaining the vacuum for 10 minutes, finally breaking the vacuum, filtering the material, and obtaining the modified epoxy resin;

[0029] The modified anhydride curing agent is prepared, comprising: taking raw materials according to the formula of the modified anhydride curing agent of the present invention, adding the anhydride, the second toughening agent and the curing accelerator in the raw materials into a stirring container, stirring at a temperature of 60-80° C. for 20 minutes, then adding the second double-particle size composite inorganic filler under stirring and maintaining the temperature at 60-80° C., starting the film vacuum degassing under stirring, stirring for 90-120 minutes under the condition of a vacuum degree of less than 133 Pa, stopping the stirring after completion and maintaining the vacuum for 10 minutes, finally breaking the vacuum, filtering the material, and obtaining the modified anhydride curing agent;

[0030] The prepared modified epoxy resin and the modified acid anhydride curing agent are mixed in a mass ratio of 100:100 to prepare the epoxy casting resin for 110kV dry-type transformer.

[0031] A 110kV dry-type transformer is a 110kV dry-type transformer cast by using the 110kV dry-type transformer and epoxy casting resin.

[0032] Preferably, in the above transformer, the 110kV dry-type transformer epoxy casting resin of the present invention is cast in the following manner to form a 110kV dry-type transformer, including:

[0033] Place the coil and mold in a 120℃ oven for preheating for 2 hours, then transfer them to a vacuum casting tank for degassing and dehumidification under the conditions of coil temperature of 100-120℃ and vacuum pressure less than 133Pa; at the same time, transfer the modified epoxy resin and modified anhydride curing agent that make up the epoxy casting resin for 110kV dry-type transformer into a static mixer, control the temperature of the mixture at 90℃, stir it thoroughly, degas and set it aside for use; after completing the preheating and dehumidification of the coil and mold, keep the temperature of the coil and mold at 90-110℃ and the discharge temperature of the static mixer at 150℃. The dry-type transformer is poured at 80-90°C, the vacuum pressure of the pouring tank is maintained at 250-400Pa, and the pouring is controlled to be completed within 180min; after the pouring is completed, the poured mold is transferred to the oven and the curing conditions are set to 100°C / 2hr+80°C / 8hr+100°C / 4hr+140°C / 8hr. After the curing is completed, the mold is demoulded at a temperature of 100-110°C, and then the cured transformer is returned to the oven for cooling, so that the epoxy resin cast 110kV dry-type transformer is made.

[0034] Compared with the prior art, the epoxy casting resin for 110kV dry-type transformer and its preparation method and transformer provided by the present invention have the following beneficial effects:

[0035] The two-component epoxy casting resin is composed of modified epoxy resin and modified anhydride curing agent. Since the modified epoxy resin and the modified anhydride curing agent both use double-particle-size compounded inorganic fillers, the viscosity can be lower and the filling ratio can be higher through the design of large and small particle size grading. The lower viscosity of the glue also has better wettability and permeability to the winding, and can better fill and avoid internal gaps, avoiding a lower partial discharge of the transformer winding. The higher inorganic filler filling ratio will make the thermal expansion coefficient and shrinkage rate of the cured product smaller, and improve the anti-cracking performance of the transformer; the double-particle-size compounded inorganic filler is also conducive to the establishment of a heat conduction path, which will make the heat dissipation effect better, reduce the operating temperature of the transformer, improve the operating stability of the transformer at high temperature and extend its service life; the addition of environmentally friendly halogen-free flame retardant effectively improves the shortcomings of the existing red phosphorus flame retardant, such as easy water absorption, poor compatibility with resin, deterioration of heat resistance, mechanical properties and its own dark color limiting application, and also avoids the shortcomings of small molecular weight phosphate liquid flame retardant that is easy to release from the surface of the product and affect the product performance. DETAILED DESCRIPTION

[0036] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the specific content of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, which does not constitute a limitation of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0037] First, the terms that may be used in this article are explained as follows:

[0038] The term “and / or” means that either or both of them can be realized at the same time. For example, X and / or Y means both “X” or “Y” and “X and Y”.

[0039] The terms "include", "comprises", "contains", "has" or other descriptions with similar semantics should be interpreted as non-exclusive inclusion. For example, including certain technical feature elements (such as raw materials, components, ingredients, carriers, dosage forms, materials, dimensions, parts, components, mechanisms, devices, steps, procedures, methods, reaction conditions, processing conditions, parameters, algorithms, signals, data, products or products, etc.) should be interpreted as including not only certain technical feature elements explicitly listed, but also other technical feature elements known in the art that are not explicitly listed.

[0040] The term "consisting of..." means excluding any technical feature elements not explicitly listed. If this term is used in a claim, it will make the claim closed, so that it does not contain technical feature elements other than the technical feature elements explicitly listed, except for the conventional impurities related to them. If this term only appears in a clause of a claim, it only limits the elements explicitly listed in the clause, and the elements recorded in other clauses are not excluded from the overall claim.

[0041] The term "parts by mass" refers to the mass ratio relationship between multiple components. For example, if it is described that component X is x parts by mass and component Y is y parts by mass, then the mass ratio of component X to component Y is x:y. 1 part by mass can represent any mass, for example, 1 part by mass can be represented as 1 kg or 3.1415926 kg. The sum of the parts by mass of all components is not necessarily 100 parts, but can be greater than 100 parts, less than 100 parts or equal to 100 parts. Unless otherwise specified, the parts, proportions and percentages described herein are all measured by mass.

