Sulfonic acid functionalized polymer, ion exchange membrane and application thereof
By grafting the sulfonic acid group onto the benzene ring of an alkoxy group or an oxy substituent in the styrene polymer, the problems of high water absorption and poor stability of the material in the prior art are solved, and the water resistance of the material is improved Resolvability and mechanical properties are suitable for fuel cells, flow batteries and other fields.
Patent Information
- Application Number
- CN202411213428.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing sulfonic acid functionalized styrene polymers have high water absorption, large swelling, poor hydrolysis resistance, free radical resistance and oxidation resistance in applications, resulting in a decrease in barrier properties and mechanical properties of the ion exchange membrane. The preparation process is complex and easy to introduce impurities.
The sulfonic acid functionalized polymer is prepared by grafting the sulfonic acid group through an alkyl, fluoroalkyl or aryl onto a benzene ring with an alkoxy or an oxy substituent, using gentle reaction conditions to avoid The introduction of multivalent cationic impurities and the cross-linking side reactions of alkylation form a long side chain structure to improve the stability and processing performance of the material.
It significantly improves the material's oxidation resistance, radical resistance and hydrolysis resistance, reduces water absorption, improves the dimensional stability and mechanical properties of the polymer under high humidity conditions, and enhances the electrochemical properties.
Smart Images

Figure CN119060221A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ion exchange membranes, and in particular to a sulfonic acid functionalized polymer, an ion exchange membrane and applications thereof. Background Art
[0002] Clean energy technologies such as fuel cell technology, water electrolysis hydrogen production technology, lithium battery and flow battery technology are crucial to the sustainable development of global energy. Ion exchange membranes, as key materials, are widely used in these fields. Aromatic polymers have the advantages of wide sources, controllable costs and diverse structures. After introducing functional groups such as sulfonic acid and phosphoric acid, they can be used as ion exchange resins to prepare ion exchange membranes. Functionalized styrene polymers are one of the earliest ion exchange resins developed and applied, and are widely studied for ion exchange membranes.
[0003] Functionalized styrene polymers have the advantage of low cost in application, but their stability is very unsatisfactory. At present, functionalized styrene polymers with sulfonic acid functional groups directly grafted on the main chain benzene ring have high water absorption, large swelling, poor stability such as hydrolysis resistance, free radical resistance, and oxidation resistance. Excessive swelling will sharply reduce the barrier properties and mechanical properties of ion exchange membranes, limiting their application in the fields of fuel cell ion exchange membranes, liquid flow battery diaphragms, and water electrolysis hydrogen production diaphragms. In addition, the current preparation method of sulfonic acid functional group styrene polymers has some defects, such as easy to cause cross-linking side reactions, harsh reaction conditions, complex preparation process, impurities are easy to remain in the product and difficult to remove, etc. Summary of the invention
[0004] The present invention is based on the inventors' discovery and understanding of the following facts and problems: the current sulfonic acid functionalized styrene polymers have high water absorption, large swelling, poor stability in hydrolysis resistance, free radical resistance, antioxidant properties, etc., and excessive water absorption and swelling will also sharply reduce the barrier properties and mechanical properties of the ion exchange membrane.
[0005] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, the embodiments of the present invention propose a sulfonic acid functionalized polymer, an ion exchange membrane and its application. In the side chain structure of the sulfonic acid functionalized polymer, the sulfonic acid group is grafted to the benzene ring with an alkoxy or oxy substituent through an alkyl, fluoroalkyl or aryl group. Compared with the sulfonic acid group directly grafted to the benzene ring or the sulfonic acid group directly grafted to the benzene ring through an alkyl, fluoroalkyl or aryl group, the reaction conditions are more mild and controllable, and multivalent cationic impurities will not be introduced to poison the ion transmission capacity, and alkylation cross-linking side reactions will not be generated to destroy the linear structure of the polymer, and it has better dissolution and processing performance. The long side chain structure can promote the formation of an ordered phase separation structure, improve the stability of the main chain structure, significantly improve the oxidation resistance, free radical resistance and hydrolysis resistance of the material, and reduce the water absorption rate of the material, thereby improving the dimensional stability of the polymer under high humidity conditions and enhancing the mechanical properties and electrochemical properties of the material.
[0006] The embodiment of the present invention provides a sulfonic acid functionalized polymer, wherein the sulfonic acid functionalized polymer comprises a repeating unit A0 represented by formula (1):
[0007]
[0008] Wherein, R1 is selected from H or F; R2 is selected from H, F or CH3; a is selected from an integer of 0 to 12; and R3 is selected from an alkyl sulfonic acid, a fluoroalkyl sulfonic acid or an aryl sulfonic acid.
