Titanium dioxide hollow microspheres as well as preparation method and application thereof

Through the combination of hard template method and hydrothermal method, nano-level rutile phase titanium dioxide hollow microspheres were prepared, which solved the problem of poor performance of titanium dioxide anode material in lithium-ion batteries after high temperature treatment, and achieved high specific surface area and cycling stability. Simplifies the preparation process and reduces costs.

CN119059554AInactive Publication Date: 2024-12-03CYG NEW ENERGY MATERIAL RESEARCH INSTITUTE (GUANGDONG) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411558219.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium-ion battery negative electrode material titanium dioxide forms a large-grain rutile phase after high temperature treatment, resulting in poor conductivity and agglomeration, limiting its application in lithium-ion batteries.

Method used

Using the combination of hard template method and hydrothermal method, the surface of PMMA microspheres is etched and the titanium dioxide layer is coated, and the low-temperature hydrothermal reaction and heat treatment are carried out to prepare nano-level rutile phase titanium dioxide hollow microspheres, increase the specific surface area and control grain assembly , avoid the high-temperature phase transition stage.

Benefits of technology

The high specific surface area, high charge and discharge specific capacity and excellent cycle stability of the hollow titanium dioxide microspheres are achieved. The preparation method is simple, the energy consumption is low, and the cost is not high, which significantly improves the electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059554A_ABST
    Figure CN119059554A_ABST
Patent Text Reader

Abstract

The invention provides titanium dioxide hollow microspheres as well as a preparation method and application thereof, the preparation method comprises the following steps: S1, mixing PMMA (polymethyl methacrylate) microspheres with 10wt% of aqueous alkali, etching, centrifuging, washing and drying to obtain etched PMMA microspheres; s2, mixing the etched PMMA microspheres obtained in S1 with a polyvinyl alcohol aqueous solution, stirring, and heating in a water bath to obtain a solution A; mixing absolute ethyl alcohol, tetrabutyl titanate and glacial acetic acid to form a solution B; and S3, slowly mixing the solution B obtained in the S1 with the solution A, carrying out hydrothermal reaction at 120-180 DEG C for 4-12 hours, centrifuging, washing, drying, and carrying out heat treatment at 80-140 DEG C for 4-6 hours to obtain the titanium dioxide hollow microspheres. The titanium dioxide hollow microspheres provided by the invention are prepared by combining a hard template method and a hydrothermal method, so that the problem that the performance is influenced by large-particle titanium dioxide formed after the materials are calcined in the prior art can be effectively avoided, and the electrochemical performance of the rutile-phase titanium dioxide nano material is fully exerted; and the material has high specific surface area, high charge-discharge specific capacity and excellent cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery materials, and in particular to titanium dioxide hollow microspheres and a preparation method and application thereof. Background Art

[0002] As a clean and renewable energy source, lithium-ion batteries are widely used in consumer electronics, transportation and other fields due to their high energy density, long cycle life and environmental friendliness. However, the positive electrode materials of lithium-ion batteries have been studied relatively extensively and in depth, while the research on negative electrode materials is relatively immature, which has become one of the important factors affecting the development of lithium-ion batteries. At present, the negative electrode materials used in lithium-ion batteries on the market are mainly graphite materials, which easily lead to the formation of a large amount of solid electrolyte membrane (SEI) during use, resulting in a decrease in the first-cycle coulomb efficiency of the material, thereby limiting the application of lithium-ion batteries.

[0003] Titanium is widely distributed in the earth's crust and has abundant reserves. It ranks ninth in the abundance of elements in the earth's crust. Relevant data show that China's ilmenite reserves reached 230 million tons in 2021, ranking first in the world, with the advantages of low cost and abundant resources. Its main oxide, titanium dioxide, has the advantages of abundant raw materials, environmental friendliness, good cycle stability and high safety. It has become one of the negative electrode materials for lithium-ion batteries that has attracted widespread attention in recent years. Titanium dioxide mainly exists in three crystalline structures: anatase, brookite and rutile. Among them, rutile phase titanium dioxide has the smallest band gap (1.78eV) and the largest density (4.13g / cm 3 ), therefore, theoretically, rutile phase titanium dioxide has a higher electronic conductivity, but it was considered unsuitable as a negative electrode material for lithium-ion batteries for a period of time because of its poor lithium conductivity at room temperature, and its high theoretical specific capacity is difficult to fully utilize, thus limiting its large-scale application.

