Gold-silver alloy nanocluster and application thereof in catalyzing carboxylation reaction of epoxy compound

Through the catalyst supported by gold and silver alloy nanoclusters on activated carbon, combined with the thermochemical strategy, the problems of low catalytic activity and harsh conditions in the carboxylation reaction of carbon dioxide epoxide are solved, and efficient and gentle catalytic effects and catalyst recyclability are achieved. It is suitable for a variety of epoxy substrates, improving the conductivity of cyclic carbonate and the safety of lithium-ion batteries.

CN119060102AActive Publication Date: 2024-12-03ANHUI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411252821.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-03
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The prior art has low catalytic activity in the epoxide carboxylation reaction of carbon dioxide, harsh conditions, poor selectivity, and difficult to recover and utilize the catalyst, limiting the efficient and gentle utilization of carbon dioxide.

Method used

Gold and silver alloy nanocluster [Au13Ag12(PPh3)10Cl8]+ is used as a catalyst. By loading on activated carbon and combining thermochemical strategies, the specific surface area and catalytic performance of the catalyst are improved to achieve efficient carboxylation reaction between epoxy compounds and carbon dioxide.

Benefits of technology

It has achieved efficient catalytic activity, the catalytic yield reaches 90%, the catalytic conditions are mild, the catalyst can be recycled many times, the product has high purity and few impurities, it is suitable for a variety of epoxy substrates, and the conductivity of cyclic carbonate is improved and The safety and cycle life of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060102A_ABST
    Figure CN119060102A_ABST
Patent Text Reader

Abstract

The invention discloses a gold-silver alloy nanocluster and application of the gold-silver alloy nanocluster in catalyzing carboxylation reaction of an epoxy compound. The molecular formula of the gold-silver alloy nanocluster is [Au13Ag12 (PPh3) 10Cl8] < + > (PF6)-, and PPh3 is triphenylphosphine. The catalyst provided by the invention shows very high catalytic activity in a carbon dioxide carboxylation reaction, the catalytic yield of a carrier-free gold-silver alloy nanocluster catalyst is lower than 5%, the catalytic yield of a supported gold-silver alloy nanocluster catalyst reaches 90%, TON reaches 3.06 * 10 < 4 >, the catalytic condition is mild, the catalyst is easy to recycle, and multiple catalytic cycle experiments can be carried out. Meanwhile, the method is suitable for carboxylation reactions of various different epoxy substrates, and corresponding cyclic carbonate products are high in purity and few in impurity quantity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical synthesis, and in particular relates to a gold-silver alloy nanocluster and an application thereof in catalyzing the carboxylation reaction of epoxy compounds. Background Art

[0002] There is a growing interest in the capture and utilization of carbon dioxide, a strategy known as carbon dioxide utilization (CDU). Its advantage is that it uses non-toxic, inexpensive, and energy-rich C1 chemical feedstocks to produce value-added products such as fuels, chemicals, and materials (10.1021 / cr4002758). Therefore, it is of great significance to vigorously develop green carbon dioxide utilization technologies. In the past few years, ligand-protected atomically precise gold nanoclusters (usually Au n (L) m To describe) can be doped with one or several foreign metal atoms (Ag, Cu, Pd, Pt) to maintain the size of the nanocluster, while the synergistic effect of gold and silver in the gold-silver alloy nanocluster triggers efficient catalytic activity (10.1021 / acscatal.0c05681). As a whole, the ligand-protected nanocluster has a clear composition and structure, which is convenient for studying the effects of composition and structure on catalysis at the atomic scale. Zhu's research group found that (AuAg) 21 The catalytic activity of the alloy clusters in the carboxylation of epoxides with carbon dioxide is consistent with that of Au 19 Ag 4 (S-Adm) 15 >Au 21 (S-Adm) 15 >Au 20 Ag 1 (S-Adm) 15 , and proposed that the reason for this phenomenon is that the exposure degree of silver atoms in different clusters is different (10.1002 / anie.202100071). Therefore, efficient and mild strategies to achieve the effective utilization of carbon dioxide have received a lot of attention. Summary of the invention

[0003] Based on the problems existing in the above-mentioned prior art, the present invention provides a gold-silver alloy nanocluster and its application in catalyzing the carboxylation reaction of epoxy compounds. The preparation method of the gold-silver alloy nanocluster of the present invention is simple and has excellent stability. The gold-silver alloy nanocluster catalyst exhibits high catalytic activity in the carboxylation reaction of carbon dioxide with a TON of 3.06×10 4 The catalytic conditions are mild, the catalyst is easy to recycle, multiple catalytic cycle experiments can be carried out, and it is also suitable for the carboxylation reactions of a variety of different epoxy substrates. The corresponding cyclic carbonate products have high purity and a small number of impurities.

