TiO2-MoO3 nano array catalyst as well as preparation method and application thereof

The TiO2-MoO3 nanoarray catalyst addresses low conversion and separation issues in cyclohexane oxidation by forming a heterostructure with enhanced light absorption and charge separation, improving efficiency and reducing operational costs.

CN119056437APending Publication Date: 2024-12-03GUANGDONG UNIV OF TECH +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411193675.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing cyclohexane oxidation processes in the petroleum industry face low conversion rates, poor selectivity, high energy consumption, and catalyst separation difficulties, leading to inefficiencies and high operational costs.

Method used

A TiO2-MoO3 nanoarray catalyst is developed, forming a heterostructure with TiO2 nanoarrays and MoO3 nanosheets, enhancing light absorption and charge separation through a photothermal synergistic effect, and facilitating easy catalyst recovery by growing it on a glass substrate.

Benefits of technology

The catalyst improves reaction efficiency by reducing activation energy and enhancing conversion rates, while simplifying product separation, thus reducing operational costs and improving the sustainability of the cyclohexane oxidation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056437A_ABST
    Figure CN119056437A_ABST
Patent Text Reader

Abstract

The invention relates to a TiO2-MoO3 composite nano-catalyst as well as a preparation method and application thereof, and belongs to the technical field of catalysts. According to the method, conductive glass is used as a substrate, water, hydrochloric acid and a titanium source are used as raw materials, and a TiO2 nano array is prepared through a hydrothermal method; taking the TiO2 nano array as a substrate, taking water, a glacial acetic acid solution and a molybdenum source as raw materials, and synthesizing a TiO2-MoO3 composite nano array material through a solvothermal method; the defect MoO3 nanosheets with rich surface oxygen vacancies are loaded on the TiO2 nano array, so that the absorption capacity of the composite material to visible light and near-infrared light regions is improved, and the charge separation effect and the photo-thermal synergistic catalytic activity are enhanced; the catalyst is immobilized on glass, so that the separation process of the subsequent reaction is optimized; when the catalyst is applied to a cyclohexane photocatalytic oxidation reaction, the conversion rate and selectivity of the reaction are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts and discloses a composite nano catalyst; specifically, it is a TiO2-MoO3 composite nano catalyst. The invention also discloses a preparation method and application of the catalyst. Background Art

[0002] In the petroleum industry, the oxidation reaction of cyclohexane is a very important reaction. Its oxidation products are cyclohexanone and cyclohexanol (collectively known as KA oil). Cyclohexanol and cyclohexanone are industrially known as KA oil, which are key raw materials for the production of caprolactam, nylon 6, adipic acid, and nylon 66.

[0003] The traditional cyclohexane oxidation industrial route mainly uses soluble cobalt salts as catalysts, and is a thermal catalytic reaction carried out at high temperature (160°C) and high pressure (2MPa). It has the disadvantages of low conversion rate (4% to 6%), poor selectivity (70-80%), and high energy consumption. On the other hand, since the catalyst is difficult to separate, it is very easy to slag in the pipeline, blocking the pipeline, affecting the normal operation of the reaction, and the cleaning cost is very high. Therefore, it is urgent to develop a green and efficient catalyst for the photocatalytic oxidation of cyclohexane to prepare KA oil, so as to improve the efficiency of the production process and promote the sustainable development of the industry.

[0004] In order to address the high energy consumption problem of high temperature and high pressure, patent CN116459840A uses cobalt-based perovskite oxide as a catalyst and optimizes the reaction conditions to 130°C and 1MPa. However, the conversion rate of the catalyst is low and it is difficult to recover, which is not conducive to industrial application.