[0009] Advantages and technical effects of the sulfonic acid functionalized polymers of the embodiments of the present invention: In the side chain structure of the sulfonic acid functionalized polymer, the sulfonic acid group is grafted onto the benzene ring with an alkoxy or oxy substituent through an alkyl, fluoroalkyl or aryl group. Compared with the sulfonic acid group being directly grafted onto the benzene ring or the sulfonic acid group being directly grafted onto the benzene ring through an alkyl, fluoroalkyl or aryl group, the reaction conditions are milder and more controllable, and sulfonic acid functionalized polymers with different ion exchange capacities can be prepared according to the number of active sites. Multivalent cationic impurities will not be introduced to poison the ion transmission capacity, and alkylation cross-linking side reactions will not be generated to destroy the linear structure of the polymer. The product structure is clear and has better dissolution and processing performance. The long side chain structure can promote the formation of an ordered phase separation structure, improve the stability of the main chain structure, significantly improve the oxidation resistance, free radical resistance and hydrolysis resistance of the material, and reduce the water absorption rate of the material, thereby improving the dimensional stability of the polymer under high humidity conditions and enhancing the mechanical and electrochemical properties of the material.
[0010] In some embodiments, R3 is selected from at least one of the following structural formulas:
[0011]
[0012] Among them, M +is selected from cations; b is selected from integers of 0 to 6; c is selected from integers of 0 to 12;
[0013] R4~R 17 Each independently selected from H, F, C1-C6 alkyl, C1-C6 perfluoroalkyl or C6-C 12 The aromatic group.
[0014] In some embodiments, the sulfonic acid functionalized polymer further comprises repeating unit A1:
[0015]
[0016] wherein R1 is selected from H or F; R2 is selected from H, F or CH3; R 18 Selected from H, C1~C 12 Alkyl, C1-C6 perfluoroalkyl or C6-C 12 The aromatic group;
[0017] and / or, the sulfonic acid functionalized polymer further comprises a repeating unit A2, wherein the repeating unit A2 comprises at least one of -C(CH3)2CH-, -CH2CH2-, -CH(CH3)CH2- or -CH(CH2CH3)CH2-;
[0018] And / or, the sulfonic acid functionalized polymer further comprises repeating unit A3:
[0019]
[0020] In the formula, R1 is selected from H or F; R2 is selected from H, F or CH3; a is selected from an integer of 0 to 12;
[0021] R 19 An alkoxy group selected from -OH, -F, -Cl, -Br, -I or C1-C4.
[0022] In some embodiments, the molar percentage of the repeating unit A0 in the repeating unit containing a benzene ring of the sulfonic acid functionalized polymer is defined as the sulfonation degree of the sulfonic acid functionalized polymer, and the sulfonation degree is ≥ 0.1%;
[0023] and / or, the sulfonic acid functionalized polymer has a n 30,000 to 1,000,000;
[0024] and / or, the sulfonic acid functionalized polymer has a w 30,000 to 1,500,000;
[0025] And / or, the EW of the sulfonic acid functionalized polymer is 244 to 5000 g / mol.
[0026] The embodiment of the present invention provides a method for preparing a sulfonic acid functionalized polymer, comprising: subjecting a hydroxyl functionalized styrene polymer to a sulfonation reaction with a hydrogen extraction reagent and a sulfonation reagent to obtain the sulfonic acid functionalized polymer.
[0027] In the embodiment of the present invention, a sulfonation reaction is carried out by a hydroxyl-functionalized styrene polymer with a hydrogen extraction agent and a sulfonation agent, and a group containing a sulfonic acid functional group is grafted onto a benzene ring having an alkoxy or oxy substituent. The reaction conditions are mild, the reaction degree is high, the reaction product has few side reactions, and there is no residual multivalent cation poisoning the product ion transmission capacity, and there is no alkyl cross-linking side reaction that causes the product to be unable to dissolve and process, and good processing and molding performance is maintained. The sulfonation degree of the product is controllable, and the chemical structure of the product is clear, which is conducive to the preparation of functional material products with stable performance.
