Metal sheath mineral insulated cable and preparation method thereof
By combining high-temperature calcined magnesium oxide and modified silicon nitride, combined with glass fiber and filler, the problems of low use temperature and low voltage resistance of mineral insulated cables are solved, and excellent insulation, fire resistance and Pressure resistance.
Patent Information
- Application Number
- CN202411175734.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing mineral insulated cables have low operating temperature, low voltage resistance and low insulation value, which are mainly due to the impurities and magnetic substances contained in the refired magnesium powder, which leads to poor performance at high temperatures.
Metal sheathed mineral insulated cables are prepared by ball milling and extrusion processes to form excellent insulation, fire resistance and pressure resistance.
By combining high-temperature calcination of magnesium oxide and modified silicon nitride, the insulation performance is improved, glass fiber reinforces the strength and stability of the material, and the filler of the outer protective layer improves the mechanical strength, making excellent insulation and fire resistance. and metal sheathed mineral insulated cable with voltage resistance.
Smart Images

Figure BDA0005010665290000111 
Figure BDA0005010665290000121 
Figure BDA0005010665290000122
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable production and relates to a metal sheathed mineral insulated cable and a preparation method thereof. Background Art
[0002] Mineral insulated (MI) cables are mainly composed of heating conductors, mineral powder (magnesium oxide powder) insulation layers and metal sheaths (stainless steel sheaths, copper sheaths, copper-nickel alloy sheaths, etc.). At present, the mineral powder insulation layer material used in mineral insulated (MI) cables is mainly dead-burned magnesium, which refers to the dense block of periclase formed by magnesium oxide after the carbon dioxide completely escapes when magnesite is calcined at 1800°C. The dead-burned magnesium powder contains impurities and magnetic substances, which causes the heating cables made of it to have technical problems such as low operating temperature, low withstand voltage level and low insulation value. Summary of the invention
[0003] The object of the present invention is to provide a metal sheathed mineral insulated cable and a preparation method thereof. The prepared metal sheathed mineral insulated cable has excellent insulation, fire resistance and pressure resistance.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A metal sheathed mineral insulated cable comprises a conductor, a mineral insulating porcelain column and a metal sheath arranged in sequence from the inside to the outside;
[0006] The conductor is a copper rod, the metal sheath comprises a metal sheath layer and an outer protective layer, wherein the metal sheath layer is made of copper or aluminum, and the mineral insulating porcelain column comprises the following raw materials by weight: 50 to 70 parts of high-temperature calcined magnesium oxide, 5 to 10 parts of glass fiber, and 12 to 18 parts of modified silicon nitride, wherein the preparation process of the modified silicon nitride is as follows:
[0007] S11, heat treating the silicon nitride at 330-350° C. for 20-25 min, and then cooling to room temperature at a rate of 2-5° C. / min to obtain heat-treated silicon nitride;
[0008] S12, adding tantalum silicide into deionized water at a weight ratio of 1:5 and dispersing the mixture evenly, then adding 2-5% of a dispersant and 1-3% of a silane coupling agent KH550 based on the total weight of the tantalum silicide, stirring the mixture for 2-3 hours, filtering and drying the mixture to obtain modified tantalum silicide;
[0009] S13, 20 to 30 parts of heat-treated silicon nitride, 0.5 to 0.8 parts of sodium citrate and 5 to 8 parts of modified tantalum silicide are mixed, and ball milled at a speed of 600 to 700 r / min for 1 to 2 hours. After the ball milling, the mixture is dried and sieved through a 200-mesh sieve to obtain modified silicon nitride.
[0010] As a preferred technical solution of the present invention, in step S12, the dispersant is one of sodium carboxymethyl cellulose, sodium carboxyethyl cellulose and polyethylene glycol 200.
