Double-layer rolling binder-free supercapacitor electrode and preparation method thereof

Through the preparation method of double-layer roll-free adhesive supercapacitor electrode, the modification of metal foam material and PEI aqueous solution, combined with MWCNT and capacitive activated carbon, the performance reduction problem caused by the use of adhesive in traditional electrodes is solved, and high efficiency is achieved , economical preparation of electrode materials, improves the bondability and energy density of the electrodes.

CN119049891AActive Publication Date: 2024-11-29XIAN XD POWER CAPACITOR CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411212644.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-29
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing supercapacitor electrodes require the use of binders during the preparation process, resulting in increased electrode weight, reduced electron transfer rate and impaired electrochemical performance. The preparation conditions of electrode materials without binders are harsh, expensive, and low output.

Method used

The preparation method of double-layer roll-pressed adhesive-free supercapacitor electrode is adopted. By etching the metal foam material in dilute hydrochloric acid or sodium hydroxide solution, then modified in PEI aqueous solution, MWCNT and capacitive activated carbon are added, and after suction filtration, Double-layer rolling treatment achieves close bonding of electrode materials.

Benefits of technology

The preparation of supercapacitor electrodes without adhesive is realized, which improves the bonding and energy density of the electrodes, simplifies the preparation process, reduces costs, and improves the conductivity and electrochemical properties of the electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049891A_ABST
    Figure CN119049891A_ABST
Patent Text Reader

Abstract

The invention provides a double-layer rolling binder-free supercapacitor electrode and a preparation method thereof, and the method comprises the steps: putting a metal foam material into a diluted hydrochloric acid or sodium hydroxide solution, carrying out the soaking under the assistance of ultrasonic waves, and then carrying out the cleaning and drying, thereby obtaining a metal foam material with a corroded and rough surface; the method comprises the following steps: soaking a metal foam material with a corroded and rough surface in a PEI aqueous solution, and carrying out ultrasonic treatment to obtain a dense and porous modified metal foam material with cohesiveness; taking MWCNT, stirring and dispersing the MWCNT in a PEI aqueous solution to obtain a dispersion liquid A, putting the modified metal foam material into the dispersion liquid A, and standing to obtain a modified MWCNT-loaded porous metal foam material; adding capacitive activated carbon into deionized water, and stirring to obtain dispersion liquid B; adding the dispersion liquid B into the modified MWCNT-loaded porous metal foam material, carrying out suction filtration operation to obtain an activated carbon-loaded electrode material, and drying to obtain an electrode plate; and laminating and rolling two electrode plates with the same shape to obtain the double-layer rolled binder-free supercapacitor electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochemical electrode material preparation, and in particular to a double-layer roll-pressed binder-free supercapacitor electrode and a preparation method thereof. Background Art

[0002] In the field of supercapacitors, the performance of the electrode is one of the key factors affecting the overall performance of the supercapacitor. Traditional supercapacitor electrodes usually require the use of binders during the preparation process, such as polytetrafluoroethylene (PVDF), polytetrafluoroethylene (PTEF), cellulose nanofibers (CNF), styrene-butadiene rubber (SBR) + polyacrylic acid, etc., to ensure close bonding between the electrode materials. However, the addition of binders not only increases the weight of the electrode, but also reduces the electron transfer rate, thereby reducing the overall energy density. It may also have an adverse effect on the conductivity and electrochemical properties of the electrode. Therefore, it is of great significance to study the preparation method of binder-free supercapacitor electrodes.

[0003] In recent years, researchers have been constantly exploring the preparation technology and methods of binder-free electrodes to improve the performance of supercapacitors. For example, many studies have grown active electrode materials on metal substrate materials to achieve binder-free use, such as application number: CN201510706762.8 (a method for preparing a metal-graphene composite porous electrode material), CN202310744599.9 (a three-dimensional porous binder-free electrode material and its preparation method and application); CN202110433457.1 (a method for preparing nickel-cobalt double metal hydroxide @ graphene @ foam nickel composite material without alkali agent) and other methods introduced the growth of active materials on metal current collectors, but there are still some problems in the preparation process, such as harsh high temperature and high pressure conditions, low yield, high cost, and complex preparation process. Therefore, developing a simple, efficient and economical method for preparing binder-free supercapacitor electrodes has important practical application value, and it is an effective method to make the electrode materials themselves closely bonded by physical or chemical methods. Summary of the invention