[0004] To solve this problem, commonly used methods include composite graphene materials, mesoporous carbon materials or element doping. However, the above-mentioned preparation methods and processes are relatively complicated and costly. Nanomaterials are considered to be a method to improve the energy storage of titanium dioxide due to their large specific surface area and short diffusion path. However, since titanium dioxide requires a temperature of at least 550°C to undergo a phase transition to form a rutile phase during heat treatment, high temperatures will cause the rutile phase titanium dioxide grains to grow rapidly, forming large particles of rutile phase titanium dioxide with many empty bonds on the surface, which makes it very easy to agglomerate during the preparation and application process, resulting in low catalytic efficiency and its excellent performance cannot be fully utilized.

[0005] Chinese patent CN117004265A "A method for preparing a composite single-shell hollow microsphere filler and its application" discloses a titanium dioxide hollow microsphere that can transform from anatase type to rutile type according to different calcination temperatures, but the patent does not study the conductive properties of the titanium dioxide hollow microsphere.

[0006] Therefore, it is of great significance to develop titanium dioxide hollow microspheres with excellent electrochemical properties and simple preparation method, as well as their preparation method and application. Summary of the invention

[0007] In view of the problems that the existing titanium dioxide nanomaterials have insufficient conductive properties and are prone to agglomeration after forming large particles after calcination, the present invention provides titanium dioxide hollow microspheres and a preparation method and application thereof. By combining a hard template method with a hydrothermal method, the problem that the existing technology and materials form large particles of titanium dioxide after calcination that affects the performance can be effectively avoided, and the electrochemical properties of rutile phase titanium dioxide nanomaterials are fully utilized. The materials have high specific surface area, high charge and discharge specific capacity and excellent cycle stability. The preparation method is simple and has good economic benefits.

[0008] To achieve the above object, the technical solution adopted by the present invention is: A method for preparing hollow titanium dioxide microspheres comprises the following steps: S1. The PMMA microspheres were mixed with a 10wt.% alkaline solution, etched, centrifuged, washed, and dried to obtain etched PMMA microspheres; S2. The etched PMMA microspheres obtained in S1 are mixed with a polyvinyl alcohol aqueous solution, stirred, and heated in a water bath to obtain a liquid A; anhydrous ethanol, tetrabutyl titanate, and glacial acetic acid are mixed to form a liquid B; S3. The liquid B obtained in S1 is slowly mixed with the liquid A, subjected to hydrothermal reaction at 120-180° C. for 4-12 h, centrifuged, washed, dried, and heat treated at 80-140° C. for 4-6 h to obtain the titanium dioxide hollow microspheres.

[0009] Furthermore, the etching treatment temperature in S1 is 30-40° C. and the time is 2-3 hours.

[0010] Furthermore, the amount of PMMA microspheres to be etched in S2 is 3-5 g; and the concentration of the polyvinyl alcohol aqueous solution is 0.01-0.02 g / mL.

[0011] Furthermore, the water bath heating temperature in S2 is 70-80° C. and the heating time is 20-30 min.

[0012] Furthermore, the volume ratio of anhydrous ethanol, tetrabutyl titanate and glacial acetic acid in S2 is (100-200):(5-10):(10-30).

[0013] Furthermore, the mass ratio of liquid B to liquid A in S3 is 1:(2-3).

[0014] Furthermore, the hydrothermal reaction temperature in S3 is 120° C. and the reaction time is 4-8 hours.

[0015] Another object of the present invention is to provide a titanium dioxide hollow microsphere.

[0016] A titanium dioxide hollow microsphere is prepared by any of the above-mentioned methods for preparing titanium dioxide hollow microspheres.

[0017] Furthermore, the titanium dioxide hollow microspheres are in rutile phase.

[0018] Another object of the present invention is to provide an application of titanium dioxide hollow microspheres.

[0019] An application of the aforementioned titanium dioxide hollow microspheres is used for preparing lithium ion battery materials.