[0028] In some embodiments, the hydrogen extraction agent includes at least one of an alkali metal oxide, an alkali metal hydride, an alkali metal peroxide, an alkali metal hydroxide, an alkali metal carbonate, or an alkali metal organic compound;
[0029] And / or, the sulfonated reagent comprises at least one of the following structural formulas:
[0030]
[0031] Among them, R4~R 17 Each independently selected from H, F, C1-C6 alkyl, C1-C6 perfluoroalkyl or C6-C 12 b is an integer selected from 0 to 6; c is an integer selected from 0 to 12; M + is selected from cations; and X is selected from halogens.
[0032] In some embodiments, the molar ratio of the hydroxyl functional group in the hydroxyl functionalized styrene polymer to the sulfonated agent is 1:0.1 to 30;
[0033] and / or, the molar ratio of the hydroxyl functional group in the hydroxyl functionalized styrene polymer to the hydrogen extraction agent is 1:0.1-20;
[0034] And / or, the temperature of the sulfonation reaction is 20-160°C;
[0035] And / or, the sulfonation reaction time is 0.5-72h.
[0036] An embodiment of the present invention provides an ion exchange membrane, comprising the sulfonic acid functionalized polymer described in the embodiment of the present invention or the sulfonic acid functionalized polymer prepared by the preparation method described in the embodiment of the present invention.
[0037] In the embodiment of the present invention, the ion exchange membrane has all the advantages of the sulfonic acid functionalized polymer, which will not be described in detail here. The stability, electrochemical performance and mechanical properties of the ion exchange membrane are significantly improved, and it is more suitable for liquid flow battery diaphragms, fuel cell proton exchange membranes and proton exchange membranes for water electrolysis.
[0038] In some embodiments, the ion exchange membrane has a thickness of 3 to 500 μm;
[0039] and / or, the IEC of the ion exchange membrane is 0.2 to 4.10 mmol / g;
[0040] And / or, the ion exchange membrane further comprises a reinforcement membrane, and the sulfonic acid functionalized polymer is supported on the reinforcement membrane.
[0041] The embodiment of the present invention provides a method for preparing an ion exchange membrane, comprising: dispersing the sulfonic acid functionalized polymer in a solvent to obtain a dispersion, forming a membrane from the dispersion, and drying to obtain an ion exchange membrane.
[0042] An embodiment of the present invention provides an application of a sulfonic acid functionalized polymer or an ion exchange membrane for use in at least one of fuel cells, water electrolysis, flow batteries, chlor-alkali industry, lithium batteries, electrodialysis, osmosis, fabric coatings, packaging materials, wearable devices, biomedical devices, medical materials or antibacterial materials.
[0043] In the embodiment of the present invention, all advantages of sulfonic acid functionalized polymer or ion exchange membrane are provided, which will not be described here. In sulfonic acid functionalized polymer or ion exchange membrane, sulfonic acid functional group is connected to polymer main chain by hydrophobic spacer, and stability and mechanical properties are significantly improved, which is more conducive to application in flow battery diaphragm, fuel cell proton exchange membrane and water electrolysis proton exchange membrane, etc., and can also be used for chlor-alkali industrial diaphragm, lithium battery polyelectrolyte, electrodialysis membrane, permeation membrane. The sulfonic acid functional group in sulfonic acid functionalized polymer has broad-spectrum antibacterial property, therefore, sulfonic acid functionalized polymer and composite material comprising the polymer can also be applied to medical fabric coating, packaging material, human wearable device, biomedical equipment, medical material or antibacterial material, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a cross-sectional SEM image of PEM-7.
[0045] Figure 2 This is the polarization curve of a single cell of a PEM-7 fuel cell.
[0046] Figure 3 This is the infrared spectrum of SPS-2.
[0047] Figure 4 This is the infrared spectrum of SPS-5. DETAILED DESCRIPTION
[0048] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0049] A sulfonic acid functionalized polymer according to an embodiment of the present invention comprises a repeating unit A0 represented by formula (1):
[0050]
[0051] wherein R1 is selected from H or F;
[0052] R2 is selected from H, F or CH3;
[0053] a is an integer selected from 0 to 12, specifically, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, preferably an integer selected from 0 to 6, more preferably 0 or 1;
[0054] R3 is selected from alkyl sulfonic acid, fluoroalkyl sulfonic acid or aryl sulfonic acid;
[0055] Optionally, the positions of the two substituents on the benzene ring of the repeating unit A0 are selected from at least one of the ortho position, meta position or para position.