[0042] When concentration, temperature, pressure, size or other parameters are expressed in the form of a numerical range, the numerical range should be understood to specifically disclose all ranges formed by the pairing of any upper limit, lower limit, and preferred value in the numerical range, regardless of whether the range is explicitly stated; for example, if a numerical range of "2 to 8" is stated, the numerical range should be interpreted as including ranges such as "2 to 7", "2 to 6", "5 to 7", "3 to 4 and 6 to 7", "3 to 5 and 7", "2 and 5 to 7", etc. Unless otherwise specified, the numerical ranges stated herein include both their end values ​​and all integers and fractions within the numerical range.

[0043] The scheme provided by the present invention is described in detail below. The contents not described in detail in the embodiments of the present invention belong to the prior art known to professionals in the field. If the specific conditions are not specified in the embodiments of the present invention, they are carried out according to the conventional conditions in the field or the conditions recommended by the manufacturer. If the manufacturers are not specified in the reagents or instruments used in the embodiments of the present invention, they are all conventional products that can be purchased commercially.

[0044] The embodiment of the present invention provides an epoxy casting resin for a 110kV dry-type transformer, comprising: a modified epoxy resin and a modified anhydride curing agent in a mass ratio of 100:100;

[0045] Wherein, the modified epoxy resin comprises the following components in parts by mass:

[0046] 100 parts of epoxy resin, 5 to 15 parts of a first toughening agent, 0.2 parts of a dispersant, 0.05 parts of a defoaming agent, 7 to 25 parts of an environmentally friendly flame retardant, and 190 to 210 parts of a first double-particle-size compound inorganic filler;

[0047] The modified acid anhydride curing agent comprises the following components: 100 parts of acid anhydride, 5 to 10 parts of a second toughening agent, 0.1 to 0.5 parts of a curing accelerator, and 225 to 265 parts of a second double-particle-size composite inorganic filler.

[0048] Furthermore, in the modified epoxy resin, the epoxy resin is one or more of bisphenol epoxy resin, novolac epoxy resin and alicyclic epoxy resin; the bisphenol epoxy resin is preferably one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydrogenated bisphenol A epoxy resin; the novolac epoxy resin is preferably one or more of phenol novolac epoxy resin, o-cresol novolac epoxy resin, dicyclopentadiene phenol epoxy resin, biphenyl phenol epoxy resin, trifunctional novolac epoxy resin and tetrafunctional novolac epoxy resin; the alicyclic epoxy resin is preferably one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydrogenated bisphenol A epoxy resin; the novolac epoxy resin is preferably one or more of phenol novolac epoxy resin, o-cresol novolac epoxy resin, dicyclopentadiene phenol epoxy resin, biphenyl phenol epoxy resin, trifunctional novolac epoxy resin and tetrafunctional novolac epoxy resin; The epoxy resin is preferably one or more of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, bis((3,4-epoxycyclohexyl)methyl)adipate, 4-vinyl-1-cyclohexene diepoxide, 1,4-cyclohexanedimethanol bis(3,4-epoxycyclohexanecarboxylate), (3,4,3',4'-diepoxy)bicyclohexane, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, 4,5-epoxytetrahydrophthalic acid diglycidyl ester, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.

[0049] Furthermore, in the modified epoxy resin, the dispersant is an organosilicon dispersant; the defoaming agents are all organosilicon defoaming agents;

[0050] The first toughening agent is one or more of CTBN-modified epoxy resin, NBR-modified epoxy resin, silicon-modified epoxy resin or a core-shell structure toughening agent.

[0051] The environmentally friendly flame retardant is a non-halogen organic flame retardant containing flame retardant elements such as phosphorus, nitrogen, and silicon;

[0052] Furthermore, in the above-mentioned modified epoxy resin, the environmentally friendly flame retardant is one or more of diethyl aluminum phosphite, 1,3-phenylene (2,6-xylyl) tetraphosphate, hexaphenoxy cyclotriphosphazene, ammonium polyphosphate, melamine cyanurate, triphenyl phosphate, tricresyl phosphate, toluene diphenyl phosphate, and modified cage-type polysilsesquioxane.

[0053] Furthermore, in the modified epoxy resin, the first dual-particle size composite inorganic filler is composed of a large-particle size filler treated with a silane coupling agent and a small-particle size filler treated with a silane coupling agent in a mass ratio of 100:5-11; wherein the small-particle size filler is angular or spherical, and the average particle size D50 is 2-5 μm; the large-particle size filler is angular or spherical, and the average particle size D50 is 20-30 μm. Preferably, the inorganic filler used for the large-particle size filler and the small-particle size filler is one or more of silicon micropowder (silicon dioxide), aluminum oxide, magnesium oxide, zinc oxide, boron nitride, and aluminum nitride. The inorganic filler designed with different particle size grading and surface modified with silane coupling agent can achieve lower viscosity and higher filling ratio. The lower viscosity of the glue also has better wettability and permeability to the winding, which can better fill the winding densely to avoid internal gaps and avoid a lower local discharge in the transformer winding. A higher filling ratio of inorganic filler will make the thermal expansion coefficient and shrinkage rate of the cured product lower, which will improve the anti-cracking performance of the transformer. The addition of environmentally friendly halogen-free flame retardant ensures that the casting resin will not produce toxic gases such as hydrogen halide of the halogen flame retardant even when it is burning, avoiding harm to the human body.

[0054] The use of alumina with good thermal conductivity and the combination of angular and spherical shapes make the filling denser and more sufficient, which is conducive to the establishment of a thermal conduction path, resulting in better heat dissipation, reducing the operating temperature of the transformer, improving the operating stability of the transformer at high temperatures and extending its service life.

[0055] Furthermore, in the above-mentioned acid anhydride curing agent, the acid anhydride is one or more of tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, nadic anhydride, and methylnadic anhydride; the acid anhydride is preferably one or more of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and methylnadic anhydride.