[0020] Compared with the prior art, the present invention has the following advantages and beneficial effects: The present application uses PMMA microspheres as hard templates and tetrabutyl titanate as a precursor, and adopts a combination of hard template method and hydrothermal method to coat a titanium dioxide layer on the surface of etched PMMA microspheres to form PMMA@TiO2, which is subjected to hydrothermal reaction and heat treatment to obtain nano-scale rutile phase titanium dioxide hollow microspheres; the specific surface area of ​​the titanium dioxide hollow microspheres is increased by surface etching the PMMA microsphere template, thereby increasing the contact area between the electrode and the electrolyte; the PMMA microspheres with etched surfaces are fully mixed with a polyvinyl alcohol aqueous solution, and then compounded with tetrabutyl titanate to fully and evenly coat the titanium dioxide on the surface of the etched PMMA microspheres to obtain PMMA@TiO2 with uniform particle size and perfect sphericity; at the same time, the hydroxyl groups of the long-chain molecules of polyvinyl alcohol are coordinated with the titanium colloid particles, combined with steric hindrance effect, effectively controlling the assembly process of rutile phase titanium dioxide grains and the growth rate of microspheres, and limiting the size of titanium dioxide hollow microspheres; obtaining rutile phase titanium dioxide hollow microspheres through low-temperature hydrothermal reaction, avoiding the high-temperature phase transition stage from anatase phase to rutile phase of titanium dioxide, thereby avoiding the problem of large particles of titanium dioxide forming after calcination in the prior art and materials that affect the performance; the nanoscale size effectively shortens the diffusion path of lithium ions, making it have excellent electrochemical properties; and effectively removing the attached organic matter produced by the hydrothermal reaction through heat treatment, avoiding the influence on the electrochemical reaction of the titanium dioxide hollow microspheres; the obtained titanium dioxide hollow microspheres have high specific surface area, high charge and discharge specific capacity and excellent cycle stability; the preparation method is simple and easy to operate, with low energy consumption and low cost, and has good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0022] Figure 1 This is the microstructure diagram of titanium dioxide hollow microspheres in Example 1 of the present application.

[0023] Figure 2 This is the XRD diagram of titanium dioxide hollow microspheres in Example 3 of the present application. DETAILED DESCRIPTION

[0024] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention is further described by the following examples. Obviously, the following examples are only part of the embodiments of the present invention, rather than all the embodiments; it should be understood that the embodiments of the present invention are only used to illustrate the technical effects of the present invention, rather than to limit the scope of protection of the present invention.

[0025] The present invention will be specifically described below by examples, and these examples are not intended to limit the present invention in any way. It will be appreciated by those skilled in the art that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods for the unrecorded specific conditions in the following examples are usually performed under normal conditions or according to the conditions recommended by the manufacturer. Unless otherwise indicated, percentages and parts are calculated by weight. The following examples are mainly for a better understanding of the analytical method of the present invention and do not exhaust all operating modes. Parts by weight hereinafter may represent conventional unit measurements in the art, such as kilograms, grams, etc., or may represent ratios between the components, such as mass or weight ratios, etc.

[0026] The raw materials in the examples can all be obtained commercially; unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0027] Embodiment 1: A method for preparing hollow titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with 10wt.% sodium hydroxide solution, stir continuously at 30°C, perform etching treatment for 3h, separate the PMMA microspheres by centrifugation, wash with deionized water 1-3 times, and dry at 60°C for 12h to obtain etched PMMA microspheres; S2. Disperse and dissolve polyvinyl alcohol in deionized water to form a transparent and uniform solution. Mix 3 g of the etched PMMA microspheres obtained in S1 with a 0.02 g / mL polyvinyl alcohol aqueous solution, heat in a water bath at 80°C and stir for 20 min to obtain liquid A. Mix 150 mL of anhydrous ethanol, 5 mL of tetrabutyl titanate and 20 mL of glacial acetic acid to form liquid B. S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 2 parts by mass of liquid A, and perform hydrothermal reaction at 120°C for 6 hours under continuous stirring. Centrifuge, wash, dry, and heat treat at 100°C for 5 hours. Allow to cool naturally to room temperature to obtain the titanium dioxide hollow microspheres.

