Honeycomb structure double-leaf airtight door made of SMC glass fiber reinforced composite material

By adopting SMC glass fiber reinforced composite honeycomb structure and molding process in human defense sealed doors, the problems of complex structure and poor corrosion resistance in the existing technology are solved, and the effects of light weight, high strength and easy maintenance are achieved, which improves the effect of improvement Protection technology and resource utilization efficiency of civil defense engineering.

CN119041807APending Publication Date: 2024-11-29WUHU BAIYI CIVIL AIR DEFENSE ENG SHELTER EQUIP CO LTD

Patent Information

Application Number
CN202411247939.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing anti-sealed doors have complex structures, are not corrosion-resistant, have poor thermal insulation performance, and are difficult to maintain, resulting in short service life and relatively poor production efficiency and quality.

Method used

The double-fan closed door of honeycomb structure is adopted for SMC glass fiber reinforced composite material. It is produced through advanced honeycomb structure molds, combining glass fiber and resin materials to increase the depth of reinforcement ribs, reduce the material usage, and use molding and molding technology to improve product strength and accuracy.

Benefits of technology

It has achieved light weight, corrosion resistance, high strength, and easy installation and maintenance, reduced labor intensity for transportation and installation, improved protection technology level, saved construction resources, and had good social and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041807A_ABST
    Figure CN119041807A_ABST
Patent Text Reader

Abstract

The invention relates to an SMC (Sheet Molding Compound) glass fiber reinforced composite honeycomb structure double-leaf air-tight door which comprises a door leaf main body and a cover plate main body, and the door leaf main body and the cover plate main body are both made of SMC glass fiber reinforced composites. Wherein the SMC comprises UP resin, glass fiber, filler and various additives such as an initiator, a low shrinkage agent, a thickening agent, an internal release agent and the like. The glass fiber bears the mechanical strength part, and the filler reduces the cost, improves the viscosity and other properties of the resin base material, and prevents the fiber from being separated or filtered out during compression. A sealing strip is filled in a connecting gap between the door leaf main body and the door leaf main body center joint, and the door leaf main body is composed of a plurality of unit door leaves. The adjacent unit door leaves are connected through bolts, a honeycomb-shaped core plate is arranged on the inner surface of each unit door leaf, the cover plate body is composed of a plurality of unit cover plates, and the adjacent unit cover plates are in lap joint and fastened through rivets. The fireproof door has the advantages of being light in weight, high in strength, resistant to corrosion, long in service life, good in insulativity, sound insulation and flame retardance, free of maintenance cost in the using process, convenient to install, time-saving and labor-saving, and capable of playing an important role in civil air defense construction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a double-leaf airtight door of an SMC glass fiber reinforced composite honeycomb structure, belonging to the field of civil air defense engineering protection equipment. Technical Background

[0002] Civil air defense doors are one of the equipment used by the government to mobilize and organize the masses, take air defense and disaster relief measures, carry out rescue operations, and prevent and reduce disaster hazards. At present, most of the air defense closed doors on the market are steel structures, which are heavy, not corrosion-resistant, have poor thermal insulation performance, poor heat and sound insulation performance, high maintenance costs, and many disassembly and assembly failures, resulting in a short service life, which seriously affects the application of steel doors.

[0003] Reinforced concrete civil defense doors are the earliest civil defense equipment used in civil defense projects. Its low price has prompted people to continuously improve reinforced concrete civil defense doors, which has significantly improved the airtightness of the doors and reduced the possibility of damage. In civil defense projects, despite the use of high-grade cement, high-strength aggregate, low cement ratio, adding water reducer to concrete to make high-strength concrete; reducing the size of concrete aggregates while adding steel fibers, etc., its shortcomings of bulky structure and inconvenient operation have not been improved. With the continuous advancement of protection technology and the continuous development of civil defense projects, the application of steel structure civil defense doors in civil defense projects has rapidly expanded. Although the structural weight of steel structure civil defense doors is greatly reduced compared with reinforced concrete civil defense doors, for large-scale protective equipment, there are still defects such as heavy weight, labor-intensive operation, easy rust, and high cost. Since civil defense projects are generally located in underground structures, the air humidity is high and there is local water accumulation. When the equipment is not properly maintained, the steel door will corrode, seriously affecting the protection, airtightness and use performance of the protective equipment.