[0004] The purpose of the present invention is to provide a double-layer roll-pressed binderless supercapacitor electrode and a preparation method thereof, so as to overcome the problem that adding a binder to the electrode material in the prior art reduces the electrochemical activity and the problems that the existing binderless electrode material has harsh technical conditions and complex preparation.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for preparing a double-layer roll-pressed binder-free supercapacitor electrode comprises the following steps:

[0007] (1) placing the metal foam material in a dilute hydrochloric acid or sodium hydroxide solution, soaking it under the assistance of ultrasound, then ultrasonically cleaning it with distilled water and ethanol for several times, and then vacuum drying it to obtain a metal foam material with a rough surface corrosion;

[0008] (2) immersing the metal foam material with rough surface corrosion in a PEI aqueous solution and subjecting it to ultrasonic treatment to obtain a dense, porous and adhesive modified metal foam material;

[0009] (3) taking MWCNT and stirring and dispersing it in a PEI aqueous solution to obtain a dispersion A, placing the modified metal foam material in the dispersion A, and allowing it to stand to obtain a modified MWCNT-loaded porous metal foam material;

[0010] (4) adding the capacitor activated carbon into deionized water and stirring to obtain dispersion B;

[0011] (5) placing the modified MWCNT loaded porous metal foam material into a suction filtration device, adding dispersion B to perform suction filtration to obtain a loaded activated carbon electrode material, and after drying, obtaining an electrode sheet;

[0012] (6) Two electrode sheets of the same shape are laminated and roll-pressed to obtain a double-layer roll-pressed binder-free supercapacitor electrode.

[0013] Furthermore, the metal foam material in step (1) is nickel foam or aluminum foam, and the thickness of the metal foam material is 0.1 mm to 1 mm, and the pore size is 0.05 mm to 0.5 mm.

[0014] Furthermore, in step (1), the concentration of the dilute hydrochloric acid is 1 to 5 mol / L; and the concentration of the sodium hydroxide solution is 0.01 to 0.1 mol / L.

[0015] Furthermore, in step (1), the soaking is carried out for 5 to 60 minutes under the assistance of ultrasound, and the vacuum drying temperature is 60°C.

[0016] Furthermore, in step (2), the molecular weight of PEI is 2000-10000 M.W., the mass concentration of the PEI aqueous solution is 1%-10%, and the ultrasonic treatment time is 30 min.

[0017] Furthermore, in step (3), the mass concentration of the PEI aqueous solution is 1%, and 0.01 to 1 part of MWCNT is added to every 100 parts of the PEI aqueous solution by mass, and the standing time is 6-12 hours.

[0018] Furthermore, in step (4), the particle size of the capacitor activated carbon is 50-200 meshes, and 1-10 parts of capacitor activated carbon are added to every 1000 parts of deionized water by mass, and the stirring time is 1-3 hours.

[0019] Furthermore, in step (5), the drying temperature is 90° C. and the drying time is 1-3 h.

[0020] Furthermore, in step (6), when two electrode sheets of the same shape are laminated, the surfaces of the two electrode sheets with more activated carbon are laminated and rolled, and the thickness of the electrode sheets after rolling is controlled to be 0.08 mm to 0.6 mm. 。

[0021] A double-layer roll-pressed binder-free supercapacitor electrode is prepared by the above-mentioned preparation method.

[0022] Compared with the prior art, the present invention has the following beneficial technical effects:

[0023] The present invention first modifies the current collector to increase more connection sites and adhesion of the active material, and then uses a simple filtration step to evenly load more active materials in the three-dimensional porous current collector to increase the specific capacity, and then uses a double-layer rolling method to prevent the active material from falling off, further improving the adhesion of the electrode. Based on this, the present invention uses physical and chemical methods to make the electrode active material and the conductive additive itself tightly combined, and prepares the supercapacitor electrode material without adding a binder. Compared with the existing binder-free technology based on the in-situ growth of active materials on the substrate, the method of the present invention is simple and easy to operate, with a wide source of raw materials and broad application prospects, specifically:

[0024] (1) The preparation method is simple. The polymer PEI can be more easily combined with the nickel foam etched on the surface by utilizing its adhesiveness and the heavy metal chelating property of its functional group. The modified nickel foam can form a dense and sticky network structure inside. At the same time, the high adhesion and adsorption of PEI make it easier for the active material to combine with the nickel foam.