[0011] A method for preparing a metal sheathed mineral insulated cable as claimed in claim 1, comprising the following steps:
[0012] S31, preparing the mineral insulating porcelain column:
[0013] After the magnesium oxide is crushed, the temperature is raised to 1100-1200° C. and calcined for 0.5-1.5 hours to obtain high-temperature calcined magnesium oxide powder, and then naturally cooled to room temperature, and the high-temperature calcined magnesium oxide powder, modified silicon nitride, and glass fiber are mixed according to mass fractions, and after fully stirring, 2-3 parts of a binder are added for molding, and after pressing and molding, a porcelain column precursor is obtained, and the porcelain column precursor is calcined and sintered to obtain the mineral insulation porcelain column;
[0014] S32, mineral insulation porcelain column filling:
[0015] First, bake the mineral insulating porcelain column at 150-200℃ for 2-3h, and when it is naturally cooled to 45-55℃, install the mineral insulating porcelain column between the copper rod and the metal sheath layer by the porcelain column assembly method;
[0016] S33, drawing annealing treatment:
[0017] First, the cable is drawn through a straight drawing machine, and then the drawing and annealing are cycled in sequence, with the annealing temperature being 580-660°C, until the specified outer diameter is reached. Then, the drawn cable is transferred to a disc drawing machine for drawing, and then the drawing and annealing are cycled in sequence, with the annealing temperature being 540-600°C, and the time being 40-60 minutes.
[0018] S34, use an extruder to extrude the outer protective layer:
[0019] The raw materials of the outer protective layer are fully mixed and evenly applied on the outer wall of the metal sheath layer by an extrusion process so that the raw materials are evenly wrapped on the metal sheath layer processed in step S33 to prepare the metal sheathed mineral insulated cable.
[0020] As a preferred technical solution of the present invention, in step S31, the binder is a mixed solution of carboxymethyl cellulose, paraffin oil, ethanol and water in a mass ratio of (0.4-0.6):(1-3):(10-15):(40-50).
[0021] As a preferred technical solution of the present invention, in step S31, the calcination and sintering process is: heating to 580-620°C at a rate of 3-5°C / min and keeping warm for 1-2h, then heating to 1200-1300°C at a rate of 7-10°C / min and keeping warm for 2-3h, naturally cooling to 580-600°C, then heating to 1200-1300°C at a rate of 7-10°C / min and keeping warm for 0.5-1.5h, and finally naturally cooling to 35-45°C.
[0022] As a preferred technical solution of the present invention, in step S34, the specific process of the extrusion process is as follows:
[0023] The uniformly mixed outer protective layer raw materials are placed in an injection molding machine, melted at a temperature of 190-195° C. for 3-5 minutes, then injection molded by the injection molding machine, and then hot pressed at 160-165° C. and a pressure of 17-19 MPa for 10-15 minutes, and then cooled in a water tank.
[0024] As a preferred technical solution of the present invention, in step S34, the raw materials of the outer protective layer include the following components in parts by mass: 25 to 35 parts of polytetrafluoroethylene, 10 to 16 parts of polyaspartic acid ester, 10 to 15 parts of vinyl silazane, 3 to 5 parts of filler, 3 to 5 parts of cross-linking agent, and 1 to 3 parts of plasticizer.
[0025] As a preferred technical solution of the present invention, the plasticizer is one of di(2-ethylhexyl) phthalate and di(2-ethylhexyl) terephthalate, and the crosslinking agent is one of tert-butyl hydroperoxide and dibenzoyl peroxide.
[0026] As a preferred technical solution of the present invention, it is characterized in that the preparation process of the filler is as follows:
[0027] Calcine wollastonite at 450-470°C for 1-2h, then wash with 15% by mass sodium hydroxide solution and dry to obtain pretreated wollastonite; disperse asbestos in a 5mM carbonic acid solution, wherein the mass fraction of asbestos in the carbonic acid solution is 20%, stir for 1-2h, then add zirconium diboride, continue stirring for 1-2h, filter, wash with water, and dry to obtain pretreated asbestos; mix the pretreated wollastonite, pretreated asbestos and aluminum nitride and ball mill them, and after the ball milling is completed, calcine at 700-800°C for 1-2.5h under flowing air to obtain the filler; wherein the mass ratio of the pretreated wollastonite, zirconium diboride, asbestos and aluminum nitride is 5:(1-1.5):(1-2):(2-3).