[0005] In response to the problems of low conversion rate and selectivity, emerging photocatalysts in recent years can improve product conversion by adjusting the energy band position of semiconductors, such as the composite semiconductor catalysts in patents CN111905768A and CN116603528A. However, the former has poor dispersibility and thermal stability as a catalyst powder, and is very easy to agglomerate in the reaction channel, making it difficult to efficiently utilize the spectrum; the latter has a high reaction temperature, high energy consumption, and a relatively complex process, and has a low utilization rate as a large particle catalyst. Summary of the invention

[0006] In view of the problems existing in the prior art, the first purpose of the present invention is to provide a composite photothermal nanoarray catalyst to reduce the conversion rate of photogenerated holes and electrons in TiO2 during the reaction and improve the light absorption band of TiO2. When participating in the reaction, the photogenerated holes in the catalyst are formed into a heterostructure by compounding photocatalytic semiconductors and thermal catalytic semiconductors of different morphologies on the nanoarray. The heterojunction can reduce the recombination rate of photogenerated holes and electrons, while increasing the contact area between the catalyst and the reactant, improving the catalytic activity, and solving the problem of low reaction conversion rate; at the same time, the form of glass-loaded nanoarray also solves the problem of difficult separation of reaction products and powder catalysts.

[0007] The second object of the present invention is to provide a method for preparing a TiO2-MoO3 nanoarray catalyst.

[0008] The third object of the present invention is to provide the application of the above-mentioned TiO2-MoO3 nanoarray catalyst in catalyzing cyclohexane oxidation.

[0009] To this end, the first technical solution provided by the present invention is as follows:

[0010] A method for preparing a TiO2-MoO3 nanoarray catalyst comprises the following steps in sequence:

[0011] S1. Preparation of TiO2 nanoarrays:

[0012] Add titanium source to deionized water, and use hydrochloric acid to adjust the pH of the solution to acidic. Place the cleaned conductive glass obliquely into the prepared precursor solution, and perform hydrothermal reaction at 180°C for 1-10 hours. After ultrasonication, washing, and natural air drying, the reaction product is obtained to obtain a TiO2 nanoarray.

[0013] The molar ratio of the titanium source to the hydrochloric acid is 1:43 to 1:100;

[0014] S2. Preparation of TiO2-MoO3 composite nanocatalyst

[0015] Add a molybdenum source to glacial acetic acid, stir for 45 minutes, then add water and stir again for 15 minutes, place the conductive glass with TiO2 nanoarray in step S1 in the prepared precursor solution, and perform hydrothermal reaction at 150°C for 0.5-8 hours, and obtain a TiO2-MoO3 composite nanocatalyst after ultrasonication, washing, and natural air drying of the reaction product, wherein the morphology of MoO3 is nanosheets;

[0016] The molybdenum source concentration is 9.5mmol / L to 15mmol / L.

[0017] Furthermore, in the above-mentioned method for preparing a TiO2-MoO3 nanoarray catalyst, the titanium source described in step S1 is tetrabutyl titanate.

[0018] Furthermore, in the above-mentioned method for preparing a TiO2-MoO3 nanoarray catalyst, the molybdenum source described in step S2 is molybdenum acetylacetonate.

[0019] Furthermore, in the above-mentioned method for preparing a TiO2-MoO3 nanoarray catalyst, the ultrasonication and cleaning steps in the ultrasonication, cleaning and natural air drying described in step S2 require deionized water as a cleaning agent.

[0020] The second technical solution provided by the present invention is the above-mentioned TiO2-MoO3 nanoarray catalyst, which is prepared by the method provided by the first technical solution.

[0021] The last technical solution of the present invention is to provide the above-mentioned TiO2-MoO3 nanoarray catalyst for application in photothermal catalytic cyclohexane oxidation reaction.