[0025] (2) Low cost. Commercially mature capacitor activated carbon materials are used. Through the process of reduced pressure filtration, the capacitor activated carbon materials are more easily integrated into the porous mesh of nickel foam, while the problem of poor dispersion of electrode activated carbon materials in water is solved.

[0026] (3) The high-temperature drying process further cross-links the PEI polymer chains, and then undergoes a double-layer rolling process, which makes the nickel foam substrate and the active material more closely bonded, without the need for a binder, thereby improving the internal conductivity and energy density of the electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. The following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0028] Figure 1 Schematic diagram of the preparation process of double-layer roll-pressed binder-free supercapacitor electrodes.

[0029] Figure 2 The charge and discharge curves of the double-layer roll-pressed binder-free electrode material in Example 1 at 1 A / g are shown. DETAILED DESCRIPTION

[0030] The present invention is described in detail below:

[0031] A method for preparing a double-layer roll-pressed binder-free supercapacitor electrode comprises the following steps:

[0032] (1) Surface corrosion treatment of porous metal foam materials: a metal foam material (nickel foam or aluminum foam) with a thickness of 0.1 mm to 1 mm and a pore size of 0.05 mm to 0.5 mm is placed in 1 to 5 mol / L dilute hydrochloric acid or 0.01 to 0.1 mol / L sodium hydroxide solution and ultrasonically soaked for 5 to 60 minutes. The material is ultrasonically cleaned three times with distilled water and ethanol respectively to remove the residual acid and other pollutants on the surface, and then vacuum dried at 60°C to obtain a metal foam material with rough surface corrosion.

[0033] (2) Modifying porous metal foam materials: Take a plurality of metal foam materials of the same size with rough surface corrosion, soak them in a polyethyleneimine (PEI, molecular weight 2000-10000 M.W.) aqueous solution with a mass concentration of 1% to 10%, and ultrasonicate for 30 minutes to obtain a dense, porous and adhesive modified metal foam material.

[0034] (3) 0.01-1 parts by mass of multi-walled carbon nanotubes (MWCNT) are stirred and dispersed in 100 parts of a 1% PEI aqueous solution to prepare a dispersion A. The modified metal foam material in step (2) above is placed in the dispersion A and allowed to stand for 6-12 hours to obtain a modified MWCNT-loaded porous metal foam material.

[0035] (4) Add 1 to 10 parts by mass of capacitor activated carbon with a particle size of 50 to 200 mesh into 1000 parts of deionized water and stir for 1 to 3 hours to obtain dispersion B.

[0036] (5) Place the modified MWCNT-loaded porous metal foam material described in step (3) into a filtration device padded with filter paper, add dispersion B and perform filtration to obtain a loaded activated carbon electrode material, and dry it at 90° C. for 1-3 hours to obtain an electrode sheet.

[0037] (6) Take two electrode sheets of the same shape obtained in step (5), and place the surfaces with more activated carbon on top of each other for roll pressing. After rolling, the thickness of the electrode sheets is controlled to be 0.08 mm to 0.6 mm to obtain a double-layer roll-pressed binder-free electrode material. The electrochemical test shows that the specific capacitance is 31.7 to 89.4 F / g when charged and discharged in the range of 0 to 1.2 V at a current density of 1 A / g.

[0038] The present invention first modifies the current collector to increase more connection sites and adhesion of the active material, and then uses a simple step of suction filtration to evenly load more active materials in the three-dimensional porous current collector to increase the specific capacity, and then uses a double-layer rolling method to prevent the active material from falling off, further improving the adhesion of the electrode. Based on this, the present invention uses physical and chemical methods to make the electrode active material and the conductive additive itself closely combined, and prepares the supercapacitor electrode material without adding a binder. Compared with the existing binder-free technology based on the in-situ growth of active materials on the substrate, the method of the present invention is simple and easy, with a wide source of raw materials and broad application prospects.