[0056] In the embodiment of the present invention, in the side chain structure of the sulfonic acid functionalized polymer, the sulfonic acid group is grafted onto the benzene ring with an alkoxy or oxy substituent through an alkyl, fluoroalkyl or aryl group. Compared with the sulfonic acid group being directly grafted onto the benzene ring or the sulfonic acid group being directly grafted onto the benzene ring through an alkyl, fluoroalkyl or aryl group, the reaction conditions are more mild and controllable, and sulfonic acid functionalized polymers with different ion exchange capacities can be prepared according to the number of active sites, and polyvalent cationic impurities will not be introduced to poison the ion transmission capacity, and alkylation cross-linking side reactions will not be generated to destroy the linear structure of the polymer, and the product structure is clear and has better dissolution and processing performance. The long side chain structure can promote the formation of an ordered phase separation structure, improve the stability of the main chain structure, significantly improve the oxidation resistance, free radical resistance and hydrolysis resistance of the material, and reduce the water absorption rate of the material, thereby improving the dimensional stability of the polymer material under high humidity conditions and enhancing the mechanical properties and electrochemical properties of the material.
[0057] In some embodiments, R3 is selected from at least one of the following structural formulas:
[0058] Formula (2) Formula (3) Formula (4) Formula (5) Or formula (6)
[0059] Among them, M + Selected from cations, optionally, selected from at least one of hydrogen ions, ammonium ions or monovalent metal cations, preferably selected from at least one of hydrogen ions, lithium ions, sodium ions or potassium ions;
[0060] b is an integer selected from 0 to 6, specifically, for example, 0, 1, 2, 3, 4, 5, 6, preferably an integer selected from 0 to 5, more preferably 0;
[0061] c is an integer selected from 0 to 12, specifically, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, preferably an integer selected from 0 to 6, more preferably 1 or 2;
[0062] R4~R 17 Each independently selected from H, F, C1-C6 alkyl, C1-C6 perfluoroalkyl or C6-C 12 At least one of the aromatic groups of , preferably at least one of H, F, methyl, ethyl, propyl or trifluoromethyl, more preferably H, F or methyl; Optionally, at least one of R4 to R9 is selected from F, C1 to C6 perfluoroalkyl; Optionally, R 10 ~R 17 At least one of them is selected from F and a C1-C6 perfluoroalkyl group.
[0063] In the embodiment of the present invention, the R3 is conducive to further improving the oxidation resistance, free radical resistance and hydrolysis resistance of the material, and improving the dimensional stability, mechanical properties and electrochemical properties of the polymer material. For example, when R3 contains a methyl group, it can improve the stability of the alkyl sulfonic acid side chain, and the methyl group is more resistant to the attack of free radicals after replacing the hydrogen atom, which is conducive to improving the free radical resistance and oxidation resistance of the polymer, and the chemical durability is better; when it contains a partial fluoroalkyl group, the sulfonic acid group and the fluorine atom are introduced into the polymer at the same time, which is conducive to improving the free radical resistance and oxidation resistance of the side chain, and the chemical durability is better. At the same time, the fluorine atom increases the electronegativity of the side chain, thereby enhancing the acidity of the sulfonic acid functional group; when it contains a perfluoroalkyl group, the fluorocarbon structure gives it excellent stability and ion transmission ability, further enhancing the electronegativity and stability of the side chain, and having the best comprehensive performance.
[0064] In some embodiments, the sulfonic acid functionalized polymer further comprises a repeating unit A1 represented by formula (7):
[0065]
[0066] wherein R1 is selected from H or F; R2 is selected from H, F or CH3; R 18 Selected from H, C1~C 12 Alkyl, C1-C6 perfluoroalkyl or C6-C 12At least one of the aryl groups is preferably selected from H, C1-C4 alkyl or phenyl, more preferably selected from H or methyl;
[0067] Optionally, the positions of the two substituents on the benzene ring of the repeating unit A1 are selected from at least one of the ortho position, meta position or para position.
[0068] In some embodiments, the sulfonic acid functionalized polymer further comprises a repeating unit A2, wherein the repeating unit A2 comprises at least one of -C(CH3)2CH-, -CH2CH2-, -CH(CH3)CH2-, or -CH(CH2CH3)CH2-, preferably at least one of -CH2CH2-, -CH(CH3)CH2-, or -CH(CH2CH3)CH2-.
[0069] In some embodiments, the sulfonic acid functionalized polymer further comprises a repeating unit A3 represented by formula (8):
[0070]
[0071] In the formula, R1 is selected from H or F; R2 is selected from H, F or CH3; a is selected from an integer of 0 to 12, specifically, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, preferably an integer of 0 to 6, more preferably 0 or 1;
[0072] R 19 At least one selected from -OH, -F, -Cl, -Br, -I, C1-C4 alkoxy; specifically, the C1-C4 alkoxy includes at least one of methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy or tert-butoxy; preferably at least one selected from -OH, methoxy, tert-butoxy, -Cl or -Br, more preferably -OH;
[0073] Optionally, the positions of the two substituents on the benzene ring of the repeating unit A3 are selected from at least one of the ortho position, meta position or para position.