[0056] The curing accelerator is a tertiary amine accelerator, specifically one or more of 2-dimethylaminomethylphenol, 2,4,6-tris(dimethylaminomethyl)phenol, and benzyldimethylamine.

[0057] The embodiment of the present invention also provides a method for preparing the above-mentioned epoxy casting resin for 110kV dry-type transformer, comprising the following steps:

[0058] The modified epoxy resin and the modified anhydride curing agent are prepared respectively, wherein:

[0059] The modified epoxy resin is prepared, comprising: taking various raw materials according to the above-mentioned modified epoxy resin formula, adding the epoxy resin and the first toughening agent in the raw materials into a stirring container, stirring at a temperature of 60 to 80° C. for 20 minutes, then adding a dispersant and a defoamer, stirring for 5 minutes, then adding an environmentally friendly flame retardant and a first double-particle-size composite inorganic filler in sequence under stirring and raising the temperature to 90 to 100° C., stirring for 30 to 60 minutes, starting a thin film vacuum degassing under stirring, stirring for 90 to 120 minutes under the condition of a vacuum degree of less than 133 Pa, stopping stirring after completion and maintaining the vacuum for 10 minutes, finally breaking the vacuum, filtering the material, and obtaining the modified epoxy resin;

[0060] The modified anhydride curing agent is prepared, comprising: taking raw materials according to the formula of the modified anhydride curing agent, adding the anhydride, the second toughening agent and the curing accelerator in the raw materials into a stirring container, stirring at a temperature of 60 to 80° C. for 20 minutes, then adding the second double-particle size composite inorganic filler under stirring and maintaining the temperature at 60 to 80° C., starting the film vacuum degassing under stirring, stirring for 90 to 120 minutes under the condition of a vacuum degree of less than 133 Pa, stopping the stirring after completion and maintaining the vacuum for 10 minutes, finally breaking the vacuum, filtering the material, and obtaining the modified anhydride curing agent;

[0061] The prepared modified epoxy resin and modified acid anhydride curing agent are mixed according to a mass ratio to prepare epoxy casting resin for 110kV dry-type transformer.

[0062] The embodiment of the present invention further provides a 110kV dry-type transformer, which is a 110kV dry-type transformer cast by using the above-mentioned 110kV dry-type transformer with epoxy casting resin.

[0063] Preferably, in the above transformer, the above 110kV dry-type transformer epoxy casting resin is used to cast a 110kV dry-type transformer in the following manner, including:

[0064] Place the coil and mold in a 120℃ oven for preheating for 2 hours, then transfer them to a vacuum casting tank for degassing and dehumidification under the conditions of coil temperature of 100-120℃ and vacuum pressure less than 133Pa; at the same time, transfer the modified epoxy resin and modified anhydride curing agent that make up the epoxy casting resin for 110kV dry-type transformer into a static mixer, control the temperature of the mixture to be fully stirred and degassed at 90℃ for standby use; after completing the preheating and dehumidification of the coil and mold, keep the temperature of the coil and mold at 90-110℃ and the discharge temperature of the static mixer at 90℃. The dry-type transformer is poured at 80-90°C, the vacuum pressure of the pouring tank is maintained at 250-400Pa, and the pouring is controlled to be completed within 180min; after the pouring is completed, the poured mold is transferred to the oven and the curing conditions are set to 100°C / 2hr+80°C / 8hr+100°C / 4hr+140°C / 8hr, and after the curing is completed, the mold is demoulded at a temperature of 100-110°C, and then the cured transformer is returned to the oven for cooling, and the manufactured product is an epoxy resin cast 110kV dry-type transformer.

[0065] The epoxy casting resin for dry-type transformers is obtained by mixing modified epoxy resin and modified acid anhydride curing agent in a specific ratio. The dry-type transformer with excellent performance is obtained by pouring and curing according to the specified curing temperature and time. In addition to basic sealing, insulation, waterproofing and dustproofing, the potting glue cured product also has higher heat resistance (glass transition temperature Tg ≥ 130°C), high mechanical properties (tensile strength ≥ 85MPa, compression strength > 170MPa), low thermal expansion coefficient (CTE ≤ 30ppm / K), and flame retardant performance meets UL94 V-0 level. The transformer cast with the epoxy casting resin has excellent heat resistance, heat dissipation performance, crack resistance, mechanical properties and flame retardant properties, which improves the high-temperature operation reliability of the dry-type transformer and prolongs its service life.

[0066] In summary, the epoxy casting resin of the embodiment of the present invention has at least the following beneficial effects:

[0067] The epoxy casting resin has the characteristics of high filling, low viscosity and long operability time: the use of low-viscosity, high-heat-resistant alicyclic epoxy resin increases the glass transition temperature (Tg) of the resin cured product, and improves the heat resistance grade and high-temperature compression strength of the cured product; the use of rubber-modified epoxy or core-shell structure toughening agent increases the toughness of the cured product and improves the anti-cracking performance of the cured product; after the surface modification of the double-particle size composite inorganic filler by silane coupling agent, it can achieve lower viscosity and higher filling ratio. The lower viscosity of the glue will also make the wettability and permeability better. The large and small particle size grading design makes the filling more dense and can better fill and avoid internal gaps. The higher inorganic filler filling ratio will make the cured product shrinkage rate and thermal expansion coefficient smaller, and improve the anti-cracking performance of the cured product; the use of silicon micropowder and alumina with good thermal conductivity and the combination of angular / spherical shapes make the filling denser and sufficient, which is conducive to the establishment of heat conduction paths, which will make the heat dissipation effect better, effectively balance the temperature difference inside and outside the transformer coil, and can improve the operating stability and extend its service life.