[0039] The embodiments of the present invention will be described in detail below in conjunction with the examples. The implementation cases are preferred embodiments of the present invention and should not be used to limit the scope of the present invention. In the following examples, the methods and experimental equipment used are all conventional methods and instruments unless otherwise specified.

[0040] Example 1

[0041] A method for preparing a double-layer roll-pressed binder-free supercapacitor electrode comprises the following steps:

[0042] (1) Surface corrosion treatment of porous nickel foam: a nickel foam with a thickness of 0.1 mm and a pore size distribution of 0.05 mm to 0.5 mm was placed in 1 mol / L dilute hydrochloric acid and immersed in ultrasound for 30 min. The nickel foam was ultrasonically cleaned three times in distilled water and ethanol respectively to remove the residual acid and other pollutants on the surface, and then vacuum dried at 60°C to obtain a nickel foam with a rough surface corrosion.

[0043] (2) Modified porous nickel foam: take a plurality of surface-treated nickel foams of the same size, soak them in a PEI aqueous solution with a mass concentration of 2% (molecular weight 10000 M.W.), and ultrasonicate for 30 minutes to obtain a dense, porous and adhesive modified nickel foam.

[0044] (3) By weight, 0.01 parts by weight of MWCNT was stirred and dispersed in 100 parts by weight of 1% PEI aqueous solution to prepare dispersion A. The modified nickel foam prepared in step (2) above was placed in solution A and allowed to stand for 6 hours to obtain a modified porous nickel foam loaded with MWCNT.

[0045] (4) By weight, add 1 part of capacitor activated carbon with a particle size of 50 mesh into 1000 parts of deionized water and stir for 3 hours to obtain capacitor activated carbon dispersion B.

[0046] (5) The modified MWCNT-loaded porous nickel foam described in step (3) is placed in a filtration device padded with filter paper, and dispersion B is added for filtration to obtain a loaded activated carbon electrode material, which is then dried at 90° C. for 1 h to obtain an electrode sheet.

[0047] (6) Take the two electrode sheets of the same shape as described in step (5), and place the surface with more activated carbon on it and roll it together. The thickness of the electrode sheet is 0.08 mm, and a double-layer roll-pressed binder-free electrode material is obtained. Figure 2 As shown, the electrochemical test was charged and discharged in the range of 0-1.2V at a current density of 1A / g, and its specific capacitance was 58.3F / g.

[0048] Example 2

[0049] A method for preparing a double-layer roll-pressed binder-free supercapacitor electrode comprises the following steps:

[0050] (1) Surface corrosion treatment of porous nickel foam: a nickel foam with a thickness of 1 mm and a pore size distribution of 0.05 mm to 0.5 mm was placed in 5 mol / L dilute hydrochloric acid and immersed in ultrasound for 60 min. Ultrasonic cleaning was performed three times in distilled water and ethanol respectively to remove the residual acid and other pollutants on the surface, and vacuum dried at 60°C to obtain a nickel foam with rough surface corrosion.

[0051] (2) Modified porous nickel foam: take a plurality of surface-treated nickel foams of the same size, soak them in a PEI aqueous solution with a mass concentration of 10% (molecular weight 2000 M.W.), and ultrasonicate for 30 minutes to obtain a dense, porous and adhesive modified nickel foam.

[0052] (3) By weight, 1 part of MWCNT was stirred and dissolved in 100 parts of 1% PEI aqueous solution to prepare dispersion A. The modified nickel foam prepared in step (2) was placed in solution A and allowed to stand for 12 hours to obtain a modified porous nickel foam loaded with MWCNT.

[0053] (4) By weight, 10 parts of capacitor activated carbon with a particle size of 200 mesh were added to 1000 parts of deionized water and stirred for 1 hour to obtain capacitor activated carbon dispersion B.

[0054] (5) The modified MWCNT-loaded porous nickel foam described in step (3) is placed in a filtration device padded with filter paper, and dispersion B is added for filtration to obtain a loaded activated carbon electrode material, which is then dried at 90° C. for 3 h to obtain an electrode sheet.