[0004] The gold-silver alloy nanoclusters of the present invention have a molecular formula of [Au 13 Ag 12 (PPh 3 ) 10 Cl 8 ] + (PF 6 ) - , where PPh 3 It is triphenylphosphine.

[0005] The method for preparing the gold-silver alloy nanoclusters of the present invention comprises the following steps: S1: Add excess dimethyl sulfide to the methanol solution of chloroauric acid and stir to obtain a white precipitate. After centrifugation, wash it three times with ethanol. By vacuum filtration and drying, a white solid of thioether gold can be obtained.

[0006] S2: The thioether gold obtained in S1 was dissolved in dichloromethane, and triphenylphosphine ligand was added. After thirty minutes, the precipitate was collected by centrifugation, washed, filtered and dried to obtain a white solid gold-phosphine complex.

[0007] S3: Add the white solid gold-phosphine complex obtained in S2 to an organic solvent and mix well, then add a silver source, stir the solution at room temperature and air atmosphere, then drop a sodium borohydride solution into the system, place it in the dark and stir it at room temperature for 15 hours, then centrifuge to remove the black precipitate, vacuum evaporate and dry, add an organic solvent to the obtained solid to wash, remove impurities, obtain a purple-red solution, vacuum evaporate to remove the organic solvent, and obtain Au 13 Ag 12 Clusters, purple solid.

[0008] In S3, the silver source is silver nitrate, and the molar ratio of the gold phosphine complex to the silver source is 1:2.

[0009] The organic solvent is a mixed solvent of methanol and dichloromethane.

[0010] The invention discloses an application of the gold-silver alloy nanoclusters in the carboxylation reaction of epoxy compounds.

[0011] Specifically, activated carbon is used as a carrier, and the gold-silver alloy nanoclusters are loaded on the carrier to obtain a loaded gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac, using the supported catalyst to catalyze the carboxylation reaction of the epoxy substrate.

[0012] The loading process includes the following steps: 49 mg of activated carbon is uniformly dispersed in a dichloromethane solvent to form a suspension, and then 1 mg of purple-red solid Au dispersed in the dichloromethane solvent is added. 13 Ag 12The clusters were stirred at room temperature for 1 hour, and the black solid was collected by centrifugation. After vacuum filtration and drying, the supported gold-silver alloy nanocluster catalyst Au was obtained. 13 Ag 12 / Ac, with a loading of 2wt%.

[0013] The synthetic route for the carboxylation reaction of epoxy substrates is as follows:

[0014] Wherein, R is selected from phenyl, allyloxy or 4-fluorophenyl.

[0015] The co-catalyst is selected from tetrabutylammonium bromide, tetrabutylammonium iodide or potassium iodide.

[0016] The carboxylation reaction includes the following steps: The supported gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac was mixed with the epoxy compound, stirred and heated, and atmospheric pressure carbon dioxide was introduced. The reaction was carried out at 65-75°C for 10 hours. After the reaction was completed, the reaction mixture was cooled to room temperature and the catalyst Au was separated by centrifugation. 13 Ag 12 / Ac, and extracted with ethyl acetate to obtain the cyclic carbonate product.

[0017] The present invention adopts a thermochemical strategy to fix carbon dioxide, and the specific surface area of ​​the gold-silver alloy nanocluster catalyst with activated carbon as the carrier is increased, which greatly enhances the catalytic performance of the carboxylation reaction of epoxy compounds and carbon dioxide. The obtained cyclic carbonate can be used as an electrolyte, has a high electrical conductivity, can provide a sufficient ion transfer rate, and ensure the migration of lithium ions between the positive and negative electrodes. In addition, the cyclic carbonate electrolyte also has a lower viscosity and better chemical stability, can improve the safety and cycle life of lithium ion batteries, so cyclic carbonate is a commonly used lithium ion battery electrolyte.