[0028] In the present invention, magnesium oxide powder, modified silicon nitride and glass fiber are mixed and calcined at high temperature to obtain a mineral insulating porcelain column, wherein tantalum silicide is modified by a silane coupling agent. First, the silane coupling agent can form a special silicon oxide protective film on the surface of tantalum silicide, which not only enhances the surface performance of tantalum silicide, but also optimizes the interface bonding between tantalum silicide and silicon nitride, thereby reducing charge accumulation and leakage at the interface, and improving the overall insulation performance of the mineral insulating porcelain column; and the silane coupling agent can fill the tiny defects and cracks on the surface of tantalum silicide during the modification process, reduce the adverse effects of these defects on the insulation performance, and promote the uniform dispersion of tantalum silicide particles, further improving the density and Insulation effect; by mixing the modified tantalum silicide with the calcined silicon nitride by ball milling, the defects and cracks at the interface can be reduced, and the strength and stability of the modified silicon nitride can be improved; and the grain size of the silicon nitride can be modified to improve the insulation performance of the material; during the ball milling process, sodium citrate is added as a grinding aid. Sodium citrate contains a large number of carboxyl and hydroxyl groups. These functional groups have strong chelating ability and can react with the metal elements in tantalum silicide and silicon nitride to form a stable complex with the metal ions on the surface of the tantalum silicide and silicon nitride particles during the ball milling process, so that the modified tantalum silicide and silicon nitride can be more evenly dispersed, reducing the agglomeration and adhesion between the particles and promoting the refinement of the modified silicon nitride particles.
[0029] By calcining magnesium oxide at high temperature, the purity and stability of magnesium oxide can be improved, and the internal defects of magnesium oxide can be reduced. In addition, the magnesium oxide calcined at high temperature has an extremely high resistivity, thereby greatly improving the insulation of the magnesium oxide material. Glass fiber, as a reinforcing material, has a low dielectric constant. When mixed with magnesium oxide, it can reduce the dielectric constant of the mineral insulating porcelain column and help further optimize the insulation performance of the material. In addition, glass fiber can improve the strength and flexibility of the material, improve the stability of the structure, and increase the service life of the material. Therefore, high-temperature calcined magnesium oxide powder, modified silicon nitride, and glass fiber are formed under the action of a binder, and the calcination process is controlled by different heating rates during the calcination process, and the cooling and insulation process is added at the same time, so that the thermal stress generated during the calcination process can be eliminated, thereby jointly improving the insulation of the mineral insulating porcelain column.
[0030] In the present invention, an outer protective layer is coated outside the metal sheath layer. The main raw materials are polytetrafluoroethylene, polyaspartic acid ester, vinyl silazane and filler. The processing fluidity and mechanical strength of the polymer material are improved by mixing the base material, and the filler obtained by sintering pretreated wollastonite, zirconium diboride, asbestos and aluminum nitride is added thereto. The porosity of the wollastonite in the filler is optimized by alkali treatment, and the surface impurities of the asbestos are removed by acid treatment. The asbestos is then ball-milled and mixed with zirconium diboride, and aluminum nitride is added and sintered to jointly improve the mechanical strength of the outer protective layer.
[0031] Beneficial effects of the present invention:
[0032] In the present invention, magnesium oxide powder, modified silicon nitride and glass fiber are calcined at high temperature, molded, calcined and sintered under the action of a binder to obtain a mineral insulating porcelain column; the mineral insulating porcelain column is then filled between a copper rod and a metal sheath layer by a porcelain column assembly method, and a drawing annealing treatment is performed and an outer protective layer is extruded by an extruder, so that the obtained metal sheathed mineral insulated cable has excellent insulation, fire resistance and pressure resistance. DETAILED DESCRIPTION
[0033] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0034] The polyaspartic acid ester in the present invention was purchased from Chongqing Ruiya Biotechnology Co., Ltd. with the product number of 68479-98-1.
[0035] Example 1
[0036] The conductor is a copper rod, and the material of the metal sheath layer is copper;
[0037] The preparation process of modified silicon nitride is as follows:
[0038] S11, heat treating the silicon nitride at 330° C. for 20 min, and then cooling to room temperature at a rate of 2° C. / min to obtain heat-treated silicon nitride;
[0039] S12, adding tantalum silicide into deionized water at a weight ratio of 1:5 and dispersing the mixture evenly, then adding 2% sodium carboxymethyl cellulose and 1% silane coupling agent KH550 based on the total mass of tantalum silicide, stirring for 2 hours, filtering, and drying to obtain modified tantalum silicide;
[0040] S13, 20 parts of heat-treated silicon nitride, 0.5 parts of sodium citrate and 5 parts of modified tantalum silicide are mixed, and the mixture is ball-milled at a speed of 600 r / min for 1 hour. After the ball-milling, the mixture is dried and sieved through a 200-mesh sieve to obtain modified silicon nitride.