[0055] (7) Take the two electrode sheets of the same shape as described in step (5), and laminate the surface with more activated carbon for roll pressing. The thickness of the electrode sheet is 0.6 mm, and a double-layer roll-pressed binder-free electrode material is obtained. Electrochemical tests show that the specific capacitance is 86.5 F / g when charged and discharged in the range of 0-1.2 V at a current density of 1 A / g.

[0056] Example 3

[0057] A method for preparing a double-layer roll-pressed binder-free supercapacitor electrode comprises the following steps:

[0058] (1) Surface corrosion treatment of porous aluminum foam: A 0.5 mm thick aluminum foam with a pore size distribution of 0.05 mm to 0.5 mm was placed in a 0.01 mol / L sodium hydroxide solution and immersed in ultrasound for 5 min. Ultrasonic cleaning was performed three times in distilled water and ethanol respectively to remove residual acid and other contaminants on the surface, and vacuum dried at 60°C to obtain aluminum foam with rough surface corrosion.

[0059] (2) Modified porous aluminum foam: take a plurality of aluminum foams of the same size that have been surface treated, immerse them in a PEI aqueous solution with a mass concentration of 10% (molecular weight 5000 M.W.), and ultrasonicate for 30 minutes to obtain a dense, porous modified aluminum foam with adhesion.

[0060] (3) By weight, 0.5 parts of MWCNT were stirred and dissolved in 100 parts of 1% PEI aqueous solution to prepare dispersion A. The modified aluminum foam prepared in step (2) was placed in solution A and allowed to stand for 8 hours to obtain a modified MWCNT-loaded porous aluminum foam.

[0061] (4) By weight, 5 parts of capacitor activated carbon with a particle size of 100 mesh were added to 1000 parts of deionized water and stirred for 2 hours to obtain capacitor activated carbon dispersion B.

[0062] (5) The modified MWCNT-loaded porous aluminum foam described in step (3) is placed in a filtration device padded with filter paper, and dispersion B is added for filtration to obtain a loaded activated carbon electrode material, which is then dried at 90° C. for 1 h to obtain an electrode sheet.

[0063] (6) Take the two electrode sheets of the same shape as described in step (5), and laminate the surface with more activated carbon for roll pressing. The thickness of the electrode sheet is 0.4 mm, and a double-layer roll-pressed binder-free electrode material is obtained. Electrochemical tests show that the specific capacitance is 45.4 F / g when charged and discharged in the range of 0-1.2 V at a current density of 1 A / g.

[0064] Example 4

[0065] A method for preparing a double-layer roll-pressed binder-free supercapacitor electrode comprises the following steps:

[0066] (1) Surface corrosion treatment of porous aluminum foam: A 1 mm thick aluminum foam with a pore size distribution of 0.05 mm to 0.5 mm was placed in a 0.1 mol / L sodium hydroxide solution and immersed in ultrasound for 6 min. Ultrasonic cleaning was performed three times in distilled water and ethanol respectively to remove residual acid and other contaminants on the surface, and vacuum dried at 60°C to obtain aluminum foam with rough surface corrosion.

[0067] (2) Modified porous aluminum foam: take a plurality of aluminum foams of the same size that have been surface treated, immerse them in a PEI aqueous solution with a mass concentration of 1% (molecular weight 10000 M.W.), and ultrasonicate for 30 minutes to obtain a dense, porous modified aluminum foam with adhesion.

[0068] (3) By weight, 0.1 parts of MWCNT were stirred and dissolved in 100 parts of 1% PEI aqueous solution to prepare dispersion A. The modified aluminum foam prepared in step (2) was placed in solution A and allowed to stand for 8 hours to obtain a modified MWCNT-loaded porous aluminum foam.

[0069] (4) By weight, 8 parts of capacitor activated carbon with a particle size of 100 mesh were added to 1000 parts of deionized water and stirred for 2 hours to obtain capacitor activated carbon dispersion B.

[0070] (5) The modified MWCNT-loaded porous aluminum foam described in step (3) is placed in a filtration device padded with filter paper, and dispersion B is added for filtration to obtain a loaded activated carbon electrode material, which is then dried at 90° C. for 2 h to obtain an electrode sheet.