[0028] Embodiment 2: A method for preparing hollow titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with 10wt.% sodium hydroxide solution, stir continuously at 40°C, perform etching treatment for 2h, separate the PMMA microspheres by centrifugation, wash with deionized water 1-3 times, and dry at 60°C for 12h to obtain etched PMMA microspheres; S2. Disperse and dissolve polyvinyl alcohol in deionized water to form a transparent and uniform solution. Mix 5 g of the etched PMMA microspheres obtained in S1 with a 0.01 g / mL polyvinyl alcohol aqueous solution, heat in a 70°C water bath and stir for 30 min to obtain liquid A. Mix 150 mL of anhydrous ethanol, 10 mL of tetrabutyl titanate and 20 mL of glacial acetic acid to form liquid B. S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 3 parts by mass of liquid A, and perform hydrothermal reaction at 180°C for 4 hours under continuous stirring. Centrifuge, wash, dry, and heat treat at 120°C for 5 hours. Allow to cool naturally to room temperature to obtain the titanium dioxide hollow microspheres.

[0029] Embodiment 3: A method for preparing hollow titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with 10wt.% sodium hydroxide solution, continue stirring at 30°C, perform etching for 2.5h, separate the PMMA microspheres by centrifugation, wash with deionized water 1-3 times, and dry at 60°C for 12h to obtain etched PMMA microspheres; S2. Disperse and dissolve polyvinyl alcohol in deionized water to form a transparent and uniform solution. Mix 4 g of the etched PMMA microspheres obtained in S1 with a 0.02 g / mL polyvinyl alcohol aqueous solution, heat in a 70°C water bath and stir for 25 min to obtain liquid A. Mix 150 mL of anhydrous ethanol, 8 mL of tetrabutyl titanate and 20 mL of glacial acetic acid to form liquid B. S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 2.5 parts by mass of liquid A, and perform hydrothermal reaction at 150°C for 10 hours under continuous stirring. Centrifuge, wash, dry, and heat treat at 80°C for 6 hours. Allow to cool naturally to room temperature to obtain the titanium dioxide hollow microspheres.

[0030] Embodiment 4: A method for preparing hollow titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with 10wt.% sodium hydroxide solution, continue stirring at 40°C, perform etching for 2.5h, separate the PMMA microspheres by centrifugation, wash with deionized water 1-3 times, and dry at 60°C for 12h to obtain etched PMMA microspheres; S2. Disperse and dissolve polyvinyl alcohol in deionized water to form a transparent and uniform solution. Mix 4 g of the etched PMMA microspheres obtained in S1 with a 0.01 g / mL polyvinyl alcohol aqueous solution, heat in a 75°C water bath and stir for 20 min to obtain liquid A. Mix 150 mL of anhydrous ethanol, 6 mL of tetrabutyl titanate and 15 mL of glacial acetic acid to form liquid B. S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 2 parts by mass of liquid A, perform hydrothermal reaction at 120°C for 6 hours under continuous stirring, centrifuge, wash, dry, and heat treat at 120°C for 6 hours, and then cool naturally to room temperature to obtain the titanium dioxide hollow microspheres.

[0031] Embodiment 5: A method for preparing hollow titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with 10wt.% sodium hydroxide solution, stir continuously at 30°C, perform etching treatment for 3h, separate the PMMA microspheres by centrifugation, wash with deionized water 1-3 times, and dry at 60°C for 12h to obtain etched PMMA microspheres; S2. Disperse and dissolve polyvinyl alcohol in deionized water to form a transparent and uniform solution. Mix 5 g of the etched PMMA microspheres obtained in S1 with a 0.01 g / mL polyvinyl alcohol aqueous solution, heat in a water bath at 80°C and stir for 25 min to obtain liquid A. Mix 180 mL of anhydrous ethanol, 9 mL of tetrabutyl titanate and 20 mL of glacial acetic acid to form liquid B. S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 3 parts by mass of liquid A, and perform hydrothermal reaction at 120°C for 8 hours under continuous stirring. Centrifuge, wash, dry, and heat treat at 100°C for 4 hours. Allow to cool naturally to room temperature to obtain the titanium dioxide hollow microspheres.