[0022] Compared with the prior art, the technical solution provided by the present invention has the following technical advantages:

[0023] 1. The TiO2-MoO3 nano-array catalyst prepared by the present invention forms a double heterogeneous structure by forming MoO3 nano-sheets on the TiO2 nano-array, and composites the TiO2 nano-array with defective MoO3 nano-sheets. The defective MoO3 sheet has rich carrier concentration due to its abundant oxygen vacancies on its surface, and has absorption capacity in the visible and near-infrared regions and good thermal effect. The TiO2 nano-array catalyst has good conductivity due to its substrate conductive glass, which is conducive to electron transmission, so that its electrons are transferred from the photocatalyst TiO2 array to the photothermal catalyst defective MoO3 nano-sheets, which improves the absorption capacity in the visible and near-infrared regions, enhances the charge separation effect and the photothermal synergistic catalytic activity, and at the same time, growing the catalyst on the glass surface can avoid the difficulty of subsequent separation of the catalyst, saving process costs.

[0024] 2. The technical solution provided by the present invention improves the light absorption effect and thus improves the reaction catalytic efficiency; the photocatalyst and the thermal catalyst are efficiently compounded together through multi-layer nesting of different nanomorphologies (nanoarray nanorods and nanosheets), effectively reducing the activation energy of the reaction, and utilizing the synergistic effect of light and heat to improve its conversion rate; the practicality lies in growing the catalyst on the glass surface, providing a feasible idea for the subsequent separation of the products of cyclohexane oxidation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the structure of the TiO2-MoO3 nanoarray catalyst of the present invention;

[0026] Figure 2 This is the SEM image of TiO3 nanoarray catalyst;

[0027] Figure 3 This is the SEM image of TiO2-MoO3 nanoarray catalyst;

[0028] Figure 4 This is the mapping image of TiO2-MoO3 nanoarray catalyst;

[0029] Figure 5 This is the mapping image of TiO2-MoO3 nanoarray catalyst;

[0030] Figure 6 This is the mapping image of TiO2-MoO3 nanoarray catalyst;

[0031] Figure 7 This is the mapping image of TiO2-MoO3 nanoarray catalyst;

[0032] Figure 8 XRD patterns for structural characterization of TiO2, MoO3 and TiO2-MoO3 nanoarray catalysts;

[0033] Fig. 9 UV-vis graphs for the performance tests of TiO2, MoO3 and TiO2-MoO3 nanoarray catalysts;

[0034] Fig.10 Tauc plots for the performance tests of TiO2, MoO3 and TiO2-MoO3 nanoarray catalysts;

[0035] Fig.11 It is the Mott-Schottky plot of TiO2 nanomaterial;

[0036] Fig.12 It is the Mott-Schottky plot of MoO3 nanomaterial;

[0037] Fig.13 The XPS O1s fine spectra of TiO2 and TiO2-MoO3 nanoarray catalysts;

[0038] Fig.14 This is a comparison chart of the conversion performance of TiO2, MoO3, and TiO2-MoO3 nanoarray catalysts used in photothermal catalytic cyclohexane oxidation reaction;

[0039] Fig.15 A comparison chart of the selectivity performance of TiO2, MoO3, and TiO2-MoO3 nanoarray catalysts in photothermal catalytic cyclohexane oxidation reaction;

[0040] Fig.16This is the gas chromatogram of the TiO2-MoO3-1 nanoarray catalyst applied to the photothermal catalytic cyclohexane oxidation reaction;

[0041] Fig.17 This is the gas chromatogram of TiO2-MoO3-2 nanoarray catalyst applied to photothermal catalytic cyclohexane oxidation reaction;

[0042] Fig.18 This is the gas chromatogram of TiO2-MoO3-3 nanoarray catalyst applied to photothermal catalytic cyclohexane oxidation reaction;

[0043] Fig.19 This is the gas chromatogram of TiO2-MoO3-4 nanoarray catalyst applied to photothermal catalytic cyclohexane oxidation reaction;

[0044] Fig. 20 This is the gas chromatogram of the TiO2 nanoarray catalyst applied to the photothermal catalytic cyclohexane oxidation reaction;

[0045] Fig.21 This is the gas chromatogram of MoO3 nanosheet catalyst applied in photothermal catalytic cyclohexane oxidation reaction. DETAILED DESCRIPTION

[0046] The claims of the present invention are further described in detail below in conjunction with specific embodiments, but do not constitute any limitation to the present invention. Any limited modifications made by anyone within the scope of the claims of the present invention are still within the scope of the claims of the present invention.