[0071] (6) Take the two electrode sheets of the same shape as described in step (5), and laminate the surface with more activated carbon for roll pressing. The thickness of the electrode sheet is 0.5 mm, and a double-layer roll-pressed binder-free electrode material is obtained. Electrochemical tests show that the specific capacitance is 56.1 F / g when charged and discharged in the range of 0-1.2 V at a current density of 1 A / g.

[0072] Example 5

[0073] A method for preparing a double-layer roll-pressed binder-free supercapacitor electrode comprises the following steps:

[0074] (1) Surface corrosion treatment of porous nickel foam: a nickel foam with a thickness of 1 mm and a pore size distribution of 0.05 mm to 0.5 mm was placed in 2 mol / L dilute hydrochloric acid and immersed in ultrasound for 30 min. The nickel foam was ultrasonically cleaned three times in distilled water and ethanol respectively to remove the residual acid and other pollutants on the surface, and then vacuum dried at 60°C to obtain a nickel foam with a rough surface corrosion.

[0075] (2) Modified porous nickel foam: take a plurality of surface-treated nickel foams of the same size, immerse them in a PEI aqueous solution with a mass concentration of 8% (molecular weight 5000 M.W.), and ultrasonicate for 30 minutes to obtain a dense, porous and adhesive modified nickel foam.

[0076] (3) By weight, 0.8 parts of MWCNT were stirred and dissolved in 100 parts of 1% PEI aqueous solution to prepare dispersion A. The modified nickel foam prepared in step (2) was placed in solution A and allowed to stand for 12 hours to obtain a modified MWCNT-loaded porous nickel foam.

[0077] (4) By weight, 8 parts of capacitor activated carbon with a particle size of 200 mesh were added to 1000 parts of deionized water and stirred for 2 hours to obtain capacitor activated carbon dispersion B.

[0078] (5) The modified MWCNT-loaded porous nickel foam described in step (3) is placed in a filtration device padded with filter paper, and dispersion B is added for filtration to obtain a loaded activated carbon electrode material, which is then dried at 90° C. for 1.5 h to obtain an electrode sheet.

[0079] (7) Take the two electrode sheets of the same shape as described in step (5), and laminate the surface with more activated carbon for roll pressing. The thickness of the electrode sheet is 0.4 mm, and a double-layer roll-pressed binder-free electrode material is obtained. Electrochemical tests show that the specific capacitance is 89.4 F / g when charged and discharged in the range of 0-1.2 V at a current density of 1 A / g.

[0080] Example 6

[0081] A method for preparing a double-layer roll-pressed binder-free supercapacitor electrode comprises the following steps:

[0082] (1) Surface corrosion treatment of porous aluminum foam: A 1 mm thick aluminum foam with a pore size distribution of 0.05 mm to 0.5 mm was placed in a 0.05 mol / L sodium hydroxide solution and immersed in ultrasound for 10 min. The foam was ultrasonically cleaned three times in distilled water and ethanol to remove residual acid and other contaminants on the surface, and then vacuum dried at 60°C to obtain aluminum foam with rough surface corrosion.

[0083] (2) Modified porous aluminum foam: take a plurality of aluminum foams of the same size that have been surface treated, immerse them in a PEI aqueous solution with a mass concentration of 2% (molecular weight 1000 M.W.), and ultrasonicate for 30 minutes to obtain a dense, porous, and adhesive modified aluminum foam.

[0084] (3) By weight, 0.05 parts of MWCNT were stirred and dissolved in 100 parts of 1% PEI aqueous solution to prepare dispersion A. The modified aluminum foam prepared in step (2) was placed in solution A and allowed to stand for 8 hours to obtain a modified MWCNT-loaded porous aluminum foam.

[0085] (4) By weight, add 1 part of capacitor activated carbon with a particle size of 100 mesh into 1000 parts of deionized water and stir for 2 hours to obtain capacitor activated carbon dispersion B.

[0086] (5) The modified MWCNT-loaded porous aluminum foam described in step (3) is placed in a filtration device padded with filter paper, and dispersion B is added for filtration to obtain a loaded activated carbon electrode material, which is then dried at 90° C. for 1 h to obtain an electrode sheet.