[0032] Comparative Example 1: A method for preparing hollow titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with deionized water, keep stirring at 30°C, soak for 3 hours, separate the PMMA microspheres, wash with deionized water 1-3 times, and dry at 60°C for 12 hours to obtain PMMA microspheres; S2. Disperse and dissolve polyvinyl alcohol in deionized water to form a transparent and uniform solution. Mix 3 g of PMMA microspheres obtained in S1 with 0.02 g / mL polyvinyl alcohol aqueous solution, heat in a water bath at 80°C and stir for 20 min to obtain liquid A. Mix 150 mL of anhydrous ethanol, 5 mL of tetrabutyl titanate and 20 mL of glacial acetic acid to form liquid B. S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 2 parts by mass of liquid A, and perform hydrothermal reaction at 120°C for 6 hours under continuous stirring. Centrifuge, wash, dry, and heat treat at 100°C for 5 hours. Allow to cool naturally to room temperature to obtain the titanium dioxide hollow microspheres.

[0033] Compared with Example 1, the PMMA microspheres in step S1 of this comparative example were not subjected to etching treatment.

[0034] Comparative Example 2: A method for preparing hollow titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with 10wt.% sodium hydroxide solution, stir continuously at 30°C, perform etching treatment for 3h, separate the PMMA microspheres by centrifugation, wash with deionized water 1-3 times, and dry at 60°C for 12h to obtain etched PMMA microspheres; S2. Disperse and dissolve polyvinyl alcohol in deionized water to form a transparent and uniform solution. Mix 3 g of the etched PMMA microspheres obtained in S1 with a 0.02 g / mL polyvinyl alcohol aqueous solution, heat in a water bath at 80°C and stir for 20 min to obtain liquid A. Mix 150 mL of anhydrous ethanol, 5 mL of tetrabutyl titanate and 20 mL of glacial acetic acid to form liquid B. S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 2 parts by mass of liquid A, centrifuge, wash, dry, heat treat at 100°C for 5h, and allow to cool naturally to room temperature to obtain the titanium dioxide hollow microspheres.

[0035] Compared with Example 1, the hydrothermal reaction is not performed in step S3 of this comparative example.

[0036] Comparative Example 3: A method for preparing hollow titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with 10wt.% sodium hydroxide solution, stir continuously at 30°C, perform etching treatment for 3h, separate the PMMA microspheres by centrifugation, wash with deionized water 1-3 times, and dry at 60°C for 12h to obtain etched PMMA microspheres; S2. Disperse and dissolve polyvinyl alcohol in deionized water to form a transparent and uniform solution to obtain a 0.02 g / mL polyvinyl alcohol aqueous solution, heat and stir in a water bath at 80°C for 20 min to obtain liquid A; mix 150 mL of anhydrous ethanol, 5 mL of tetrabutyl titanate and 20 mL of glacial acetic acid to form liquid B; S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 2 parts by mass of liquid A, and carry out hydrothermal reaction at 120°C for 6 hours under continuous stirring. Mix 3 g of etched PMMA microspheres obtained in S1 with the solution, stir for 1 hour, centrifuge, wash, dry, and heat treat at 100°C for 5 hours. Allow to cool naturally to room temperature to obtain the titanium dioxide hollow microspheres.

[0037] Compared with Example 1, the PMMA microspheres etched in this comparative example are added separately.

[0038] Comparative Example 4: A method for preparing hollow titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with 10wt.% sodium hydroxide solution, stir continuously at 30°C, perform etching treatment for 3h, separate the PMMA microspheres by centrifugation, wash with deionized water 1-3 times, and dry at 60°C for 12h to obtain etched PMMA microspheres; S2. Disperse and dissolve ethylene glycol in deionized water to form a transparent and uniform solution. Mix 3 g of the etched PMMA microspheres obtained in S1 with 0.02 g / mL ethylene glycol aqueous solution, heat in a water bath at 80°C and stir for 20 min to obtain liquid A. Mix 150 mL of anhydrous ethanol, 5 mL of tetrabutyl titanate and 20 mL of glacial acetic acid to form liquid B. S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 2 parts by mass of liquid A, and perform hydrothermal reaction at 120°C for 6 hours under continuous stirring. Centrifuge, wash, dry, and heat treat at 100°C for 5 hours. Allow to cool naturally to room temperature to obtain the titanium dioxide hollow microspheres.

[0039] Compared with Example 1, ethylene glycol is used instead of polyvinyl alcohol in step S2 of this comparative example.