[0068] In order to more clearly demonstrate the technical solutions and technical effects provided by the present invention, the solutions provided by the embodiments of the present invention are described in detail with specific examples below. It should be noted that the experimental methods described in the following embodiments are conventional methods unless otherwise specified, and the reagents and materials can be obtained from commercial channels unless otherwise specified.

[0069] Example 1

[0070] This embodiment provides an epoxy casting resin for a 110 kV dry-type transformer, and a preparation method thereof comprises the following steps (each component is calculated by weight):

[0071] The modified epoxy resin and the modified anhydride curing agent are prepared respectively, wherein:

[0072] Preparation of modified epoxy resin: 80 parts of bisphenol A epoxy resin (YD-128, Guodu Chemical (Kunshan) Co., Ltd.), 20 parts of 4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester (TTA21P, Jiangsu Taitel New Materials Technology Co., Ltd.), and 15 parts of CTBN modified epoxy (KR-207, Guodu Chemical (Kunshan) Co., Ltd.) were added into a stirring container, stirred at 60-70°C for 20 minutes, and then 0.2 parts of dispersant (BYK-W 980, BYK Chemical), 0.05 parts of defoamer (DOWSIL SH5500, Dow Chemical) was stirred for 5 minutes, and then 14.5 parts of hexaphenoxy cyclotriphosphazene, 10 parts of triphenyl phosphate, 180 parts of active spherical alumina (NA2200W, D50 = 20 μm, Jiangsu Lianrui New Materials Co., Ltd.), and 10 parts of active angular alumina (Y4-1, D50 = 4 μm, Suzhou Jinyi New Materials Technology Co., Ltd.) were added in sequence under stirring, and the temperature was raised to 90-100° C. and stirred for 30-60 minutes. Under stirring, the film degassing equipment was turned on, and the mixture was stirred for 90-120 minutes under the condition of vacuum degree <133 Pa. After completion, stirring was stopped and the vacuum was maintained for 10 minutes. Finally, the vacuum was broken and the material was filtered to obtain the modified epoxy resin;

[0073] Preparation of modified anhydride curing agent: 100 parts of methyltetrahydrophthalic anhydride, 10 parts of core-shell structure toughening agent (MZ-120, Zhonghua Trading Co., Ltd.), and 0.3 parts of curing accelerator benzyldimethylamine are added to a stirring container, stirred at 60-70°C for 20 minutes, and then 215 parts of active spherical alumina (NA2200W, D50=20μm, Jiangsu Lianrui New Materials Co., Ltd.) and 20 parts of active angular alumina (Y4-1, D50=4μm, Suzhou Jinyi New Materials Technology Co., Ltd.) are added in sequence under stirring and the temperature is kept at 60-70°C. The film degassing equipment is turned on under stirring and stirred for 90-120 minutes under the condition of vacuum degree <133Pa. After completion, stirring is stopped and the vacuum is maintained for 10 minutes. Finally, the vacuum is broken and the material is filtered to obtain a modified anhydride curing agent.

[0074] When in use, the prepared modified epoxy resin is combined with the modified acid anhydride curing agent in a mass ratio of 100:100 to obtain the epoxy casting resin for 110kV dry-type transformer.

[0075] Example 2

[0076] This embodiment provides an epoxy casting resin for a 110 kV dry-type transformer, and a preparation method thereof comprises the following steps (each component is calculated by weight):

[0077] The modified epoxy resin and the modified anhydride curing agent are prepared respectively, wherein:

[0078] Preparation of modified epoxy resin: 80 parts of bisphenol A epoxy resin (YD-127, Guodu Chemical (Kunshan) Co., Ltd.), 20 parts of bis((3,4-epoxycyclohexyl)methyl) adipate (TTA26E, Jiangsu Taitel New Materials Technology Co., Ltd.), 5 parts of silicon-modified epoxy (KSR-1000, Guodu Chemical (Kunshan) Co., Ltd.) were added into a stirring container, stirred at 60-70°C for 20 minutes, and then 0.2 parts of dispersant (BYK-W 980, BYK Chemical), 0.05 parts of defoamer (DOWSILSH5500, Dow Chemical) were stirred for 5 minutes, and then 10 parts of aluminum diethylphosphinate, 195 parts of active spherical alumina (NA2300W, D50 = 30μm, Jiangsu Lianrui New Materials Co., Ltd.), and 15 parts of active angular alumina (Y2-1, D50 = 2μm, Suzhou Jinyi New Materials Technology Co., Ltd.) were added in sequence under stirring, and the temperature was raised to 90-100°C, and stirred for 30-60min. Under stirring, the film degassing equipment was turned on, and the vacuum was less than 133Pa for 90-120min. After completion, the stirring was stopped and the vacuum was maintained for 10min. Finally, the vacuum was broken, and the material was filtered to obtain a modified epoxy resin;

[0079] Preparation of modified anhydride curing agent: 100 parts of methyl hexahydrophthalic anhydride, 5 parts of core-shell structure toughening agent (MZ-200, Zhonghua Trading Co., Ltd.), and 0.3 parts of curing accelerator benzyl dimethylamine are added to a stirring container, stirred at 60-70°C for 20 minutes, and then 240 parts of active spherical alumina (NA2300W, D50 = 30 μm, Jiangsu Lianrui New Materials Co., Ltd.) and 25 parts of active angular alumina (Y2-1, D50 = 2 μm, Suzhou Jinyi New Materials Technology Co., Ltd.) are added in sequence under stirring and the temperature is kept at 60-70°C. The film degassing equipment is turned on under stirring and stirred for 90-120 minutes under the condition of vacuum degree <133Pa. After completion, stirring is stopped and the vacuum is maintained for 10 minutes. Finally, the vacuum is broken and the material is filtered to obtain the modified anhydride curing agent;

[0080] When in use, the prepared modified epoxy resin is combined with the modified acid anhydride curing agent in a mass ratio of 100:100 to obtain the epoxy casting resin for 110kV dry-type transformer.