[0004] In recent years, with the rapid development of urban construction, the scale of civil air defense construction has continued to expand, and the number of projects has also continued to increase. In order to achieve the construction speed of the project and ensure the normal operation of the civil air defense project when protection is needed, it is necessary to develop a civil air defense door that is light in weight, fast in installation and debugging, easy to use and maintain, beautiful and practical, and moderately priced. At the same time, materials with different properties are selected for doors with different uses and different resistances, so that the materials can give full play to their respective advantages. Therefore, the door should have the characteristics of light material, high strength, good impact resistance, good toughness, good crushing resistance, low price, and easy material acquisition. Through the research on methods and technical measures for lightweight civil air defense doors, a new material civil air defense door that is safe, reliable, and easy to manufacture and install has been developed, which can effectively reduce labor intensity, improve work efficiency, speed up construction progress, and save construction investment.

[0005] To this end, designers combined material science and technology, carbon fiber, active powder concrete, basalt fiber, glass fiber, etc. Although the material cost is high and the processing technology is complicated, the comprehensive performance of the protective equipment has been greatly improved, so it has been vigorously promoted and applied.

[0006] SMC composite material is the abbreviation of Sheet molding compound, which is sheet molding compound. The main raw materials are GF (special yarn), UP (unsaturated resin), low shrinkage additives, MD (filler) and various additives. Compared with traditional materials, SMC composite materials and SMC molded products have excellent electrical insulation, mechanical properties, and thermal stability. Special properties such as chemical corrosion resistance can effectively solve the shortcomings of wood, steel, and plastic materials that are easy to age, easy to corrode, poor insulation, poor cold resistance, poor flame retardancy, and short life, so they are widely favored in various industries.

[0007] Honeycomb structure is a natural or artificial geometric shape that can minimize the amount of materials used to achieve the lowest weight and lowest cost. Honeycomb materials are widely used in various fields. Their light weight and high strength have always been favored by people. Products with honeycomb structures are constantly being researched.

[0008] At present, the inner side of the civil air defense closed door generally has well-shaped reinforcement ribs to increase the strength of the product. The height of the reinforcement ribs is generally 1-2cm. Due to the limited depth, the reinforcement effect is also limited, the material saving is also quite limited, and the weight reduction degree is also general. If the depth of the reinforcement ribs can be greatly increased, the material can be greatly saved, the product weight can be reduced, and it is beneficial for enterprises to save costs. However, the current production molds cannot produce deeper reinforcement ribs. The deeper the reinforcement ribs, the more difficult it is to demold. At present, the mold generally uses cutting to cut out several bumps with a height of 1-2cm for processing reinforcement ribs. This structural form is destined to not be too deep, and the surface of the bumps is rough, and it is not easy to demold. Therefore, the structure of the existing mold needs to be strengthened.

[0009] So far, the double-leaf closed door using SMC glass fiber reinforced composite honeycomb structure has not been developed in the project. It cannot meet the needs of the project, and the relevant research and development work is imminent. Summary of the invention

[0010] The present invention provides a double-leaf closed door of an SMC glass fiber reinforced composite honeycomb structure, so as to solve the problems existing in the prior art such as complex structure, corrosion resistance, poor heat insulation and sound insulation, and difficulty in maintenance resulting in short service life, poor production efficiency, and relatively poor quality.

[0011] In order to solve the above technical problems, the present invention adopts the following technical solutions: A double-leaf closed door with an SMC glass fiber reinforced composite honeycomb structure, comprising a door leaf main body and a cover plate main body, both of which are made of glass fiber reinforced composite material integral molding process, the door leaf main body is produced by an advanced honeycomb structure mold, the door leaf main body and the middle seam connecting gap of the door leaf main body are filled with sealing strips, the door leaf main body is composed of a plurality of unit door leaves, adjacent unit door leaves are connected by bolts, a honeycomb core plate is arranged on the inner surface of each unit door leaf, the cover plate main body is composed of a plurality of unit cover plates, adjacent unit cover plates are overlapped with each other and fastened by rivets.

[0012] Furthermore, the door leaf is made of SMC glass fiber reinforced composite material.