[0018] The beneficial effects of the present invention are embodied in: 1. Compared with cobalt, zinc, and nickel complex catalysts, the gold-silver alloy nanocluster catalyst of the present invention is basically non-toxic. As a highly efficient heterogeneous catalyst, it has a high specific surface area and can show high recyclability and long-term stability under many harsh conditions.

[0019] 2. The gold-silver alloy nanocluster catalyst of the present invention exhibits high catalytic activity in the carbon dioxide carboxylation reaction. The catalytic yield of the unsupported gold-silver alloy nanocluster catalyst is less than 5%, while the catalytic yield of the supported gold-silver alloy nanocluster catalyst is 90%, and the TON is 3.06×10 4 .

[0020] 3. The catalytic conditions of the present invention are mild, which overcomes the problems of harsh carbon dioxide carboxylation reaction conditions, poor selectivity and low yield. The catalyst can be recycled and can be used for more than 8 times of carbon dioxide carboxylation reaction, which has high economic and environmental benefits.

[0021] 4. The gold-silver alloy nanocluster catalyst of the present invention is simultaneously applicable to the carboxylation reaction of a variety of different epoxy substrates, and the corresponding cyclic carbonate products have high purity and a small amount of impurities. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a single crystal structure diagram of the gold-silver alloy nanocluster of the present invention.

[0023] Figure 2 It is the ultraviolet absorption spectrum of the gold-silver alloy nanoclusters of the present invention.

[0024] Figure 3 This is the hydrogen nuclear magnetic resonance spectrum of styrene carbonate prepared in Example 8.

[0025] Figure 4 The hydrogen nuclear magnetic resonance spectrum of 4-((allyloxy)methyl)-1,3-dioxolan-2-one prepared in Example 9.

[0026] Figure 5 This is the hydrogen nuclear magnetic resonance spectrum of 4-(4-fluorophenyl)-1,3-dioxolane-2-one prepared in Example 10. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further explained below in conjunction with specific embodiments.

[0028] Example 1: Gold-silver alloy nanoclusters Au 13 Ag 12 Preparation 1. Add 400 µL HAuCl 4 ·4H 2 Add 200 µL excess Me 2 S dimethyl sulfide was stirred to obtain a white precipitate, which was centrifuged and washed three times with ethanol. The sulfide gold Au (Me 2 S)Cl as a white solid.

[0029] 2. 301 mg Au(Me 2 S)Cl thioether gold was dissolved in 20 mL of dichloromethane and 334 mg of (PPh 3 ) triphenylphosphine ligand, and after 30 minutes, centrifuge, wash, filter and collect the precipitate, and dry it to obtain a white solid Au(PPh 3 )Cl gold phosphine complex.

[0030] 3. Add 50 mg Au(PPh 3 )Cl gold phosphine complex was added to a mixed solution of 10 mL dichloromethane and 10 mL methanol, stirred evenly, and then 32 mg AgNO 3 Silver nitrate, stir the solution at room temperature in air atmosphere, and then add 5 mL of NaBH 4 (6 mg) sodium borohydride methanol solution, placed in the dark and stirred at room temperature for 15 hours, then centrifuged to remove the black precipitate, and evaporated to dryness in vacuum. The obtained solid was washed with 1:2 (V / V) dichloromethane and methanol to remove impurities, and a purple-red solution was obtained. The organic solvent was removed by vacuum evaporation to obtain Au 13 Ag 12 Clusters, purple solid.

[0031] Example 2: Supported gold-silver alloy nanocluster catalyst Au 13 Ag 12 Preparation of / Ac 1. Disperse 49 mg of activated carbon evenly in 15 mL of dichloromethane solvent to form a suspension. Then add 1 mg of purple-red solid Au dispersed in dichloromethane solvent. 13 Ag 12 The clusters were stirred at room temperature for 1 hour, and the black solid was collected by centrifugation. After vacuum filtration and drying, the supported gold-silver alloy nanocluster catalyst Au was obtained. 13 Ag 12 / Ac, with a loading of 2wt%.