[0041] Preparation of metal sheathed mineral insulated cables:
[0042] S31, preparing the mineral insulating porcelain column:
[0043] According to the mass fraction, 50 parts of magnesium oxide are crushed, heated to 1100°C and calcined for 0.5h to obtain high-temperature calcined magnesium oxide powder, and then naturally cooled to room temperature, and the high-temperature calcined magnesium oxide powder, 5 parts of glass fiber, and 12 parts of modified silicon nitride are mixed, and 2 parts of binder are added after sufficient stirring for molding, and a porcelain column precursor is obtained after pressing and molding, and the porcelain column precursor is calcined and sintered, first heated to 580°C at a rate of 3°C / min and kept warm for 1h, and then heated to 1200°C at a rate of 7°C / min and kept warm for 2h, and then naturally cooled to 580°C and heated to 1200°C at a rate of 7°C / min and kept warm for 0.5h, and finally naturally cooled to 35°C to obtain the mineral insulation porcelain column, wherein the binder is a mixed solution of carboxymethyl cellulose, paraffin oil, ethanol and water with a mass ratio of 0.4:1:10:40;
[0044] S32, mineral insulation porcelain column filling:
[0045] First, bake the mineral insulating porcelain column at 150℃ for 2h, and when it cools naturally to 45℃, install the mineral insulating porcelain column between the copper rod and the metal sheath layer by the porcelain column assembly method;
[0046] S33, drawing annealing treatment:
[0047] First, the cable is drawn through a straight drawing machine, and then cyclically drawn and annealed at a temperature of 580°C until the specified outer diameter is reached. Then, the drawn cable is transferred to a disc drawing machine for drawing, and then cyclically drawn and annealed at a temperature of 540°C for 40 minutes.
[0048] S34, use an extruder to extrude the outer protective layer:
[0049] The raw materials of the outer protective layer are fully mixed in parts by mass: 25 parts of polytetrafluoroethylene, 10 parts of polyaspartic acid ester, 10 parts of vinyl silazane, 3 parts of filler, 3 parts of tert-butyl hydroperoxide, and 1 part of di(2-ethylhexyl) phthalate, and the outer protective layer raw materials are laid on the outer wall of the metal sheath layer by extrusion. The specific process is to place the mixed outer protective layer raw materials in an injection molding machine, melt them at a temperature of 190° C. for 3 minutes, and then perform injection molding through the injection molding machine, and then hot press them at 160° C. and a pressure of 17 MPa for 10 minutes, and then cool them in a water tank so that they are evenly wrapped on the metal sheath layer treated in step S33 to prepare the metal sheathed mineral insulated cable;
[0050] The preparation process of the filler is as follows:
[0051] Calcine wollastonite at 450°C for 1 hour, then wash with 15% by mass sodium hydroxide solution and dry to obtain pretreated wollastonite; disperse asbestos in a 5mM carbonic acid solution, wherein the mass fraction of asbestos in the carbonic acid solution is 20%, stir for 1 hour, then add zirconium diboride, continue stirring for 1 hour, filter, wash with water, and dry to obtain pretreated asbestos; mix the pretreated wollastonite, pretreated asbestos and aluminum nitride and ball mill them, and after the ball milling is completed, calcine at 700°C for 1 hour under flowing air to obtain the filler; wherein the mass ratio of the pretreated wollastonite, zirconium diboride, asbestos and aluminum nitride is 5:1:1:2.