[0040] Comparative Example 5: A method for preparing titanium dioxide microspheres, comprising the following steps: S1. Place an appropriate amount of PMMA microspheres in a beaker, mix with 10wt.% sodium hydroxide solution, stir continuously at 30°C, perform etching treatment for 3h, separate the PMMA microspheres by centrifugation, wash with deionized water 1-3 times, and dry at 60°C for 12h to obtain etched PMMA microspheres; S2. Disperse and dissolve polyvinyl alcohol in deionized water to form a transparent and uniform solution. Mix 3 g of the etched PMMA microspheres obtained in S1 with a 0.02 g / mL polyvinyl alcohol aqueous solution, heat in a water bath at 80°C and stir for 20 min to obtain liquid A. Mix 150 mL of anhydrous ethanol, 5 mL of tetrabutyl titanate and 20 mL of glacial acetic acid to form liquid B. S3. Slowly mix 1 part by mass of liquid B obtained in S1 with 2 parts by mass of liquid A, and perform hydrothermal reaction at 120° C. for 6 h under continuous stirring. Centrifuge, wash, and dry, and then cool naturally to room temperature to obtain the titanium dioxide microspheres.

[0041] Compared with Example 1, step S3 of this comparative example does not perform heat treatment.

[0042] The titanium dioxide hollow microspheres of Example 1 were characterized and analyzed, and the results are as follows: The microstructure of the titanium dioxide hollow microspheres obtained in this example is shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the titanium dioxide hollow microspheres obtained in this example are hollow shell structures with good sphericity and uniform particle sizes of about 100 nm, without obvious agglomeration.

[0043] like Figure 2 As shown, the diffraction peaks of the titanium dioxide hollow microspheres obtained in this example are consistent with the diffraction peaks of the JCPDS standard card (21-1276), and there is no obvious impurity peak, indicating that the prepared sample is pure rutile phase titanium dioxide.

[0044] The test results of the other embodiments are basically consistent with it.

[0045] Electrochemical tests were performed on Examples 1-5 and Comparative Examples 1-5, and the specific test methods are as follows: Titanium dioxide hollow microspheres were mixed with a binder and conductive carbon black to prepare a slurry, which was then coated as the negative electrode material. The battery was assembled in a glove box and placed in an electrolyte solution with current densities of 200 and 1000 mA / g. The negative electrode material was subjected to a constant current charge and discharge cycle test, and its electrochemical properties were measured and calculated.

[0046] The results are shown in the following table:

[0047] After 100 and 300 cycles, the charge-discharge cycle performance was measured and calculated.

[0048] The results are shown in Table 2 below:

[0049] It can be seen from Table 1 and Table 2 above that the titanium dioxide hollow microspheres prepared in each embodiment of the present invention have a charge and discharge specific capacity of more than 240 mAh / g at a current density of 200 mA / g, and a charge and discharge specific capacity of more than 140 mAh / g at a current density of 1000 mA / g. The capacity retention rate is higher than 99% after 100 cycles, and the capacity retention rate is still higher than 95% after 300 cycles, and has excellent electrochemical performance and cycle stability.

[0050] In Comparative Example 1, since the PMMA microspheres were not etched, the specific surface area of ​​the titanium dioxide hollow microspheres was reduced, and its electrochemical performance was poor and the cycle stability was also average; in Comparative Example 2, no hydrothermal reaction was performed, and the hollow titanium dioxide microspheres failed to be converted into rutile phase, and the electrochemical performance and cycle stability were poor; in Comparative Example 3, the etched PMMA microspheres were added after the titanium gel was formed, and the titanium dioxide gel was not fully coated, resulting in the titanium dioxide hollow microspheres of different sizes and thicknesses, affecting their electrochemical performance; in Comparative Example 4, ethylene glycol was used instead of polyvinyl alcohol, and the obtained titanium dioxide hollow microspheres had a larger particle size, and the electrochemical performance could not be compared with those of the embodiments; in Comparative Example 5, no heat treatment was performed, and the attached organic matter produced by the hydrothermal reaction affected the electrochemical reaction of the hollow titanium dioxide microspheres, and the electrochemical performance and cycle stability were poor.