[0047] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the present technical field.

[0048] Example 1

[0049] The present embodiment provides a method for preparing a TiO2-MoO3 nanoarray catalyst, comprising the following steps:

[0050] 1) Preparation of TiO2 nanoarrays

[0051] 20 ml of deionized water and 20 ml of concentrated hydrochloric acid were mixed and stirred, and then 0.6 ml of tetrabutyl titanate was added dropwise and stirred for 30 minutes to obtain precursor solution A. The cleaned FTO conductive glass was immersed in the prepared precursor solution A with the conductive surface facing downward, heated to 180°C in a reactor for 1.5 hours, cooled to room temperature, ultrasonically washed with deionized water for 15 minutes, and naturally air-dried to obtain the conductive glass loaded with TiO2 nanoarrays.

[0052] 2) Preparation of TiO2-MoO3 composite nanocatalyst

[0053] 0.114 g of molybdenum acetylacetonate was dissolved in 35 ml of glacial acetic acid, stirred for 45 min, then 2 ml of deionized water was added and stirred for 15 minutes to obtain a precursor solution B. The conductive glass loaded with the TiO2 nanoarray was immersed downward in the precursor solution B, heated at 150°C in a reactor for 0.5 hour, cooled to room temperature, ultrasonically washed with deionized water for 15 minutes, and naturally air-dried to obtain a TiO2-MoO3 composite material, wherein MoO3 was nanosheets.

[0054] Sample characterization:

[0055] The TiO2 nanoarray prepared in step 1) was characterized by SEM, XRD, UV spectrum and Tauc plot. Figure 2 ,pass Figure 2 It is confirmed to be tetragonal system, XRD characterization diagram see Figure 8 ,pass Figure 8 The rutile phase confirmed to be TiO2 showed characteristic peaks containing TiO2, and the UV spectrum ( Fig. 9 )、Tauc plot( Fig.10 ) and the Mott Schottky potential ( Fig.11 ) shows that the prepared TiO2 is an n-type semiconductor with a band gap of 3.12eV. The XPS O1s fine spectrum of the TiO2 nanoarray catalyst ( Fig.13 ) shows that the oxygen vacancy content of the TiO2 array catalyst is 21.08%

[0056] Step 2) The mapping diagram of the TiO2-MoO3 nanoarray catalyst prepared ( Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 ) shows that the M element is evenly distributed on the TiO2 nanoarray, and the morphology SEM ( Figure 3 ) confirmed that MoO3 was loaded on the top of TiO2 nanoarray in the form of nanosheets. XRD pattern ( Figure 8 ) confirmed that the MoO3α-crystalline phase has been successfully prepared. The structural schematic diagram of the TiO2-MoO3 nanoarray catalyst is shown in Figure 1 . UV spectrum ( Fig. 9 )、Tauc plot( Fig.10 ) and Mott-Schottky potential diagram ( Fig.12 ) shows that MoO3 is an n-type semiconductor with a band gap of 3.11 eV ( Fig.12 ), and the potential and band gap confirm that TiO2-MoO3 forms a type II heterojunction. The XPS O1s fine spectrum of the TiO2-MoO3 nanoarray catalyst ( Fig.13 ) showed that the oxygen vacancy content of the TiO2-MoO3 nanoarray catalyst was 23.41%.

[0057] Example 2

[0058] The present embodiment provides a method for preparing a TiO2-MoO3 nanoarray catalyst, comprising the following steps:

[0059] 1) Preparation of TiO2 nanoarrays

[0060] 20 ml of deionized water and 20 ml of concentrated hydrochloric acid were mixed and stirred, and then 0.8 ml of tetrabutyl titanate was added dropwise and stirred for 30 minutes to obtain precursor solution A. The cleaned FTO conductive glass was immersed in the prepared precursor solution A with the conductive surface facing downward, heated to 180°C in a reactor for 1.5 hours, cooled to room temperature, ultrasonically washed with deionized water for 15 minutes, and naturally air-dried to obtain the conductive glass loaded with TiO2 nanoarrays.