[0052] Example 2
[0053] The conductor is a copper rod, and the metal sheath is made of aluminum;
[0054] The preparation process of modified silicon nitride is as follows:
[0055] S11, heat treating the silicon nitride at 340° C. for 22 min, and then cooling to room temperature at a rate of 3° C. / min to obtain heat-treated silicon nitride;
[0056] S12, adding tantalum silicide into deionized water at a weight ratio of 1:5 and dispersing the mixture evenly, then adding 3% sodium carboxymethyl cellulose and 2% silane coupling agent KH550 based on the total mass of tantalum silicide, stirring for 2.5 hours, filtering and drying to obtain modified tantalum silicide;
[0057] S13, 25 parts of heat-treated silicon nitride, 0.7 parts of sodium citrate and 6 parts of modified tantalum silicide are mixed, and the mixture is ball-milled at a speed of 650 r / min for 1.5 h. After the ball-milling, the mixture is dried and sieved through a 200-mesh sieve to obtain modified silicon nitride.
[0058] Preparation of metal sheathed mineral insulated cables:
[0059] S31, preparing the mineral insulating porcelain column:
[0060] According to the mass fraction, 60 parts of magnesium oxide are crushed, heated to 1150°C and calcined for 1 hour to obtain high-temperature calcined magnesium oxide powder, and then naturally cooled to room temperature, and the high-temperature calcined magnesium oxide powder, 8 parts of glass fiber, and 15 parts of modified silicon nitride are mixed, and 2.5 parts of a binder are added after sufficient stirring for molding, and a porcelain column precursor is obtained after pressing and molding, and the porcelain column precursor is calcined and sintered, first heated to 600°C at a rate of 4°C / min and kept warm for 1.5 hours, and then heated to 1230°C at a rate of 8°C / min and kept warm for 2.5 hours, and then naturally cooled to 590°C and then heated to 1250°C at a rate of 8°C / min and kept warm for 1 hour, and finally naturally cooled to 39°C to obtain the mineral insulation porcelain column, wherein the binder is a mixed solution of carboxymethyl cellulose, paraffin oil, ethanol and water with a mass ratio of 0.5:2:12:45;
[0061] S32, mineral insulation porcelain column filling:
[0062] First, bake the mineral insulating porcelain column at 180℃ for 2.5h, and when it cools naturally to 50℃, install the mineral insulating porcelain column between the copper rod and the metal sheath layer by the porcelain column assembly method;
[0063] S33, drawing annealing treatment:
[0064] First, the cable is drawn through a straight drawing machine, and then cyclically drawn and annealed at a temperature of 610°C until the specified outer diameter is reached. Then, the drawn cable is transferred to a disc drawing machine for drawing, and then cyclically drawn and annealed at a temperature of 560°C for 50 minutes.
[0065] S34, use an extruder to extrude the outer protective layer:
[0066] The raw materials of the outer protective layer: 30 parts of polytetrafluoroethylene, 13 parts of polyaspartic acid ester, 12 parts of vinyl silazane, 4 parts of filler, 4 parts of dibenzoyl peroxide, and 2 parts of di(2-ethylhexyl) phthalate are fully mixed and evenly coated, and the outer protective layer raw materials are laid on the outer wall of the metal sheath layer by an extrusion process. The specific process is to place the mixed outer protective layer raw materials in an injection molding machine, melt them at a temperature of 192° C. for 4 minutes, and then perform injection molding by the injection molding machine, and then hot press them at 163° C. and a pressure of 18 MPa for 13 minutes, and then cool them in a water tank to make them evenly wrapped on the metal sheath layer treated in step S33, so as to prepare the metal sheathed mineral insulated cable;
[0067] The preparation process of the filler is as follows:
[0068] Calcine wollastonite at 460°C for 1.5h, then wash with 15% by mass sodium hydroxide solution and dry to obtain pretreated wollastonite; disperse asbestos in a 5mM carbonic acid solution, wherein the mass fraction of asbestos in the carbonic acid solution is 20%, stir for 1.5h, then add zirconium diboride, continue stirring for 1.5h, filter, wash with water, and dry to obtain pretreated asbestos; mix the pretreated wollastonite, pretreated asbestos and aluminum nitride and ball mill them, and after the ball milling is completed, calcine at 750°C for 2h under flowing air to obtain the filler; wherein the mass ratio of the pretreated wollastonite, zirconium diboride, asbestos and aluminum nitride is 5:1.2:1.5:2.5.