[0081] Example 3

[0082] This embodiment provides an epoxy casting resin for a 110 kV dry-type transformer, and a preparation method thereof comprises the following steps (each component is calculated by weight):

[0083] The modified epoxy resin and the modified anhydride curing agent are prepared respectively, wherein:

[0084] Preparation of modified epoxy resin: 40 parts of bisphenol A epoxy resin (YD-128, Guodu Chemical (Kunshan) Co., Ltd.), 40 parts of bisphenol F epoxy resin (YDF-170, Guodu Chemical (Kunshan) Co., Ltd.), 20 parts of (3,4,3',4'-diepoxy)dicyclohexane (TTA800, Jiangsu Taitel New Materials Technology Co., Ltd.), 5 parts of core-shell structure toughening agent (MX-154, Zhonghua Trading Co., Ltd.) were added into a stirring container, stirred at 60-70°C for 20 minutes, and then 0.2 parts of dispersant (BYK-W 980, BYK Chemical), 0.05 parts of defoaming agent (DOWSIL SH5500, Dow Chemical) was stirred for 5 minutes, and then 6 parts of 1,3-phenylene phosphate (2,6-xylyl) tetraester, 5.8 parts of ammonium polyphosphate, 90 parts of active angular silica powder (DC2170, D50 = 17μm, Jiangsu Lianrui New Materials Co., Ltd.), 90 parts of active spherical alumina (NA2200W, D50 = 20μm, Jiangsu Lianrui New Materials Co., Ltd.), 10 parts of active spherical alumina (NA2020W, D50 = 2μm, Jiangsu Lianrui New Materials Co., Ltd.) were added in sequence under stirring, and the temperature was raised to 90-100°C, and stirred for 30-60min. Under stirring, the film degassing equipment was turned on, and the vacuum was less than 133Pa for 90-120min. After completion, the stirring was stopped and the vacuum was maintained for 10min. Finally, the vacuum was broken, and the material was filtered to obtain a modified epoxy resin;

[0085] Preparation of modified anhydride curing agent: 100 parts of methyltetrahydrophthalic anhydride, 10 parts of core-shell structure toughening agent (MZ-120, Zhonghua Trading Co., Ltd.), and 0.3 parts of curing accelerator benzyldimethylamine are added to a stirring container, stirred at 60-70°C for 20 minutes, and then 115 parts of active angular silicon powder (DC2170, D50=17μm, Jiangsu Lianrui New Materials Co., Ltd.), 90 parts of active spherical alumina (NA2200W, D50=20μm, Jiangsu Lianrui New Materials Co., Ltd.), and 20 parts of active spherical alumina (NA2020W, D50=2μm, Jiangsu Lianrui New Materials Co., Ltd.) are added under stirring and the temperature is kept at 60-70°C. The film degassing equipment is turned on under stirring, and the vacuum is less than 133Pa. Stir for 90-120 minutes. After completion, stop stirring and keep the vacuum for 10 minutes. Finally, break the vacuum, filter the material, and obtain the modified anhydride curing agent.

[0086] When in use, the prepared modified epoxy resin is combined with the modified acid anhydride curing agent in a mass ratio of 100:100 to obtain the epoxy casting resin for 110kV dry-type transformer.

[0087] Example 4

[0088] This embodiment provides an epoxy casting resin for a 110 kV dry-type transformer, and a preparation method thereof comprises the following steps (each component is calculated by weight):

[0089] The modified epoxy resin and the modified anhydride curing agent are prepared respectively, wherein:

[0090] Preparation of modified epoxy resin: 80 parts of bisphenol A epoxy resin (YD-128, Guodu Chemical (Kunshan) Co., Ltd.), 20 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester (TTA21P, Jiangsu Taitel New Materials Technology Co., Ltd.), and 10 parts of NBR modified epoxy (KR-208, Guodu Chemical (Kunshan) Co., Ltd.) were added into a stirring container, stirred at 60-70°C for 20 minutes, and then 0.2 parts of dispersant (BYK-W 980, BYK Chemical), 0.05 parts of defoamer (DOWSIL SH5500, Dow Chemical) was stirred for 5 minutes, and then 7.6 parts of ammonium polyphosphate, 190 parts of active spherical alumina (NA2300W, D50=30μm, Jiangsu Lianrui New Materials Co., Ltd.), and 10 parts of active angular alumina (Y2-1, D50=2μm, Suzhou Jinyi New Materials Technology Co., Ltd.) were added in sequence under stirring, and the temperature was raised to 90-100°C, and stirred for 30-60min. Under stirring, the film degassing equipment was turned on, and the mixture was stirred for 90-120min under the condition of vacuum degree <133Pa. After completion, stirring was stopped and the vacuum was maintained for 10min. Finally, the vacuum was broken, and the material was filtered to obtain a modified epoxy resin;

[0091] Preparation of modified anhydride curing agent: 100 parts of methyl hexahydrophthalic anhydride, 10 parts of core-shell structure toughening agent (MZ-120, Zhonghua Trading Co., Ltd.), and 0.3 parts of curing accelerator 2,4,6-tris (dimethylaminomethyl) phenol are added into a stirring container, stirred at 60-70°C for 20 minutes, and then 225 parts of active spherical alumina (NA2300W, D50 = 30 μm, Jiangsu Lianrui New Materials Co., Ltd.) and 20 parts of active angular alumina (Y2-1, D50 = 2 μm, Suzhou Jinyi New Materials Technology Co., Ltd.) are added in sequence under stirring and the temperature is kept at 60-70°C. The film degassing equipment is turned on under stirring and stirred for 90-120 minutes under the condition of vacuum degree <133Pa. After completion, stirring is stopped and vacuum is maintained for 10 minutes. Finally, the vacuum is broken and the material is filtered to obtain the modified anhydride curing agent.