[0061] 2) Preparation of TiO2-MoO3 composite nanocatalyst

[0062] 0.114 g of molybdenum acetylacetonate was dissolved in 35 ml of glacial acetic acid, and the mixture was stirred for 45 min, then 2 ml of deionized water was added and stirred for 15 minutes to obtain a precursor solution B. The conductive glass loaded with the TiO2 nanoarray was immersed downward in the precursor solution B, and the mixture was heated at 150° C. in a reactor for 0.5 hour. After cooling to room temperature, the mixture was ultrasonically washed with deionized water for 15 minutes and naturally air-dried to obtain a TiO2-MoO3 composite material, in which MoO3 was nanosheets.

[0063] Example 3

[0064] The present embodiment provides a method for preparing a TiO2-MoO3 nanoarray catalyst, comprising the following steps:

[0065] 1) Preparation of TiO2 nanoarrays

[0066] 20 ml of deionized water and 20 ml of concentrated hydrochloric acid were mixed and stirred, and then 1.2 ml of tetrabutyl titanate was added dropwise and stirred for 10 minutes to obtain precursor solution A. The cleaned FTO conductive glass was immersed in the prepared precursor solution A with the conductive surface facing downward, heated to 180°C in a reactor for 1.5 hours, cooled to room temperature, ultrasonically washed with deionized water for 15 minutes, and naturally air-dried to obtain conductive glass loaded with TiO2 nanoarrays.

[0067] 2) Preparation of TiO2-MoO3 composite nanocatalyst

[0068] 0.228 g of molybdenum acetylacetonate was dissolved in 35 ml of glacial acetic acid, stirred for 45 min, then 2 ml of deionized water was added and stirred for 15 minutes to obtain a precursor solution B. The conductive glass loaded with the TiO2 nanoarray was immersed downward in the precursor solution B, heated at 150° C. in a reactor for 2 hours, cooled to room temperature, ultrasonically washed with deionized water for 15 minutes, and naturally air-dried to obtain a TiO2-MoO3 composite material, wherein MoO3 was nanosheets.

[0069] Example 4

[0070] The present embodiment provides a method for preparing a TiO2-MoO3 nanoarray catalyst, comprising the following steps:

[0071] 1) Preparation of TiO2 nanoarrays

[0072] Mix 20 ml of deionized water and 20 ml of concentrated hydrochloric acid, then add 0.8 ml of tetrabutyl titanate dropwise and stir for 30 minutes. Soak the cleaned FTO conductive glass with the conductive surface facing down in the newly prepared precursor solution A, heat it in a reactor at 180°C for 1.5 hours, cool it to room temperature, ultrasonically wash it with deionized water for 15 minutes, and air dry it naturally to obtain the conductive glass loaded with TiO2 nanoarrays.

[0073] 2) Preparation of TiO2-MoO3 composite nanocatalyst

[0074] 0.228 g of molybdenum acetylacetonate was dissolved in 35 ml of glacial acetic acid, stirred for 45 min, then 2 ml of deionized water was added and stirred for 15 minutes to obtain a precursor solution B. The conductive glass loaded with the TiO2 nanoarray was immersed downward in the precursor solution B, heated at 150° C. in a reactor for 2 hours, cooled to room temperature, ultrasonically washed with deionized water for 15 minutes, and naturally air-dried to obtain a TiO2-MoO3 composite material, wherein MoO3 was nanosheets.