[0069] Example 3
[0070] The conductor is a copper rod, and the material of the metal sheath layer is copper;
[0071] The preparation process of modified silicon nitride is as follows:
[0072] S11, heat treating the silicon nitride at 350° C. for 25 min, and then cooling to room temperature at a rate of 5° C. / min to obtain heat-treated silicon nitride;
[0073] S12, adding tantalum silicide into deionized water at a weight ratio of 1:5 and dispersing the mixture evenly, then adding 5% sodium carboxyethyl cellulose and 3% silane coupling agent KH550 based on the total weight of tantalum silicide, stirring for 3 hours, filtering and drying to obtain modified tantalum silicide;
[0074] S13, 30 parts of heat-treated silicon nitride, 0.8 parts of sodium citrate and 8 parts of modified tantalum silicide are mixed, and the mixture is ball-milled at a speed of 700 r / min for 2 h. After the ball-milling, the mixture is dried and sieved through a 200-mesh sieve to obtain modified silicon nitride.
[0075] Preparation of metal sheathed mineral insulated cables:
[0076] S31, preparing the mineral insulating porcelain column:
[0077] According to the mass fraction, 70 parts of magnesium oxide are crushed, heated to 1200°C and calcined for 1.5 hours to obtain high-temperature calcined magnesium oxide powder, and then naturally cooled to room temperature, and the high-temperature calcined magnesium oxide powder, 10 parts of glass fiber, and 18 parts of modified silicon nitride are mixed, and 3 parts of a binder are added after sufficient stirring for molding, and a porcelain column precursor is obtained after pressing and molding, and the porcelain column precursor is calcined and sintered, first heated to 620°C at a rate of 5°C / min and kept warm for 2 hours, and then heated to 1300°C at a rate of 10°C / min and kept warm for 3 hours, and then naturally cooled to 600°C and heated to 1300°C at a rate of 10°C / min again and kept warm for 1.5 hours, and finally naturally cooled to 45°C to obtain the mineral insulation porcelain column, wherein the binder is a mixed solution of carboxymethyl cellulose, paraffin oil, ethanol and water with a mass ratio of 0.6:3:15:50;
[0078] S32, mineral insulation porcelain column filling:
[0079] First, the mineral insulating porcelain column is baked at 200°C for 3 hours, and when it is naturally cooled to 55°C, the mineral insulating porcelain column is installed between the copper rod and the metal sheath layer by the porcelain column assembly method;
[0080] S33, drawing annealing treatment:
[0081] First, the cable is drawn through a straight drawing machine, and then the drawing and annealing are cycled in sequence, with the annealing temperature at 660°C, until the specified outer diameter is reached. Then, the drawn cable is transferred to a disc drawing machine for drawing, and then the drawing and annealing are cycled in sequence, with the annealing temperature at 600°C and the time for 60 minutes.
[0082] S34, use an extruder to extrude the outer protective layer:
[0083] The raw materials of the outer protective layer: 35 parts of polytetrafluoroethylene, 16 parts of polyaspartic acid ester, 15 parts of vinyl silazane, 5 parts of filler, 5 parts of dibenzoyl peroxide, and 3 parts of di(2-ethylhexyl) terephthalate are fully mixed and evenly coated, and the outer protective layer raw materials are laid on the outer wall of the metal sheath layer by an extrusion process. The specific process is to place the mixed outer protective layer raw materials in an injection molding machine, melt them at a temperature of 195° C. for 5 minutes, and then perform injection molding by the injection molding machine, and then hot press them at 165° C. and a pressure of 19Mpa for 15 minutes, and then cool them in a water tank to make them evenly wrapped on the metal sheath layer treated in step S33, so as to prepare the metal sheathed mineral insulated cable;
[0084] The preparation process of the filler is as follows:
[0085] Calcine wollastonite at 470°C for 2h, then wash with 15% by mass sodium hydroxide solution and dry to obtain pretreated wollastonite; disperse asbestos in a 5mM carbonic acid solution, wherein the mass fraction of asbestos in the carbonic acid solution is 20%, stir for 2h, then add zirconium diboride, continue stirring for 2h, filter, wash with water, and dry to obtain pretreated asbestos; mix the pretreated wollastonite, pretreated asbestos and aluminum nitride and ball mill them, and after ball milling, calcine at 800°C for 2.5h under flowing air to obtain the filler; wherein the mass ratio of the pretreated wollastonite, zirconium diboride, asbestos and aluminum nitride is 5:1.5:2:3.