[0092] When in use, the prepared modified epoxy resin is combined with the modified acid anhydride curing agent in a mass ratio of 100:100 to obtain the epoxy casting resin for 110kV dry-type transformer.

[0093] Example 5

[0094] This embodiment provides an epoxy casting resin for a 110 kV dry-type transformer, and a preparation method thereof comprises the following steps (each component is calculated by weight):

[0095] The modified epoxy resin and the modified anhydride curing agent are prepared respectively, wherein:

[0096] Preparation of modified epoxy resin: 40 parts of bisphenol F epoxy resin (YDF-170, Guodu Chemical (Kunshan) Co., Ltd.), 40 parts of phenol novolac epoxy resin (YDPN-631, Guodu Chemical (Kunshan) Co., Ltd.), 20 parts of cyclohexane-1,2-dicarboxylic acid diglycidyl ester (TTA184, Jiangsu Taitel New Materials Technology Co., Ltd.), 10 parts of silicon-modified epoxy (KSR-1000, Guodu Chemical (Kunshan) Co., Ltd.), 5 parts of core-shell structure toughening agent (MX-154, Zhonghua Trading Co., Ltd.) were added into a stirring container, stirred at 60-70°C for 20 minutes, and then 0.2 parts of dispersant (BYK-W980, BYK Chemical), 0.05 parts of defoaming agent (DOWSIL SH5500, Dow Chemical) was stirred for 5 minutes, and then 19.1 parts of hexaphenoxy cyclotriphosphazene, 190 parts of active spherical alumina (NA2200W, D50 = 20 μm, Jiangsu Lianrui New Materials Co., Ltd.), and 15 parts of active angular alumina (Y2-1, D50 = 2 μm, Suzhou Jinyi New Materials Technology Co., Ltd.) were added in sequence under stirring, and the temperature was raised to 90-100° C. and stirred for 30-60 minutes. Under stirring, the film degassing equipment was turned on, and the mixture was stirred for 90-120 minutes under the condition of vacuum degree <133 Pa. After completion, stirring was stopped and the vacuum was maintained for 10 minutes. Finally, the vacuum was broken, and the material was filtered to obtain a modified epoxy resin;

[0097] Preparation of modified anhydride curing agent: 100 parts of methyltetrahydrophthalic anhydride, 5 parts of core-shell structure toughening agent (MZ-200, Zhonghua Trading Co., Ltd.), and 0.3 parts of curing accelerator benzyldimethylamine are added to a stirring container, stirred at 60-70°C for 20 minutes, and then 230 parts of active spherical alumina (NA2300W, D50=30μm, Jiangsu Lianrui New Materials Co., Ltd.) and 20 parts of active angular alumina (Y2-1, D50=2μm, Suzhou Jinyi New Materials Technology Co., Ltd.) are added under stirring and the temperature is kept at 60-70°C. The film degassing equipment is turned on under stirring, and the vacuum is less than 133Pa. Stir for 90-120 minutes. After completion, stop stirring and maintain the vacuum for 10 minutes. Finally, break the vacuum, filter the material, and obtain the modified anhydride curing agent.

[0098] When in use, the prepared modified epoxy resin is combined with the modified acid anhydride curing agent in a mass ratio of 100:100 to obtain the epoxy casting resin for 110kV dry-type transformer.

[0099] Comparative Example 1

[0100] This comparative example provides an epoxy casting resin for a dry-type transformer, and its preparation method comprises the following steps (each component is calculated by weight):

[0101] Preparation of modified epoxy resin: 100 parts of bisphenol A epoxy resin (YD-128, Guodu Chemical (Kunshan) Co., Ltd.) are added into a stirring container, and then 0.2 parts of dispersant (BYK-W 980, BYK Chemical) and 0.05 parts of defoamer (DOWSIL SH5500, Dow Chemical) are added in sequence and stirred for 5 minutes, and then 165 parts of active silicon powder (DC2170, Jiangsu Lianrui New Materials Co., Ltd.) are added under stirring and the temperature is increased to 90-100°C, and stirred for 30-60 minutes. The film degassing equipment is turned on under stirring, and the mixture is stirred for 90-120 minutes under the condition of vacuum degree <133Pa. After completion, the stirring is stopped and the vacuum is maintained for 10 minutes. Finally, the vacuum is broken, and the material is filtered to obtain the modified epoxy resin;

[0102] Preparation of modified anhydride curing agent: 100 parts of methyltetrahydrophthalic anhydride and 0.5 parts of curing accelerator benzyldimethylamine are added to a stirring container, stirred at 60-70°C for 20 minutes, and then 190 parts of active silicon micropowder of a single particle size (DC2170, Jiangsu Lianrui New Materials Co., Ltd.) are added under stirring and the temperature is maintained at 60-70°C. The thin film degassing equipment is turned on under stirring and stirred for 90-120 minutes under the condition of vacuum degree <133Pa. After completion, stirring is stopped and the vacuum is maintained for 10 minutes. Finally, the vacuum is broken and the material is filtered to obtain the modified anhydride curing agent.

[0103] It can be known that the above comparative examples are not prior art, but comparative examples designed to compare the performance of the products of the present invention.