[0087] (6) Take the two electrode sheets of the same shape as described in step (5), and laminate the surface with more activated carbon for roll pressing. The thickness of the electrode sheet is 0.4 mm, and a double-layer roll-pressed binder-free electrode material is obtained. Electrochemical tests show that the specific capacitance is 31.7 F / g when charged and discharged in the range of 0-1.2 V at a current density of 1 A / g.

[0088] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing a double-layer roll-pressed binder-free supercapacitor electrode, characterized in that: The following steps are involved: (1) placing the metal foam material in a dilute hydrochloric acid or sodium hydroxide solution, soaking it under the assistance of ultrasound, then ultrasonically cleaning it with distilled water and ethanol for several times, and then vacuum drying it to obtain a metal foam material with a rough surface corrosion; (2) immersing the metal foam material with rough surface corrosion in a PEI aqueous solution and subjecting it to ultrasonic treatment to obtain a dense, porous and adhesive modified metal foam material; (3) taking MWCNT and stirring and dispersing it in a PEI aqueous solution to obtain a dispersion A, placing the modified metal foam material in the dispersion A, and allowing it to stand to obtain a modified MWCNT-loaded porous metal foam material; (4) adding the capacitor activated carbon into deionized water and stirring to obtain dispersion B; (5) placing the modified MWCNT loaded porous metal foam material into a suction filtration device, adding dispersion B to perform suction filtration to obtain a loaded activated carbon electrode material, and after drying, obtaining an electrode sheet; (6) Two electrode sheets of the same shape are laminated and roll-pressed to obtain a double-layer roll-pressed binder-free supercapacitor electrode.

2. The method for preparing a double-layer roll-pressed binder-free supercapacitor electrode according to claim 1, characterized in that: The metal foam material in step (1) is foamed nickel or foamed aluminum, and the thickness of the metal foam material is 0.1 mm to 1 mm, and the pore size is 0.05 mm to 0.5 mm.

3. The method for preparing a double-layer roll-pressed binder-free supercapacitor electrode according to claim 1, characterized in that: The concentration of the dilute hydrochloric acid in step (1) is 1-5 mol / L; the concentration of the sodium hydroxide solution is 0.01-0.1 mol / L.

4. The method for preparing a double-layer roll-pressed binder-free supercapacitor electrode according to claim 1, characterized in that: In step (1), the soaking is carried out for 5 to 60 minutes under the assistance of ultrasound, and the vacuum drying temperature is 60°C.

5. The method for preparing a double-layer roll-pressed binder-free supercapacitor electrode according to claim 1, characterized in that: In step (2), the molecular weight of PEI is 2000-10000 MW, the mass concentration of the PEI aqueous solution is 1%-10%, and the ultrasonic treatment time is 30 minutes.

6. The method for preparing a double-layer roll-pressed binder-free supercapacitor electrode according to claim 1, characterized in that: The mass concentration of the PEI aqueous solution in step (3) is 1%. By mass, 0.01 to 1 part of MWCNT is added to every 100 parts of the PEI aqueous solution, and the standing time is 6 to 12 hours.

7. The method for preparing a double-layer roll-pressed binder-free supercapacitor electrode according to claim 1, characterized in that: In step (4), the particle size of the capacitor activated carbon is 50-200 meshes. By mass, 1-10 parts of capacitor activated carbon are added to every 1000 parts of deionized water, and the stirring time is 1-3 hours.

8. The method for preparing a double-layer roll-pressed binder-free supercapacitor electrode according to claim 1, characterized in that: In step (5), the drying temperature is 90° C. and the drying time is 1-3 h.

9. The method for preparing a double-layer roll-pressed binder-free supercapacitor electrode according to claim 1, characterized in that: When two electrode sheets of the same shape are laminated in step (6), the surfaces of the two electrode sheets with more activated carbon are laminated and rolled. The thickness of the electrode sheets after rolling is controlled to be 0.08 mm to 0.6 mm. 。 10. A double-layer roll-pressed binder-free supercapacitor electrode, characterized in that: The method is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Metal form stack and manufacturing method therefor

    CN106660163A