[0013] Furthermore, the components of the SMC glass fiber reinforced composite material include 30-40 parts of UP resin, 30-40 parts of glass fiber, 40-50 parts of filler and various additives such as 0.3-1 parts of initiator, 10-20 parts of low shrinkage agent, 1-2 parts of thickener, 2-10 parts of internal release agent and the like.

[0014] Furthermore, the UP resin is formed by polycondensation of dibasic acid and diol, and the water content is controlled at 0.1-0.15%.

[0015] Furthermore, the glass fiber is in the form of chopped filaments, untwisted roving, or chopped fiber mat.

[0016] Furthermore, the filler is carbonate, sulfate, oxide, silicon oxide and silicate, etc.

[0017] Furthermore, the initiator is BPO, TBPO, DCP, CHP and the like.

[0018] Furthermore, the low shrinkage agent is PMMA, PS, PVAC, PE, PVC, PCL, PB, etc.

[0019] Furthermore, the thickener is a Group IIA metal oxide.

[0020] Furthermore, the internal release agent is stearic acid, zinc stearate, magnesium stearate, calcium stearate, etc.

[0021] Compared with the prior art, the present invention has the following technical effects: the present invention adopts a double-leaf civil air defense closed door using glass fiber reinforced sheet film plastic (SMC) as the door leaf substrate. The double-leaf civil air defense closed door can be applied to civil air defense basements, subway civil air defense projects, civil air defense command posts and other civil air defense projects. Compared with traditional steel structures and reinforced concrete doors, the door has the advantages of light weight, corrosion resistance, high specific strength, easy installation and maintenance, and good economy. It not only ensures the protective function of the civil air defense project department, but also has good performance in use, which can greatly reduce the labor intensity of transportation and installation of civil air defense doors, reduce safety hazards during equipment installation, adapt to the harmonious and unified requirements of wartime and peacetime use, fully realize the requirements for the use of civil air defense projects in peacetime and wartime, improve the protection technology level of civil air defense projects, save construction resources, and have good social benefits, economic benefits and combat readiness benefits. This invention combines fiber-reinforced sheet molding compound (SMC) material with honeycomb structure for the first time and applies it to the production of civil air defense door panels. It uses advanced honeycomb structure to produce molds, which greatly increases the depth of the reinforcing ribs, greatly saves materials, improves product quality, saves costs, reduces the size of the door, facilitates demoulding, and improves overall strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a front view of the double-leaf closed door of the SMC glass fiber reinforced composite honeycomb structure of the present invention; Figure 2 It is a side view of the double-leaf closed door of the SMC glass fiber reinforced composite honeycomb structure of the present invention; Figure 3 It is a top view of the double-leaf closed door of the SMC glass fiber reinforced composite honeycomb structure of the present invention; Figure 4 It is a schematic diagram of SMC production; Figure 5 It is a schematic diagram of SMC molding; Figure 6 It is a schematic diagram of the internal honeycomb structure. Specific implementation methods

[0023] The specific embodiments of the present invention will be further described in detail below in conjunction with the accompanying drawings. However, it should be noted that these embodiments are only for explaining the present invention rather than limiting the present invention. Example 1

[0024] like Figure 1As shown, an SMC glass fiber reinforced composite honeycomb structure double-leaf closed door includes a door leaf main body and a cover plate main body. Both the door leaf main body and the cover plate main body are made of glass fiber reinforced composite materials. The door leaf main body is produced by an advanced honeycomb structure mold. A sealing strip is filled in the gap between the door leaf main body and the middle seam of the door leaf. The door leaf main body is composed of a plurality of unit door leaves. Adjacent unit door leaves are connected by bolts. A honeycomb core plate is arranged on the inner surface of each unit door leaf. The cover plate main body is composed of a plurality of unit cover plates. Adjacent unit cover plates are overlapped with each other and fastened by rivets.

[0025] The present invention adopts compression molding process to produce civil air defense door leaf, which puts a certain amount of compression molding sheet into preheated mold, and after heating and pressurizing, the product has high strength, high geometrical dimension accuracy, and is not deformed by external environment temperature. It is suitable for large-scale and complex structure products.