[0032] Example 3: Unsupported Au-Ag Alloy Nanocluster Catalyst Au 13 Ag 12 Catalytic Synthesis of Styrene Carbonate 1. Add 600 mg of raw material styrene oxide and 160 mg of co-catalyst tetrabutylammonium bromide in a molar ratio of 10:1 into a 10 mL Schlenk tube, and then add unloaded gold-silver alloy nanocluster catalyst Au 13 Ag 12 (1 mg, 0.145 µmol). The Schlenk tube was sealed with a rubber stopper and evacuated using a vacuum pump to remove the trapped air. A carbon dioxide balloon was attached. After stirring at 65 °C for 10 hours, the reaction mixture was cooled to room temperature and the carbon dioxide balloon was removed.

[0033] 2. Dissolve the reaction mixture with a solvent (such as ethyl acetate), remove the catalyst by centrifugation (10,000 rpm), and obtain the target product styrene carbonate. The yield is less than 5% as determined by gas chromatography (GC).

[0034] Example 4: Au 13 Ag 12 / Ac catalytic synthesis of styrene carbonate (co-catalyst is tetrabutylammonium bromide) 1. Add 600 mg of raw material styrene oxide and 160 mg of co-catalyst tetrabutylammonium bromide in a molar ratio of 10:1 into a 10 mL Schlenk tube, and then add the supported gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac (20 mg, 2 wt%). The Schlenk tube was sealed with a rubber stopper and evacuated using a vacuum pump to remove the remaining air. A carbon dioxide balloon was attached. After stirring at 65 °C for 10 hours, the reaction mixture was cooled to room temperature and the carbon dioxide balloon was removed.

[0035] 2. Dissolve the reaction mixture with a solvent (such as ethyl acetate), remove the catalyst by centrifugation (10,000 rpm), and obtain the target product styrene carbonate. The yield is 90% as determined by gas chromatography (GC).

[0036] Example 5: Au 13 Ag 12 / Ac catalytic synthesis of styrene carbonate (co-catalyst is tetrabutylammonium iodide) 1. Add 600 mg of raw material styrene oxide and 184 mg of co-catalyst tetrabutylammonium iodide in a molar ratio of 10:1 into a 10 mL Schlenk tube, and then add the supported gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac (20 mg, 2 wt%). The Schlenk tube was sealed with a rubber stopper and evacuated using a vacuum pump to remove the remaining air. A carbon dioxide balloon was attached. After stirring at 65 °C for 10 hours, the reaction mixture was cooled to room temperature and the carbon dioxide balloon was removed.

[0037] 2. Dissolve the reaction mixture with a solvent (such as ethyl acetate), remove the catalyst by centrifugation (10,000 rpm), and obtain the target product styrene carbonate. The yield is 46% as determined by gas chromatography (GC).

[0038] Example 6: Au 13 Ag 12 / Ac catalytic synthesis of styrene carbonate (co-catalyst is potassium iodide) 1. Put 600 mg of raw material styrene oxide and 83 mg of co-catalyst potassium iodide into a 10 mL Schlenk tube at a molar ratio of 10:1, and then add the supported gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac (20 mg, 2 wt%). The Schlenk tube was sealed with a rubber stopper and evacuated using a vacuum pump to remove the remaining air. A carbon dioxide balloon was attached. After stirring at 65 °C for 10 hours, the reaction mixture was cooled to room temperature and the carbon dioxide balloon was removed.

[0039] 2. Dissolve the reaction mixture with a solvent (such as ethyl acetate), remove the catalyst by centrifugation (10,000 rpm), and obtain the target product styrene carbonate. The yield is 14% as determined by gas chromatography (GC).

[0040] Example 7: Recycling experiment: Recycling Au 13 Ag 12 / Ac Synthesis of Styrene Carbonate 1. After completing the fresh experiment of synthesizing styrene carbonate, the Au separated by centrifugation 13 Ag 12 / Ac was washed with dichloromethane three times and vacuum dried at 60°C for 8 hours. Then 600 mg of new raw material styrene oxide and 160 mg of co-catalyst tetrabutylammonium bromide were added, and the recovered gold-silver alloy nanoclusters were used as catalysts. The Schlenk tube was sealed with a rubber stopper and evacuated using a vacuum pump to remove residual air. A carbon dioxide balloon was tied. At 65 o After stirring at 400 °C for 10 hours, the reaction mixture was cooled to room temperature and the carbon dioxide balloon was removed. The reaction mixture was dissolved with a solvent (such as ethyl acetate), and the catalyst was removed by centrifugation (10,000 rpm) to obtain the target product styrene carbonate, and the yield was 88% as determined by gas chromatography (GC).