[0075] Application Example 1

[0076] This application example uses the TiO2-MoO3 nanoarray catalyst provided in Example 1 to catalyze the photothermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:

[0077] Dissolve 5 mg of conductive glass loaded with TiO2-MoO3 composite photothermal catalyst in a mixture of 7 mL of cyclohexane and 8 mL of acetonitrile, with the catalyst side facing upwards;

[0078] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120°C; reaction time is 8h; reaction light source is ultraviolet partial area light source (300-780nm) of xenon lamp;

[0079] After the reaction was completed, the product was subjected to gas chromatography ( Fig.16 ) detection, the contents of cyclohexanol and cyclohexanone were determined by the internal standard method, and the conversion rate was calculated to be 9.02% ( Fig.14 ), with a selectivity of 98.75% ( Fig.15 ), and the sample was recorded as TiO2-MoO3-1.

[0080] Application Example 2

[0081] This application example uses the TiO2-MoO3 nanoarray catalyst provided in Example 2 to catalyze the photothermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:

[0082] Dissolve 5 mg of conductive glass loaded with TiO2-MoO3 composite photothermal catalyst in a mixture of 7 mL of cyclohexane and 8 mL of acetonitrile, with the catalyst side facing upwards;

[0083] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120°C; reaction time is 8h; reaction light source is ultraviolet partial area light source (300-780nm) of xenon lamp;

[0084] After the reaction was completed, the product was subjected to gas chromatography ( Fig.17 ) detection, the contents of cyclohexanol and cyclohexanone were determined by the internal standard method, and the conversion rate was calculated to be 8.01% ( Fig.14 ), with a selectivity of 98.66% ( Fig.15 ), and the sample was recorded as TiO2-MoO3-2.

[0085] Application Example 3

[0086] This application example uses the TiO2-MoO3 nanoarray catalyst provided in Example 3 to catalyze the photothermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:

[0087] Dissolve 5 mg of conductive glass loaded with TiO2-MoO3 composite photothermal catalyst in a mixture of 7 mL of cyclohexane and 8 mL of acetonitrile, with the catalyst side facing upwards;

[0088] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120°C; reaction time is 8h; reaction light source is ultraviolet partial area light source (300-780nm) of xenon lamp;

[0089] After the reaction was completed, the product was subjected to gas chromatography ( Fig.18 ) detection, the contents of cyclohexanol and cyclohexanone were determined by the internal standard method, and the conversion rate was calculated to be 8.59% ( Fig.14 ), with a selectivity of 98.70% ( Fig.15 ), and the sample was recorded as TiO2-MoO3-3.

[0090] Application Example 4

[0091] This application example uses the TiO2-MoO3 nanoarray catalyst provided in Example 4 to catalyze the photothermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:

[0092] Dissolve 5 mg of conductive glass loaded with TiO2-MoO3 composite photothermal catalyst in a mixture of 7 mL of cyclohexane and 8 mL of acetonitrile, with the catalyst side facing upwards;

[0093] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120°C; reaction time is 8h; reaction light source is ultraviolet partial area light source (300-780nm) of xenon lamp;

[0094] After the reaction was completed, the product was subjected to gas chromatography ( Fig.19 ) detection, the contents of cyclohexanol and cyclohexanone were determined by the internal standard method, and the conversion rate was calculated to be 8.20% ( Fig.14 ), with a selectivity of 98.50% ( Fig.15 ), and the sample was recorded as TiO2-MoO3-4.

[0095] Comparative application example 1

[0096] This comparative application example uses the TiO2 nanoarray catalyst provided in step S1 of Example 1 to catalyze the photothermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:

[0097] Dissolve 5 mg of conductive glass loaded with TiO2 nanoarray catalyst in a mixture of 7 mL of cyclohexane and 8 mL of acetonitrile, with the catalyst side facing upwards;

[0098] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120°C; reaction time is 8h; reaction light source is ultraviolet partial area light source (300-780nm) of xenon lamp;

[0099] After the reaction was completed, the product was subjected to gas chromatography ( Fig. 20 ) detection, the contents of cyclohexanol and cyclohexanone were determined by the internal standard method, and the conversion rate was calculated to be 6.07% ( Fig.14 ), with a selectivity of 97.89% ( Fig.15 ).