[0104] A 110 kV dry-type transformer was made by using the epoxy casting resin obtained in Examples 1 to 5 and Comparative Example 1. The manufacturing process was as follows: the coil and the mold were placed in an oven at 120° C. for preheating for 2 hours, and then transferred to a vacuum casting tank for degassing and dehumidification under the conditions of a coil temperature of 100 to 120° C. and a vacuum pressure of less than 133 Pa; at the same time, the modified epoxy and the modified anhydride were transferred to a static mixer, and the mixture temperature was controlled to be fully stirred at 90° C., degassed and used for standby; after the coil and the mold were preheated and dehumidified, the dry-type transformer was cast while maintaining the coil and the mold temperature at 90 to 110° C. and the static mixer discharge temperature at 80 to 90° C., the vacuum pressure of the casting tank was maintained at 250 to 400 Pa, and the casting was controlled to be completed within 180 minutes;

[0105] After pouring is completed, the poured mold is transferred to the oven and the curing conditions are set to 100℃ / 2hr+80℃ / 8hr+100℃ / 4hr+140℃ / 8hr. After curing is completed, demoulding is carried out at a temperature of 100-110℃, and then the cured transformer is returned to the oven to cool down.

[0106] Potting glue performance test:

[0107] The performance of the epoxy casting resin for 110 kV dry-type transformer in Examples 1 to 5 and the epoxy casting resin in Comparative Example 1 was tested, and the test results are shown in Table 1.

[0108] Table 1 Performance parameters of epoxy casting resin for 110kV dry-type transformer

[0109]

[0110] As can be seen from Table 1, the epoxy casting resins of Examples 1 to 5 have moderate mixing viscosity and gel time, do not require high temperature and high pressure operation, and reduce the operating requirements on the application end. Whether it is manual or automatic perfusion, it can meet the requirements.

[0111] Curing performance test:

[0112] The curing properties of the epoxy casting resin for 110 kV dry-type transformer in Examples 1 to 5 and the epoxy casting resin in Comparative Example 1 were tested. The test results are shown in Table 2.

[0113] Table 2 Curing characteristics of epoxy casting resin for dry-type transformer

[0114]

[0115]

[0116] As can be seen from Table 2, the epoxy casting resin for dry-type transformers of Examples 1 to 5 of the present invention has a greatly improved heat resistance (Tg ≥ 130°C) due to the use of alicyclic epoxy resin with high heat resistance and low viscosity, so that the heat resistance of the dry-type transformer is higher. The use of alumina makes the thermal expansion coefficient of the cured product (compared with angular silica powder) lower, ensuring that the expansion is smaller when the operating temperature of the transformer changes, and improving the anti-cracking performance; the addition of environmentally friendly flame retardants ensures that the combustion resistance of the transformer can reach V-0 level; at the same time, the addition of alumina greatly improves the thermal conductivity, which effectively balances the temperature difference between the inside and outside of the coil, ensures that the dry-type transformer can operate stably, and extends its service life.

[0117] The epoxy casting resin for 110kV dry-type transformer provided by the present invention may contain pigments such as dark red, bright red or green color pastes of organic or inorganic pigments, in addition to the various organic systems mentioned above, within the limits necessary and not contrary to the purpose of the present invention.

[0118] In summary, in the case of high filling of inorganic fillers, the viscosity of the casting resin is still relatively low. The epoxy casting resin of the present invention has the advantages of low viscosity, high filling and long operability time. The transformer cast with the epoxy casting resin has excellent heat resistance, heat dissipation performance, crack resistance, mechanical properties and flame retardant properties, which improves the high temperature operation reliability of the dry-type transformer and prolongs its service life.

[0119] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims. The information disclosed in the background technology section of this article is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or in any form that the information constitutes prior art known to those skilled in the art.

Claims

1. An epoxy casting resin for a 110kV dry-type transformer, characterized in that: include: A modified epoxy resin and a modified anhydride curing agent in a mass ratio of 100:100; wherein, The modified epoxy resin is prepared from the following components in parts by mass, including: 100 parts of epoxy resin, 5 to 15 parts of a first toughening agent, 0.2 parts of a dispersant, 0.05 parts of a defoaming agent, 7 to 25 parts of an environmentally friendly flame retardant, and 190 to 210 parts of a first double-particle-size composite inorganic filler; The modified acid anhydride curing agent is prepared from the following components in parts by mass, including: 100 parts of acid anhydride, 5 to 10 parts of a second toughening agent, 0.1 to 0.5 parts of a curing accelerator and 235 to 265 parts of a second double-particle-size composite inorganic filler.

2. The epoxy casting resin for 110kV dry-type transformer according to claim 1, characterized in that: The first dual-particle size composite inorganic filler and the second dual-particle size composite inorganic filler are both composed of a large-particle size filler treated with a silane coupling agent for surface activation and a small-particle size filler treated with a silane coupling agent for surface activation in a mass ratio of 100:5-13, wherein the average particle size D50 of the large-particle size filler is 17-20 μm, and the average particle size D50 of the small-particle size filler is 2-5 μm.

3. The epoxy casting resin for 110kV dry-type transformer according to claim 2, characterized in that: The large-particle filler is an inorganic filler in an angular shape or an inorganic filler in a spherical shape; The small particle size filler is an angular inorganic filler or a spherical inorganic filler.

4. The epoxy casting resin for 110kV dry-type transformer according to claim 2 or 3, characterized in that: In the first double-particle size composite inorganic filler and the second double-particle size composite inorganic filler, the large-particle size filler and the small-particle size filler are any one or more of silicon micropowder, aluminum oxide, magnesium oxide, zinc oxide, boron nitride, and aluminum nitride.