[0086] Comparative Example 1
[0087] The difference between Comparative Example 1 and Example 1 is that the tantalum silicide in Comparative Example 1 is not modified, and the other operations are the same.
[0088] Comparative Example 2
[0089] The difference between Comparative Example 2 and Example 1 is that the silicon nitride in Comparative Example 2 is not modified, and the other operations are the same.
[0090] Comparative Example 3
[0091] The difference between Comparative Example 3 and Example 1 is that the preparation process of the filler in Comparative Example 3 is as follows: wollastonite, asbestos and aluminum nitride are mixed and ball-milled, and after the ball milling is completed, they are calcined at 700°C for 1 hour under flowing air to obtain the filler; wherein the mass ratio of wollastonite, asbestos and aluminum nitride is 5:1:2, and the other operations are the same.
[0092] Performance Test:
[0093] Water absorption rate: measured by MTSY-4 digital ceramic water absorption rate tester;
[0094] Insulation volume resistivity: refer to GB / T 13033.1-2007;
[0095] Fire resistance: Refer to GB / T 13033.1-2007, the test results are shown in Table 1:
[0096] Table 1
[0097]
[0098]
[0099] Withstand voltage test: According to the withstand voltage test after bending in Article 12.2 and Article 13.2 of GB13033.1-2007 (1250V for 15min), the minimum bending radius of the test examples and comparative examples was measured. The test results are shown in Table 2:
[0100] Table 2
[0101]
[0102] According to Table 2, the standard of the minimum bending radius of the inner side of the cable is 2D when D<7, 3D when 7≤D≤12, 4D when 12≤D≤15, and 6D when D≥15. The data of the embodiment are better than the standard and the comparative example. Therefore, the metal sheathed mineral insulated cable prepared by the present invention has excellent pressure resistance. At the same time, it can be seen from Table 1 that it has excellent insulation and fire resistance.
[0103] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A metal sheathed mineral insulated cable, It is characterized in that From the inside to the outside, it includes a conductor, a mineral insulating porcelain column and a metal sheath arranged in sequence; The conductor is a copper rod, the metal sheath comprises a metal sheath layer and an outer protective layer, wherein the metal sheath layer is made of copper or aluminum, and the mineral insulating porcelain column comprises the following raw materials by weight: 50 to 70 parts of high-temperature calcined magnesium oxide, 5 to 10 parts of glass fiber, and 12 to 18 parts of modified silicon nitride, wherein the preparation process of the modified silicon nitride is as follows: S11, heat treating the silicon nitride at 330-350° C. for 20-25 min, and then cooling to room temperature at a rate of 2-5° C. / min to obtain heat-treated silicon nitride; S12, adding tantalum silicide into deionized water at a weight ratio of 1:5 and dispersing the mixture evenly, then adding 2-5% of a dispersant and 1-3% of a silane coupling agent KH550 based on the total weight of the tantalum silicide, stirring the mixture for 2-3 hours, filtering and drying the mixture to obtain modified tantalum silicide; S13, 20 to 30 parts of heat-treated silicon nitride, 0.5 to 0.8 parts of sodium citrate and 5 to 8 parts of modified tantalum silicide are mixed, and ball milled at a speed of 600 to 700 r / min for 1 to 2 hours. After the ball milling, the mixture is dried and sieved through a 200-mesh sieve to obtain modified silicon nitride.
2. The metal sheathed mineral insulated cable according to claim 1, It is characterized in that In step S12, the dispersant is one of sodium carboxymethyl cellulose, sodium carboxyethyl cellulose and polyethylene glycol 200.