[0074] In the embodiment of the present invention, the sulfonic acid functionalized polymer is grafted with the sulfonic acid functional group by a nucleophilic substitution reaction between a sulfonating agent and a hydroxyl group. For the application of the sulfonic acid functionalized polymer in the embodiment of the present invention, if A3 is contained, the ideal state is that the R of the repeating unit of A3 is 19 All are -OH.
[0075] In some embodiments, the sulfonic acid functionalized polymer further comprises at least one of a repeating unit A1 of formula (7), a repeating unit A2 or a repeating unit A3 of formula (8).
[0076] In the embodiment of the present invention, the sulfonic acid functionalized polymer may contain only repeating unit A0, or may contain other repeating units. Among them, A2 is preferred, because the A2 repeating unit can form a random / block copolymer structure with the A0 repeating unit, and A2 as a hydrophobic structure can promote the material to form a hydrophilic and hydrophobic phase separation structure, improve the mechanical properties, chemical stability and electrochemical properties of the material. The complete reaction of A3 to A0 can improve the ion exchange capacity of the material, and the chemical structure of the sulfonic acid functionalized polymer is more clear, and the performance consistency of the product is better.
[0077] In some embodiments, the sulfonic acid functionalized polymer is a polymer comprising (q1-q0-q3) repeating units A1, q0 repeating units A0 and q3 repeating units A3; or, the sulfonic acid functionalized polymer is a random copolymer or block copolymer comprising (q1-q0-q3) repeating units A1, q0 repeating units A0, q3 repeating units A3 and q2 repeating units A2;
[0078] Optionally, q0 is an integer from 200 to 8000, preferably, an integer from 400 to 7000, more preferably, an integer from 500 to 6000;
[0079] q1 is an integer of 250 to 8000, preferably an integer of 400 to 6000, more preferably an integer of 500 to 4800;
[0080] q2 is an integer of 250 to 8000, preferably an integer of 400 to 6000, more preferably an integer of 500 to 4800;
[0081] q3 is an integer ≤6000, preferably, an integer ≤1000, further preferably, an integer ≤100, and more preferably, q3 is 0.
[0082] In some embodiments, in the sulfonic acid functionalized polymer, the molar percentage of repeating unit A0 in all repeating units containing benzene rings in the sulfonic acid functionalized polymer is defined as the sulfonation degree of the sulfonic acid functionalized polymer; in a specific embodiment, in the sulfonic acid functionalized polymer, the molar amount of repeating unit A0 is N0, the sum of the molar amounts of repeating unit A0, repeating unit A1 and repeating unit A3 is N1, and the ratio of N0 to N1 is defined as the sulfonation degree of the sulfonic acid functionalized polymer;
[0083] Optionally, the sulfonation degree of the sulfonic acid functionalized polymer is ≥0.1%, specifically, for example, 0.1%, 0.5%, 1%, 2%, 5%, 10%, 20%, 50%, preferably, the sulfonation degree is ≥0.5%, more preferably, the sulfonation degree is ≥2%.
[0084] In the embodiment of the present invention, when the sulfonation degree of the sulfonic acid functionalized polymer is low, the content of ion exchange groups per unit mass in the material is small, the ion exchange effect is weak, and the application is limited. In addition, a low degree of sulfonation may cause the mechanical properties to be similar to those of unsulfonated polymers, resulting in poor mechanical properties, poor hydrophilicity, and too low adsorption, exchange and transmission capabilities of ions. The preparation cost difference between the material with a low degree of sulfonation and the material with a high degree of sulfonation is small, and the performance difference is extremely large. The sulfonic acid group is randomly grafted on the benzene ring of the polymer main chain. The lower the degree of sulfonation, the less clear the chemical structure is. The higher the degree of sulfonation, the clearer the chemical structure of the material is, and the more stable the product performance is.
[0085] In some embodiments, the M of the sulfonic acid functionalized polymer is n The M of the sulfonic acid functionalized polymer is 30,000 to 1,000,000, preferably 40,000 to 800,000, more preferably 50,000 to 600,000. w It is 30,000-1,500,000, preferably, 40,000-1,000,000, more preferably, 50,000-800,000.