5. The epoxy casting resin for 110kV dry-type transformer according to any one of claims 1 to 3, characterized in that: In the modified epoxy resin, the epoxy resin is any one or more of a bisphenol epoxy resin, a novolac epoxy resin, and an alicyclic epoxy resin; The dispersant is an organosilicon dispersant; The defoamers are all silicone defoamers; The environmentally friendly flame retardant is any one or more of diethyl aluminum phosphinate, 1,3-phenylene (2,6-xylyl) tetraphosphate, hexaphenoxy cyclotriphosphazene, ammonium polyphosphate, melamine cyanurate, triphenyl phosphate, tricresyl phosphate, toluene diphenyl phosphate, and modified cage-type polysilsesquioxane; The first toughening agent is any one or more of CTBN-modified epoxy resin, NBR-modified epoxy resin, silicon-modified epoxy resin, and core-shell structure toughening agent.

6. The epoxy casting resin for 110kV dry-type transformer according to claim 5, characterized in that: The bisphenol epoxy resin is at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, and hydrogenated bisphenol A epoxy resin; The novolac epoxy resin is at least one of phenol novolac epoxy resin, o-cresol novolac epoxy resin, dicyclopentadiene phenol epoxy resin, biphenyl phenol epoxy resin, trifunctional novolac epoxy resin, and tetrafunctional novolac epoxy resin; The alicyclic epoxy resin is at least one of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, bis((3,4-epoxycyclohexyl)methyl)adipate, 4-vinyl-1-cyclohexene diepoxide, 1,4-cyclohexanedimethanol bis(3,4-epoxycyclohexanecarboxylate), (3,4,3',4'-diepoxy)dicyclohexane, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, 4,5-epoxytetrahydrophthalic acid diglycidyl ester, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.

7. The epoxy casting resin for 110kV dry-type transformer according to any one of claims 1 to 3, characterized in that: In the modified acid anhydride curing agent, the acid anhydride is any one or more of tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, nadic anhydride, and methylnadic anhydride; The curing accelerator is a tertiary amine accelerator; The second toughening agent is any one or more of CTBN-modified epoxy resin, NBR-modified epoxy resin, silicon-modified epoxy resin, and core-shell structure toughening agent.

8. A method for preparing the epoxy casting resin for 110 kV dry-type transformer according to any one of claims 1 to 7, characterized in that: The following steps are involved: The modified epoxy resin and the modified anhydride curing agent are prepared respectively, wherein: The modified epoxy resin is prepared, comprising: taking raw materials according to the formula of the modified epoxy resin according to any one of claims 1 to 7, adding the epoxy resin and the first toughening agent in the raw materials into a stirring container, stirring at a temperature of 60 to 80° C. for 20 minutes, then adding a dispersant and a defoamer, stirring for 5 minutes, then adding an environmentally friendly flame retardant and a first double-particle-size composite inorganic filler in sequence under stirring and raising the temperature to 90 to 100° C., stirring for 30 to 60 minutes, starting a thin film vacuum degassing under stirring, stirring for 90 to 120 minutes under the condition that the vacuum degree is less than 133 Pa, stopping stirring after completion and maintaining the vacuum for 10 minutes, finally breaking the vacuum, filtering the material, and obtaining the modified epoxy resin; The modified anhydride curing agent is prepared, comprising: taking raw materials according to the formula of the modified anhydride curing agent according to any one of claims 1 to 7, adding the anhydride, the second toughening agent and the curing accelerator in the raw materials into a stirring container, stirring at a temperature of 60 to 80° C. for 20 minutes, then adding the second double-particle size composite inorganic filler under stirring and maintaining the temperature at 60 to 80° C., starting the film vacuum degassing under stirring, stirring for 90 to 120 minutes under the condition of a vacuum degree of less than 133 Pa, stopping the stirring after completion and maintaining the vacuum for 10 minutes, finally breaking the vacuum, filtering the material, and obtaining the modified anhydride curing agent; The prepared modified epoxy resin and the modified acid anhydride curing agent are mixed in a mass ratio of 100:100 to prepare the epoxy casting resin for 110kV dry-type transformer.

9. A 110kV dry-type transformer, characterized in that: The invention relates to a 110kV dry-type transformer which is cast by using the epoxy casting resin for the 110kV dry-type transformer as described in any one of claims 1 to 7.

10. The 110kV dry-type transformer according to claim 9, characterized in that: The 110 kV dry-type transformer epoxy casting resin according to any one of claims 1 to 7 is cast in the following manner to form a 110 kV dry-type transformer, comprising: Place the coil and mold in a 120℃ oven for preheating for 2 hours, then transfer them to a vacuum casting tank for degassing and dehumidification under the conditions of coil temperature of 100-120℃ and vacuum pressure less than 133Pa; at the same time, transfer the modified epoxy resin and modified anhydride curing agent that make up the epoxy casting resin for 110kV dry-type transformer into a static mixer, control the temperature of the mixture at 90℃, stir it thoroughly, degas and set it aside for use; after completing the preheating and dehumidification of the coil and mold, keep the temperature of the coil and mold at 90-110℃ and the discharge temperature of the static mixer at 150℃. The dry-type transformer is poured at 80-90°C, the vacuum pressure of the pouring tank is maintained at 250-400Pa, and the pouring is controlled to be completed within 180min; after the pouring is completed, the poured mold is transferred to the oven and the curing conditions are set to 100°C / 2hr+80°C / 8hr+100°C / 4hr+140°C / 8hr, and after the curing is completed, the mold is demoulded at a temperature of 100-110°C, and then the cured transformer is returned to the oven for cooling, so that the epoxy resin cast 110kV dry-type transformer is made.

Citation Information

Cited By

  • Epoxy resin castable as well as preparation method and application thereof

    CN121064602A