[0026] like Figure 4 As shown in the figure, the process flow of SMC production mainly includes resin paste preparation, paste operation, fiber cutting, sedimentation and impregnation, resin thickening and other processes, which are mainly divided into the following steps: 1. Preparation of resin paste: Add 30 parts of unsaturated polyester UP, 40 parts of filler calcium carbonate, 2 parts of release agent zinc stearate, 1 part of thickener magnesium oxide, and 10 parts of low shrinkage agent PMMA into high-speed shear mixer 1 and mix evenly, then add 0.5 parts of initiator DCP, and increase the stirring speed at the same time to make each raw material highly dispersed. In the process of preparing the resin paste, pay attention to controlling the stirring temperature and the time of adding the thickener to obtain the ideal resin paste viscosity and thickening speed. Finally, put the mixed resin into the resin storage tank 2; 2. Glass fiber cutting, pressure impregnation and winding: First, draw 30 portions of untwisted glass fiber roving from the creel 10 and feed them into the roller cutter 4. Adjust the roller distance so that the shear length of the roving is 25 mm. Then adjust the width of the resin tank 3 and the gap between the flowing paste, put the resin paste in the storage tank into the resin tank, and the resin paste is coated on the upper and lower film carriers under the action of gravity. At this time, start the conveyor belt machine 6, and make the roller cutter and the film roll 5 run synchronously with the conveyor belt machine. After being cut, the roving falls freely on the resin paste of the lower film. In this way, a sandwich layer prepreg of resin paste-chopped yarn-resin paste is formed between the upper and lower layers of film. Under the action of the pressure roller 7, the prepreg and the film are combined to make the resin paste and the fiber penetrate into one, and the air is removed by the adjustment roller 8. Wind it into an SMC roll with the winding device 9; 3. Ripening and packaging: Put the compounded SMC roll into the temperature-adjusting aging room (25-40℃) for aging. When the viscosity increases to the required value, it is the finished SMC product. 4. Pressing and molding: like Figure 5 Figure 6 As shown, a certain amount of prepared SMC molding material is placed in the preheated honeycomb mold, and then the mold is closed at a certain speed. The SMC molding material flows under pressure and fills the entire mold cavity. It is kept at the required temperature and pressure for a certain period of time. When it is cured and shaped under physical and chemical effects and reaches the best performance, the mold is opened and the product is taken out. The production of SMC glass fiber composite materials is completed. Example 2

[0027] like Figure 1 As shown, an SMC glass fiber reinforced composite honeycomb structure double-leaf closed door includes a door leaf main body and a cover plate main body. Both the door leaf main body and the cover plate main body are made of glass fiber reinforced composite materials. The door leaf main body is produced by an advanced honeycomb structure mold. A sealing strip is filled in the gap between the door leaf main body and the middle seam of the door leaf. The door leaf main body is composed of a plurality of unit door leaves. Adjacent unit door leaves are connected by bolts. A honeycomb core plate is arranged on the inner surface of each unit door leaf. The cover plate main body is composed of a plurality of unit cover plates. Adjacent unit cover plates are overlapped with each other and fastened by rivets.

[0028] The present invention adopts compression molding process to produce civil air defense door leaf, which puts a certain amount of compression molding sheet into preheated mold, and after heating and pressurizing, the product has high strength, high geometrical dimension accuracy, and is not deformed by external environment temperature. It is suitable for large-scale and complex structure products.