[0100] Comparative Application Example 2

[0101] This application example uses the MoO3 nanosheet catalyst provided in step S2 of Example 1 to catalyze the photothermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:

[0102] Weigh 5 mg of MoO3 and dissolve it in a mixture of 7 mL of cyclohexane and 8 mL of acetonitrile;

[0103] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120℃; reaction time is 8h; reaction light source is ultraviolet partial area light source of xenon lamp (300-780nm)

[0104] After the reaction was completed, the product was subjected to gas chromatography ( Fig.21 ) detection, the contents of cyclohexanol and cyclohexanone were determined by the internal standard method, and the conversion rate was calculated to be 6.79% ( Fig.14 ), with a selectivity of 97.42% ( Fig.15 ).

Claims

1. A method for preparing a TiO2-MoO3 composite nanocatalyst, characterized in that: The following steps are included in sequence: S1. Preparation of TiO2 nanoarrays: Tetrabutyl titanate is added to deionized water, and the pH of the solution is adjusted to acidic to obtain a precursor solution A. The cleaned conductive glass is placed obliquely into the prepared precursor solution A, and a hydrothermal reaction is performed at 170-190° C. for 1-10 hours. The reaction product is subjected to ultrasonication, cleaning, and natural air drying to obtain a conductive glass loaded with TiO2 nanoarrays. S2. Preparation of TiO2-MoO3 composite nanocatalyst: Add molybdenum acetylacetonate to glacial acetic acid, stir for 30-60 minutes to obtain a precursor solution B, add water and stir again for 10-20 minutes, place the conductive glass loaded with TiO2 nanoarray in step S1 in the prepared precursor solution B, and perform hydrothermal reaction at 120-180°C for 0.5-8 hours. After ultrasonic treatment, cleaning, and natural air drying, the reaction product is obtained to obtain a TiO2-MoO3 composite nanocatalyst, wherein the morphology of MoO3 is nanosheets.

2. The method for preparing a TiO2-MoO3 nanoarray catalyst according to claim 1, characterized in that: The molar ratio of tetrabutyl titanate to hydrochloric acid in step S1 is 1:43 to 1:

100.

3. The method for preparing a TiO2-MoO3 nanoarray catalyst according to claim 1, characterized in that: The step S1 of adjusting the pH value of the solution to acidic is to use a hydrochloric acid solution to adjust the pH value of the solution to acidic.

4. The method for preparing a TiO2-MoO3 nanoarray catalyst according to claim 1, characterized in that: The pH value described in step S1 is 2.

5. The method for preparing a TiO2-MoO3 nanoarray catalyst according to claim 3, characterized in that: The hydrochloric acid solution described in step S1 is 3 mol / L.

6. The method for preparing a TiO2-MoO3 nanoarray catalyst according to claim 1, characterized in that: The concentration of the platinum acetylacetonate described in step S2 is 9.5mmol / L to 15mmol / L.

7. The method for preparing a TiO2-MoO3 nanoarray catalyst according to claim 1, characterized in that: The cleaning in steps S1 and S2 uses deionized water as a cleaning agent.

8. A TiO2-MoO3 nanoarray catalyst, characterized in that: The method is prepared by any one of claims 1 to 7.

9. The TiO2-MoO3 nanoarray catalyst according to claim 8 is used for photothermal catalytic cyclohexane oxidation reaction.

Citation Information

Patent Citations

  • MoS2 / MoO3 / TiO2 composite photocatalytic material, and preparation method and application thereof

    CN111905768A

  • Cobalt-based perovskite oxide catalyst and preparation and application thereof

    CN116459840A

  • Large-particle carbon microsphere supported cyclohexane oxidation catalyst as well as preparation method and application thereof

    CN116603528A

  • Method for in-situ growth of MoO3 nano-sheets on ceramic tubes, and gas-sensitive sensor

    CN107337473A

  • Z-type WO3-Co3O4 composite catalytic material as well as preparation method and application thereof

    CN115779919A