[0086] In some embodiments, the sulfonic acid functionalized polymer has an EW of 244 to 5000 g / mol, preferably, 256 to 3000 g / mol, and more preferably, 260 to 2000 g / mol.
[0087] In the embodiments of the present invention, different application scenarios have different requirements for EW values. Materials with medium EW values can be used alone to prepare ion exchange membranes. Sulfonic acid functionalized polymers with low EW values (high IEC) can be compounded with other polymer materials to prepare ion exchange membranes with equivalent or better performance. Ion exchange resins and electrodialysis ion exchange membranes used for water treatment or adsorption usually select materials with medium EW values and high EW values (low IEC). For biological materials, taking wound dressings as an example, sulfonic acid functionalized polymers are required to be in the form of solutions, emulsions or gels, and low EW (high IEC) is required to facilitate dispersion in the disinfectant mixture.
[0088] A method for preparing a sulfonic acid functionalized polymer according to an embodiment of the present invention comprises: subjecting a hydroxyl functionalized styrene polymer to a sulfonation reaction with a hydrogen extraction agent and a sulfonation agent to obtain a sulfonic acid functionalized polymer.
[0089] In the embodiment of the present invention, a sulfonation reaction is carried out by a hydroxyl-functionalized styrene polymer with a hydrogen extraction agent and a sulfonation agent, and a group containing a sulfonic acid functional group is grafted onto a benzene ring having an alkoxy or oxy substituent. The reaction conditions are mild, the reaction degree is high, the reaction product has few side reactions, and there is no residual multivalent cation poisoning the product ion transmission capacity, and there is no alkyl cross-linking side reaction that causes the product to be unable to dissolve and process, and good processing and molding performance is maintained. The sulfonation degree of the product is controllable, and the chemical structure of the product is clear, which is conducive to the preparation of functional material products with stable performance.
[0090] In some embodiments, a hydroxyl-functionalized styrene polymer is dispersed in an organic medium and then subjected to a sulfonation reaction with a hydrogen abstraction agent and a sulfonation agent to obtain a sulfonic acid-functionalized polymer.
[0091] In some embodiments, the hydroxyl-functionalized styrene polymer comprises a repeating unit A3 represented by formula (8); optionally, R 19 Selected from -OH; Optionally, the hydroxyl-functionalized styrene polymer further comprises at least one of the repeating units A1 and A2 shown in formula (7).
[0092] In some embodiments, the structural formula of the hydroxyl-functionalized styrene polymer is selected from at least one of the structural formulas shown in formula (9) or formula (10):
[0093]
[0094]
[0095] In some embodiments, the hydroxyl-functionalized styrene polymer is a polymer comprising (q1-q0-q3) repeating units A1 and q3 repeating units A3; or, the hydroxyl-functionalized styrene polymer is a random copolymer or block copolymer comprising (q1-q0-q3) repeating units A1, q3 repeating units A3 and q2 repeating units A2;
[0096] Optionally, q0 is an integer of 200 to 8000, preferably, an integer of 400 to 7000, more preferably, an integer of 500 to 6000;
[0097] q1 is an integer of 250 to 8000, preferably an integer of 400 to 6000, more preferably an integer of 500 to 4800;
[0098] q2 is an integer of 250 to 8000, preferably an integer of 400 to 6000, more preferably an integer of 500 to 4800;
[0099] q3 is an integer ≤6000, preferably, an integer ≤1000, further preferably, an integer ≤100, and more preferably, q3 is 0.
[0100] In the embodiment of the present invention, the hydroxyl-functionalized styrene polymer is grafted with the sulfonic acid functional group by a nucleophilic substitution reaction between a sulfonating agent and a hydroxyl group. The halogen group in the repeating unit A3 can be converted into a hydroxyl group through an esterification reaction and a hydrolysis reaction. However, the unreacted halogen group and the hydroxyl group will undergo a nucleophilic substitution reaction to form an ether bond, and a cross-linking side reaction will occur. However, the temperature of the nucleophilic substitution reaction of the halogen group and the hydroxyl group is higher than that of the sulfonation reaction. Therefore, when the temperature of the sulfonation reaction is low, the degree of the cross-linking side reaction of the halogen group and the hydroxyl group is low or does not react. The ideal state of the hydroxyl-functionalized styrene polymer is that the R of the A3 repeating unit 19 All are -OH.