[0029] like Figure 4 As shown in the figure, the process flow of SMC production mainly includes resin paste preparation, paste operation, fiber cutting, sedimentation and impregnation, resin thickening and other processes, which are mainly divided into the following steps: 1. Preparation of resin paste: Add 40 parts of unsaturated polyester UP into high-speed shear mixer 1 and mix evenly, then add 1 part of initiator BPO, and increase the stirring speed at the same time to make all the raw materials highly dispersed. Then add 1.5 parts of thickener calcium oxide and 10 parts of release agent magnesium stearate, and continue stirring. Then add 50 parts of filler aluminum hydroxide and 10 parts of low shrinkage agent PE, and continue stirring until all the components listed in the formula are dispersed, stop stirring, and let it stand for use. During the preparation of the resin paste, pay attention to controlling the stirring temperature and the time of adding the thickener to obtain the ideal resin paste viscosity and thickening speed. Finally, put the mixed resin into the resin storage tank 2; 2. Glass fiber cutting, pressure impregnation and winding: First, 35 portions of untwisted glass fiber roving are drawn out from the creel 10 and fed into the roller cutter 4. The roller distance is adjusted so that the shear length of the roving is 25 mm. Then adjust the width of the resin tank 3 and the gap between the flowing pastes, put the resin paste in the storage tank into the resin tank, and the resin paste is coated on the upper and lower film carriers under the action of gravity. At this time, start the conveyor belt machine 6, and make the roller cutter and the film roll 5 run synchronously with the conveyor belt machine. After being cut, the roving falls freely onto the resin paste of the lower film. In this way, a sandwich layer prepreg of resin paste-chopped yarn-resin paste is formed between the upper and lower layers of film. The prepreg and the film are combined under the action of the pressure roller 7 to make the resin paste and the fiber penetrate into one, and the air is removed by the adjustment roller 8. It is wound into an SMC roll using the winding device 9; 3. Ripening and packaging: Put the compounded SMC roll into the temperature-adjusting aging room (25-40℃) for aging. When the viscosity increases to the required value, it is the finished SMC product. 4. Pressing and molding: like Figure 5 Figure 6 As shown, a certain amount of prepared SMC molding material is placed in the preheated honeycomb mold, and then the mold is closed at a certain speed. The SMC molding material flows under pressure and fills the entire mold cavity. It is kept at the required temperature and pressure for a certain period of time. When it is cured and shaped under physical and chemical effects and reaches the best performance, the mold is opened and the product is taken out. The production of SMC glass fiber composite materials is completed. Example 3

[0030] like Figure 1 As shown, an SMC glass fiber reinforced composite honeycomb structure double-leaf closed door includes a door leaf main body and a cover plate main body. Both the door leaf main body and the cover plate main body are made of glass fiber reinforced composite materials. The door leaf main body is produced by an advanced honeycomb structure mold. A sealing strip is filled in the gap between the door leaf main body and the middle seam of the door leaf. The door leaf main body is composed of a plurality of unit door leaves. Adjacent unit door leaves are connected by bolts. A honeycomb core plate is arranged on the inner surface of each unit door leaf. The cover plate main body is composed of a plurality of unit cover plates. Adjacent unit cover plates are overlapped with each other and fastened by rivets.

[0031] The present invention adopts compression molding process to produce civil air defense door leaf, which puts a certain amount of compression molding sheet into preheated mold, and after heating and pressurizing, the product has high strength, high geometrical dimension accuracy, and is not deformed by external environment temperature. It is suitable for large-scale and complex structure products.

[0032] like Figure 4 As shown in the figure, the process flow of SMC production mainly includes resin paste preparation, paste operation, fiber cutting, sedimentation and impregnation, resin thickening and other processes, which are mainly divided into the following steps: 1. Preparation of resin paste: Add 35 parts of unsaturated polyester UP into high-speed shear mixer 1 and mix evenly, then add 0.5 parts of initiator CHP, and increase the stirring speed at the same time to make all the raw materials highly dispersed. Then add 2 parts of thickener magnesium hydroxide and 5 parts of release agent calcium stearate, and continue stirring. Then add 45 parts of filler barium sulfate and 15 parts of low shrinkage agent PE, and continue stirring until all the components listed in the formula are dispersed, stop stirring, and let it stand for use. In the process of preparing the resin paste, pay attention to controlling the stirring temperature and the time of adding the thickener to obtain the ideal resin paste viscosity and thickening speed. Finally, put the mixed resin into the resin storage tank 2; 2. Glass fiber cutting, pressure impregnation and winding: First, lead 40 portions of untwisted glass fiber roving from the creel 10 and feed them into the roller cutter 4. Adjust the roller distance so that the shear length of the roving is 25 mm. Then adjust the width of the resin tank 3 and the gap between the flowing pastes, put the resin paste in the storage tank into the resin tank, and the resin paste is coated on the upper and lower film carriers under the action of gravity. At this time, start the conveyor belt machine 6, and make the roller cutter and the film roll 5 run synchronously with the conveyor belt machine. After being cut, the roving falls freely on the resin paste of the lower film. In this way, a sandwich layer prepreg of resin paste-chopped yarn-resin paste is formed between the upper and lower layers of film. Under the action of the pressure roller 7, the prepreg and the film are combined to make the resin paste and the fiber penetrate into one, and the air is removed by the adjustment roller 8. Wind it into an SMC roll with the winding device 9; 3. Ripening and packaging: Put the compounded SMC roll into the temperature-adjusting aging room (25-40℃) for aging. When the viscosity increases to the required value, it is the finished SMC product. 4. Pressing and molding: like Figure 5 Figure 6 As shown, a certain amount of prepared SMC molding material is placed in the preheated honeycomb mold, and then the mold is closed at a certain speed. The SMC molding material flows under pressure and fills the entire mold cavity. It is kept at the required temperature and pressure for a certain period of time. When it is cured and shaped under physical and chemical effects and reaches the best performance, the mold is opened and the product is taken out. The production of SMC glass fiber composite materials is completed.