[0041] 2. Repeat the experiment with the recovered catalyst under the above reaction conditions until the 8th cycle of the experiment, dissolve the reaction mixture with a solvent (such as ethyl acetate), remove the catalyst by centrifugation (10,000 rpm), and obtain the target product styrene carbonate. The yield is determined by gas chromatography (GC) to be 80%.

[0042] Example 8: Au 13 Ag 12 Synthesis of Styrene Carbonate Catalyzed by Ac 1. Add 600 mg of raw material styrene oxide and 160 mg of co-catalyst tetrabutylammonium bromide in a molar ratio of 10:1 into a 10 mL Schlenk tube, and then add the supported gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac (20 mg, 2 wt%). The Schlenk tube was sealed with a rubber stopper and evacuated using a vacuum pump to remove the remaining air. A carbon dioxide balloon was attached. After stirring at 65°C for 10 hours, the reaction mixture was cooled to room temperature and the carbon dioxide balloon was removed.

[0043] 2. Dissolve the reaction mixture with a solvent (such as ethyl acetate), remove the catalyst by centrifugation (10,000 rpm), and obtain the target product styrene carbonate. The yield is 90% as determined by gas chromatography (GC). Subsequently, an appropriate separation method (such as silica gel column chromatography) is used to purify the sample.

[0044] Figure 3 It is the hydrogen nuclear magnetic resonance spectrum of styrene carbonate of the present invention.

[0045] 1H NMR (400 MHz, CDCl 3 ) δ 7.58 - 7.17 (m, 5H), 5.67 (t, J = 8.0 Hz, 1H), 4.80 (t, J = 8.4 Hz, 1H), 4.34 (t, J = 8.3 Hz, 1H).

[0046] Example 9: Au 13 Ag 12 Synthesis of 4-((allyloxy)methyl)-1,3-dioxolane-2-one catalyzed by Ac 1. Add 570 mg of raw material allyl glycidyl ether and 160 mg of co-catalyst tetrabutylammonium bromide in a molar ratio of 10:1 into a 10 mL Schlenk tube, and then add the supported gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac (20 mg, 2 wt%). The Schlenk tube was sealed with a rubber stopper and evacuated using a vacuum pump to remove the remaining air. A carbon dioxide balloon was attached. After stirring at 65°C for 10 hours, the reaction mixture was cooled to room temperature and the carbon dioxide balloon was removed.

[0047] 2. Dissolve the reaction mixture with a solvent (such as ethyl acetate), remove the catalyst by centrifugation (10,000 rpm), and obtain the target product 4-((allyloxy)methyl)-1,3-dioxolane-2-one. The yield is 97% as determined by gas chromatography (GC). Subsequently, an appropriate separation method (such as silica gel column chromatography) is used to purify the sample.

[0048] Figure 4 This is the hydrogen nuclear magnetic resonance spectrum of 4-((allyloxy)methyl)-1,3-dioxolan-2-one.

[0049] 1 H NMR (400 MHz, CDCl 3 ) δ 5.86 (m, 1H), 5.27 (d, J = 17.1 Hz, 1H), 5.21 (d, J = 10.3 Hz, 1H), 4.82 (p, J = 7.9, 4.0, 1.9 Hz, 1H), 4.49 (t, J =8.4 Hz, 1H), 4.39 (t, J = 7.2 Hz, 1H), 4.07 - 4.00 (m, 2H), 3.68 (dd, J =11.0, 3.7 Hz, 2H), 3.60 (dd, J = 11.0, 3.8 Hz, 1H).

[0050] Example 10: Au 13 Ag 12 Synthesis of 4-(4-fluorophenyl)-1,3-dioxolane-2-one catalyzed by Ac 1. Add 690 mg of raw material 4-fluorostyrene epoxide and 160 mg of co-catalyst tetrabutylammonium bromide in a molar ratio of 10:1 into a 10 mL Schlenk tube, and then add the supported gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac (20 mg, 2 wt%). The Schlenk tube was sealed with a rubber stopper and evacuated using a vacuum pump to remove the remaining air. A carbon dioxide balloon was attached. After stirring at 65°C for 10 hours, the reaction mixture was cooled to room temperature and the carbon dioxide balloon was removed.