[0101] In some embodiments, in the hydroxyl-functionalized styrene polymer, the molar amount of the repeating unit A3 is N3, the molar amount of the repeating unit A3 containing a hydroxyl group is N4, and the ratio of N4 to N3 is defined as the degree of functionalization of the hydroxyl-functionalized styrene polymer;
[0102] Optionally, the degree of functionalization of the hydroxyl-functionalized styrene polymer is ≥10%, specifically, for example, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 99%, 100%, preferably, ≥50%, further preferably, ≥90%, more preferably, ≥99%.
[0103] In the embodiments of the present invention, it is beneficial to improve the ion exchange capacity of the prepared sulfonic acid functionalized polymer, improve the stability of the material, and reduce or avoid cross-linking side reactions. When the functionalization degree of the hydroxyl-functionalized styrene polymer is low, there are fewer sites available for grafting sulfonic acid functional groups, and the ion exchange capacity of the subsequently prepared sulfonic acid functionalized polymer is weak, and the repeating unit A3 containing a halogen group will undergo a cross-linking side reaction with the repeating unit A3 containing a hydroxyl group.
[0104] In some embodiments, the hydroxyl-functionalized styrene polymer is obtained by polymerization of monomers, or by subjecting a styrene polymer to a hydroxyl-functionalization reaction; optionally, the preparation method of the hydroxylated styrene polymer comprises subjecting an alkoxy styrene polymer or a halomethylated styrene polymer to a substitution reaction, and optionally, the alkoxy styrene polymer is subjected to a substitution reaction by acidification treatment to obtain a phenolic hydroxylated styrene polymer.
[0105] In some embodiments, the styrene polymer is a polymer comprising q1 repeating units A1, or the styrene polymer is a random copolymer comprising q1 repeating units A1 and q2 repeating units A2, or the styrene polymer is a block copolymer comprising q1 repeating units A1 and q2 repeating units A2;
[0106] Optionally, q1 is an integer of 250 to 8000, preferably, an integer of 400 to 6000, more preferably, an integer of 500 to 4800; q2 is an integer of 250 to 8000, preferably, an integer of 400 to 6000, more preferably, an integer of 500 to 4800.
[0107] In some embodiments, the styrenic polymer includes at least one of polystyrene, poly(3-methylstyrene), poly(4-methylstyrene), poly(α-methylstyrene), poly(styrene-ran-α-methylstyrene), polytrifluorostyrene, poly(styrene-ran-ethylene), poly(styrene-ran-butylene), poly(styrene-b-ethylene), poly(styrene-b-(ethylene-ran-butylene)-b-styrene) (SEBS), poly(styrene-b-(ethylene-ran-propylene)-b-styrene) (SEPS), poly(styrene-b-(ethylene-ethylene-propylene)-b-styrene) (SEEPS);
[0108] Preferably, it comprises at least one of polystyrene, poly(3-methylstyrene), poly(4-methylstyrene), poly(α-methylstyrene), poly(styrene-ran-α-methylstyrene), polytrifluorostyrene, SEBS, SEPS, and SEEPS;
[0109] More preferably, it includes at least one of polystyrene, poly(4-methylstyrene), poly(α-methylstyrene), polytrifluorostyrene, and SEBS.
[0110] In some embodiments, the hydrogen extraction agent includes at least one of an alkali metal oxide, an alkali metal hydride, an alkali metal peroxide, an alkali metal hydroxide, an alkali metal carbonate, or an alkali metal organic compound;
[0111] Optionally, the alkali metal includes at least one of lithium, sodium and potassium;
[0112] Optionally, the hydrogen removal reagent includes at least one of lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium hydride, potassium hydride, sodium oxide, sodium peroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium tert-butoxide, sodium tert-butoxide or potassium tert-butoxide; preferably, it includes at least one of sodium hydroxide, potassium hydroxide, lithium hydride, sodium hydride, sodium carbonate, potassium carbonate, lithium tert-butoxide, sodium tert-butoxide or potassium tert-butoxide; more preferably, it includes at least one of sodium hydroxide, potassium hydroxide, lithium hydride, sodium hydride, lithium tert-butoxide, potassium tert-butoxide or potassium carbonate.
[0113] In the embodiment of the present invention, the hydrogen extraction agent can replace the H of the hydroxyl group on the polymer molecule with the alkali metal ion and maintain an alkaline environment, which is conducive to the generation of oxygen anions on the polymer and then combines with the carbon cation of the sulfonation agent to undergo a nucleophilic substitution reaction.