[0033] Compared with the traditional processing method of suspended swing valve bottom plate, the valve bottom plate processing method using composite materials as raw materials and molding technology as production method has significant advantages. It not only avoids the problem of long production cycle caused by maintenance, but also avoids the problem of uncontrollable product quality stability caused by complex steel welding. It effectively improves the production efficiency and quality stability of valve plate production and reduces the labor intensity of workers.

[0034] This invention combines fiber-reinforced sheet molding compound (SMC) materials with honeycomb structures for the first time in the production of civil air defense door panels. The relevant civil air defense door panels are manufactured through an integral molding process, which features advanced technology, efficient production, and reliable product quality. The honeycomb structure reduces the weight of the door and the size of the door panel, and the overall strength is improved. It has the advantages of light weight, high strength, corrosion resistance, and long life, as well as good insulation, sound insulation, and flame retardancy. It does not incur maintenance costs during use, is easy to install, and saves time and effort. It can play an important role in civil air defense construction.

Claims

1. A double-leaf closed door made of SMC glass fiber reinforced composite honeycomb structure, Features It includes a door leaf body and a cover plate body, both of which are made of SMC glass fiber reinforced composite materials. The door leaf body is molded with an advanced honeycomb structure mold. The gap between the door leaf body and the middle seam of the door leaf body is filled with a sealing strip. The door leaf body is composed of several unit door leaves. Adjacent unit door leaves are connected by bolts, and a honeycomb core plate is set on the inner surface of each unit door leaf. The cover plate body is composed of several unit cover plates, and adjacent unit cover plates are overlapped and fastened by rivets.

2. The SMC glass fiber reinforced composite material as described in claim 1, Features The components of SMC glass fiber reinforced composite materials include 30-40 parts of UP resin, 30-40 parts of glass fiber, 40-50 parts of fillers and various additives such as 0.3-1 parts of initiator, 10-20 parts of low shrinkage agent, 1-2 parts of thickener, 2-10 parts of internal release agent, etc.

3. The SMC glass fiber reinforced composite material according to claim 2, Features 30-40 parts of UP resin are condensed from dibasic acid and diol, and the water content is controlled at 0.1-0.15%.

4. The SMC glass fiber reinforced composite material according to claim 2, Features 30-40 parts of glass fiber, in the form of chopped filaments, untwisted roving, or chopped fiber mat.

5. The SMC glass fiber reinforced composite material according to claim 2, Features 40-50 parts of fillers are carbonates, sulfates, oxides, silicon oxides and silicates.

6. The SMC glass fiber reinforced composite material according to claim 2, Features 0.3-1 part of the initiator is BPO, TBPO, DCP, CHP, etc.

7. The SMC glass fiber reinforced composite material according to claim 2, Features 10-20 parts of low shrinkage agent are PMMA, PS, PVAC, PE, PVC, PCL, PB, etc.

8. The SMC glass fiber reinforced composite material according to claim 2, Features 1-2 parts of the thickener are Group IIA metal oxides.

9. The SMC glass fiber reinforced composite material according to claim 2, Features 2-10 parts of the internal release agent are stearic acid, zinc stearate, magnesium stearate, calcium stearate and the like.

Citation Information

Patent Citations

  • Unsaturated polyester sheet moulding material and preparation method thereof

    CN101058666A

  • Saturated polyester resin for molding compound as shrinking agent and production method thereof

    CN101508828A

  • High-gloss and low-density SMC (Sheet Molding Compound) material suitable for large cavity depth

    CN115449187A

  • Light double-leaf air-tight door

    CN215761312U

Cited By

  • Honeycomb structure composite material and preparation method and application thereof

    CN119682200A

  • Concrete anti-collision wall, construction method, used anti-corrosion plate and preparation method

    CN119754196A