[0051] In summary, the present invention combines a hard template method with a hydrothermal method to coat a titanium dioxide layer on the surface of an etched PMMA microsphere, and then performs a hydrothermal reaction and a heat treatment to obtain nano-scale rutile phase titanium dioxide hollow microspheres; the specific surface area of ​​the titanium dioxide hollow microspheres is increased by performing a surface etching treatment on the PMMA microsphere template; the PMMA microspheres with etched surfaces are fully mixed with a polyvinyl alcohol aqueous solution, and then compounded with tetrabutyl titanate, so that titanium dioxide is fully and evenly coated on the surface of the etched PMMA microspheres; at the same time, the hydroxyl groups of the long-chain molecules of the polyvinyl alcohol are coordinated with the titanium colloid particles, and the steric hindrance effect is combined to effectively control the The assembly process of rutile phase titanium dioxide grains and the growth rate of microspheres limit the size of titanium dioxide hollow microspheres; rutile phase titanium dioxide hollow microspheres are obtained by low-temperature hydrothermal reaction, avoiding the high-temperature phase transition stage from anatase phase to rutile phase of titanium dioxide, so that it has excellent electrochemical properties, and the attached organic matter produced by the hydrothermal reaction is effectively removed by heat treatment to avoid affecting the electrochemical reaction of the titanium dioxide hollow microspheres. The obtained titanium dioxide hollow microspheres have high specific surface area, high charge and discharge specific capacity and excellent cycle stability. The preparation method is simple and easy to operate, low energy consumption, low cost, and has good economic benefits.

[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing hollow titanium dioxide microspheres, characterized in that: The following steps are involved: S1. The PMMA microspheres were mixed with a 10wt.% alkaline solution, etched, centrifuged, washed, and dried to obtain etched PMMA microspheres; S2. The etched PMMA microspheres obtained in S1 are mixed with a polyvinyl alcohol aqueous solution, stirred, and heated in a water bath to obtain a liquid A; anhydrous ethanol, tetrabutyl titanate, and glacial acetic acid are mixed to form a liquid B; S3. The liquid B obtained in S1 is slowly mixed with the liquid A, subjected to hydrothermal reaction at 120-180° C. for 4-12 h, centrifuged, washed, dried, and heat treated at 80-140° C. for 4-6 h to obtain the titanium dioxide hollow microspheres.

2. A method for preparing hollow titanium dioxide microspheres according to claim 1, characterized in that: The etching treatment temperature in S1 is 30-40° C. and the time is 2-3 hours.

3. A method for preparing hollow titanium dioxide microspheres according to claim 1, characterized in that: S2: The amount of PMMA microspheres to be etched is 3-5 g; the concentration of the polyvinyl alcohol aqueous solution is 0.01-0.02 g / mL.

4. A method for preparing hollow titanium dioxide microspheres according to claim 1, characterized in that: The water bath heating temperature in S2 is 70-80°C for 20-30 minutes.

5. A method for preparing hollow titanium dioxide microspheres according to claim 1, characterized in that: The volume ratio of anhydrous ethanol, tetrabutyl titanate and glacial acetic acid in S2 is (100-200):(5-10):(10-30).

6. A method for preparing hollow titanium dioxide microspheres according to claim 1, characterized in that: The mass ratio of liquid B to liquid A in S3 is 1:(2-3).

7. A method for preparing hollow titanium dioxide microspheres according to claim 1, characterized in that: The hydrothermal reaction temperature in S3 is 120° C. and the reaction time is 4-8 hours.

8. A titanium dioxide hollow microsphere, characterized in that: The hollow titanium dioxide microspheres are prepared by the method for preparing the hollow titanium dioxide microspheres according to any one of claims 1 to 7.

9. A titanium dioxide hollow microsphere according to claim 8, characterized in that: The titanium dioxide hollow microspheres are in rutile phase.

10. An application of the titanium dioxide hollow microspheres according to any one of claims 8 to 9, characterized in that: Used to prepare lithium-ion battery materials.

Citation Information

Patent Citations

  • Preparation method of hollow oxide microspheres

    CN107140606A

  • Preparation method and application of composite single-shell hollow microsphere filler

    CN117004265A

  • Preparation of rutile-phase titanium dioxide porous microspheres and application of rutile-phase titanium dioxide porous microspheres in sodium-ion battery

    CN117199332A