[0051] 2. Dissolve the reaction mixture with a solvent (such as ethyl acetate), remove the catalyst by centrifugation (10,000 rpm), and obtain the target product 4-(4-fluorophenyl)-1,3-dioxolane-2-one. The yield is 75% as determined by gas chromatography (GC). Then, use an appropriate separation method (such as silica gel column chromatography) to purify the sample.

[0052] Figure 5 This is the hydrogen nuclear magnetic resonance spectrum of 4-(4-fluorophenyl)-1,3-dioxolane-2-one.

[0053] 1H NMR (400 MHz, CD 2 Cl 2) δ 7.69 - 6.74 (m, 4H), 5.66 (t, J = 8.0 Hz,1H), 4.78 (t, J = 8.4 Hz, 1H), 4.31 (t, J = 8.0 Hz, 1H)。

Claims

1. A gold-silver alloy nanocluster, characterized in that: The molecular formula of the gold-silver alloy nanocluster is [Au 13 Ag 12 (PPh3) 10 Cl8] + (PF6) - , wherein PPh3 represents triphenylphosphine.

2. The method for preparing the gold-silver alloy nanoclusters according to claim 1, characterized in that The steps include: S1: Add excess dimethyl sulfide to a methanol solution of chloroauric acid and stir to obtain a white precipitate, which is then centrifuged and washed with ethanol, filtered under reduced pressure and dried to obtain thioether gold; S2: dissolving the thioether gold obtained in S1 in dichloromethane, adding triphenylphosphine ligand, and after 30 minutes, centrifuging, washing, collecting the precipitate by suction filtration and drying to obtain a white solid gold-phosphine complex; S3: Add the white solid gold-phosphine complex obtained in S2 to an organic solvent and mix well, then add a silver source, stir the solution at room temperature and air atmosphere, then drop a sodium borohydride solution into the system, place it in the dark and stir it at room temperature for 15 hours, then centrifuge to remove the black precipitate, vacuum evaporate and dry, add an organic solvent to the obtained solid to wash, remove impurities, obtain a purple-red solution, vacuum evaporate to remove the organic solvent, and obtain Au 13 Ag 12 Clusters, purple solid.

3. The preparation method according to claim 2, characterized in that: In S3, the silver source is silver nitrate.

4. The preparation method according to claim 3, characterized in that: The molar ratio of the gold phosphine complex to the silver source is 1:

2.

5. Use of the gold-silver alloy nanoclusters according to claim 1 in catalyzing the carboxylation reaction of epoxy compounds.

6. The use according to claim 5, characterized in that: Using activated carbon as a carrier, the gold-silver alloy nanoclusters are loaded on the carrier to obtain a loaded gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac, using the supported catalyst to catalyze the carboxylation reaction of the epoxide compound.

7. The use according to claim 6, characterized in that: The loading process includes the following steps: 49 mg of activated carbon is uniformly dispersed in a dichloromethane solvent to form a suspension, and then 1 mg of purple-red solid Au dispersed in the dichloromethane solvent is added. 13 Ag 12 The clusters were stirred at room temperature for 1 hour, and the black solid was collected by centrifugation. After vacuum filtration and drying, the supported gold-silver alloy nanocluster catalyst Au was obtained. 13 Ag 12 / Ac, with a loading of 2 wt%.

8. The use according to claim 6, characterized in that: The carboxylation reaction includes the following steps: In the presence of a co-catalyst, the supported gold-silver alloy nanocluster catalyst Au 13 Ag 12 / Ac is mixed with the epoxy compound, stirred and heated, and atmospheric pressure carbon dioxide is introduced to react at 65-75°C. After the reaction is completed, the reaction mixture is cooled to room temperature and the catalyst Au is separated by centrifugation. 13 Ag 12 / Ac, dichloromethane extraction to obtain cyclic carbonate product; The synthetic route is as follows: ; Wherein, R is selected from phenyl, allyloxy or 4-fluorophenyl.

9. The use according to claim 8, characterized in that: The co-catalyst is selected from tetrabutylammonium bromide, tetrabutylammonium iodide or potassium iodide.

Citation Information

Patent Citations

  • Gold-silver nanocluster catalyst for acetylene hydrochlorination

    CN112007696A

  • Supported Au-Ag nanocluster catalyst and application thereof in ketone alkynylation reaction

    CN115041236A

  • Silver nanocluster and application thereof in epoxy addition reaction of styrene oxide and CO2

    CN118206591A