3. A method for preparing a metal sheathed mineral insulated cable according to any one of claims 1 to 2, It is characterized in that The following steps are involved: S31, preparing the mineral insulating porcelain column: After the magnesium oxide is crushed, the temperature is raised to 1100-1200° C. and calcined for 0.5-1.5 hours to obtain high-temperature calcined magnesium oxide powder, and then naturally cooled to room temperature, and the high-temperature calcined magnesium oxide powder, modified silicon nitride, and glass fiber are mixed according to mass fractions, and after fully stirring, 2-3 parts of a binder are added for molding, and after pressing and molding, a porcelain column precursor is obtained, and the porcelain column precursor is calcined and sintered to obtain the mineral insulation porcelain column; S32, mineral insulation porcelain column filling: First, bake the mineral insulating porcelain column at 150-200℃ for 2-3h, and when it is naturally cooled to 45-55℃, install the mineral insulating porcelain column between the copper rod and the metal sheath layer by the porcelain column assembly method; S33, drawing annealing treatment: First, the cable is drawn through a straight drawing machine, and then the drawing and annealing are cycled in sequence, with the annealing temperature being 580-660°C, until the specified outer diameter is reached. Then, the drawn cable is transferred to a disc drawing machine for drawing, and then the drawing and annealing are cycled in sequence, with the annealing temperature being 540-600°C, and the time being 40-60 minutes. S34, use an extruder to extrude the outer protective layer: The raw materials of the outer protective layer are fully mixed and evenly applied on the outer wall of the metal sheath layer by an extrusion process so that the raw materials are evenly wrapped on the metal sheath layer processed in step S33 to prepare the metal sheathed mineral insulated cable.
4. The method for preparing a metal sheathed mineral insulated cable according to claim 3, It is characterized in that In step S31, the binder is a mixed solution of carboxymethyl cellulose, paraffin oil, ethanol and water in a mass ratio of (0.4-0.6):(1-3):(10-15):(40-50).
5. The method for preparing the metal sheathed mineral insulated cable according to claim 3, It is characterized in that In step S31, the calcination and sintering process is: heating to 580-620°C at a rate of 3-5°C / min and keeping warm for 1-2h, then heating to 1200-1300°C at a rate of 7-10°C / min and keeping warm for 2-3h, naturally cooling to 580-600°C, then heating to 1200-1300°C at a rate of 7-10°C / min and keeping warm for 0.5-1.5h, and finally naturally cooling to 35-45°C.
6. The method for preparing the metal sheathed mineral insulated cable according to claim 3, It is characterized in that In step S34, the specific process of the extrusion process is as follows: The uniformly mixed outer protective layer raw materials are placed in an injection molding machine, melted at a temperature of 190-195° C. for 3-5 minutes, then injection molded by the injection molding machine, and then hot pressed at 160-165° C. and a pressure of 17-19 MPa for 10-15 minutes, and then cooled in a water tank.
7. The method for preparing the metal sheathed mineral insulated cable according to claim 3, It is characterized in that In step S34, the raw materials of the outer protective layer include the following components in parts by mass: 25 to 35 parts of polytetrafluoroethylene, 10 to 16 parts of polyaspartic acid ester, 10 to 15 parts of vinyl silazane, 3 to 5 parts of filler, 3 to 5 parts of cross-linking agent, and 1 to 3 parts of plasticizer.
8. The method for preparing the metal sheathed mineral insulated cable according to claim 7, It is characterized in that The plasticizer is one of di(2-ethylhexyl)phthalate and di(2-ethylhexyl)terephthalate, and the crosslinking agent is one of tert-butyl hydroperoxide and dibenzoyl peroxide.
9. The method for preparing a metal sheathed mineral insulated cable according to claim 7, It is characterized in that The preparation process of the filler is as follows: Calcine wollastonite at 450-470°C for 1-2h, then wash with 15% by mass sodium hydroxide solution and dry to obtain pretreated wollastonite; disperse asbestos in a 5mM carbonic acid solution, wherein the mass fraction of asbestos in the carbonic acid solution is 20%, stir for 1-2h, then add zirconium diboride, continue stirring for 1-2h, filter, wash with water, and dry to obtain pretreated asbestos; Pretreated wollastonite, pretreated asbestos and aluminum nitride are mixed and ball-milled, and after the ball-milling is completed, they are calcined at 700-800°C for 1-2.5 hours under flowing air to obtain the filler; wherein the mass ratio of the pretreated wollastonite, zirconium diboride, asbestos and aluminum nitride is 5:(1-1.5):(1-2):(2-3).
Citation Information
Cited By
Mineral magnesium oxide insulated fireproof cable and preparation method thereof
CN121748054A
A mineral magnesium oxide insulated fireproof cable and its preparation method
CN121748054B