[0114] In some embodiments, the sulfonated reagent comprises at least one of the following structural formulas:
[0115] Formula (11) Formula (12) Formula (13) Formula (14) Or formula (15)
[0116] Among them, R4~R 17 Each independently selected from H, F, C1-C6 alkyl, C1-C6 perfluoroalkyl or C6-C 12 At least one of the aromatic groups of , preferably at least one of H, F, methyl, ethyl, propyl or trifluoromethyl, more preferably H, F, methyl; Optionally, at least one of R4 to R9 is selected from F, C1 to C6 perfluoroalkyl; Optionally, R 10 ~R 17 At least one of them is selected from F, C1-C6 perfluoroalkyl;
[0117] b is an integer selected from 0 to 6, specifically, for example, 0, 1, 2, 3, 4, 5, 6, preferably an integer selected from 0 to 5, more preferably 0;
[0118] c is an integer selected from 0 to 12, specifically, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, preferably an integer selected from 0 to 6, more preferably 1 or 2;
[0119] M + Selected from cations, optionally, selected from at least one of hydrogen ions, ammonium ions or monovalent metal cations, preferably selected from at least one of hydrogen ions, lithium ions, sodium ions or potassium ions;
[0120] X is selected from at least one of F, Cl, Br or I, preferably at least one of Cl or Br, more preferably Br.
[0121] R3 in the sulfonic acid functionalized polymer depends on the sulfonating reagent selected, and the corresponding relationship is shown in Table 1.
[0122] Table 1
[0123] Sulfonation reagent <![CDATA[R3 in the sulfonic acid functionalized polymer]]> Formula (11) Formula (2) Formula (12) Formula (3) Formula (13) Formula (4) Formula (14) Formula (5) Formula (15) Formula (6)
[0124] In some embodiments, the sulfonating agent includes at least one of the following compounds: 1,3-propane sultone, 1,4-butane sultone, 1-methyl-1,3-propane sultone, 2-methyl-1,3-propane sultone, 3-methyl-1,3-propane sultone, 1-methyl-1,4-butane sultone, 2-methyl-1,4-butane sultone, 3-methyl-1,4-butane sultone, 4-methyl-1,4-butane sultone, 1-fluoro-1,3-propane sultone, 2-fluoro-1,3-propane sultone, 3-fluoro-1,3-propane sultone, 1-fluoro-1,4-butane sultone, 2-fluoro-1,4-but ... -fluoro-1,4-butane sultone, 4-fluoro-1,4-butane sultone, 1-(trifluoromethyl)-2,3-di(ethyl)-propane sultone, 1-(trifluoromethyl)-2,3-di(methyl)-propane sultone, 2-(trifluoromethyl)-1,3-di(methyl)-propane sultone, 2-(trifluoromethyl)-1,3-di(ethyl)-propane sultone, 1-(trifluoromethyl)-2,3,4-tri(methyl)-butane sultone, 2-(trifluoromethyl)-1,3,4-tri(ethyl)-butane sultone, 3-(trifluoromethyl)-1,2,4-tri(ethyl)-butane sultone, 2-(trifluoromethyl)-1,3,4-tri(methyl)-butane sultone, 3 ,3,4,4-tetrafluoro-1,2-oxathietane 2,2-dioxide (also known as tetrafluorosulfone, CAS: 697-18-7), 1,2,2-trifluoro-2-hydroxy-1-trifluoromethylethanesulfonic acid (CAS: 773-15-9), 3,4,4-trifluoro-3-(pentafluoroethyl)-1,2-oxathiophene 2,2-dioxo (CAS: 108858-07-7), 3,4,4-trifluoro-3-(perfluoropropyl)-1,2-oxathiophene 2,2-dioxo (CAS: 156465-44-0), 3,4,4-trifluoro-3-(perfluorobutyl)-1,2-oxathiophene 2,2-dioxo (CAS: 85211-95 -6), 3,4,4-trifluoro-3-(perfluoropentyl)-1,2-oxathiophene 2,2-dioxo (CAS: 1894-92-4), 3,4,4-trifluoro-3-(perfluorohexyl)-1,2-oxathiophene 2,2-dioxo (CAS: 1131541-76-8), p-bromomethylbenzenesulfonic acid, alkali metal salts of p-bromomethylbenzenesulfonic acid, 4-(2-bromoethyl)benzenesulfonic acid, alkali metal salts of 4-(2-bromoethyl)benzenesulfonic acid, 4-bromobenzenesulfonic acid, alkali metal salts of 4-bromobenzenesulfonic acid, 4-chlorobenzenesulfonic acid, alkali metal salts of 4-chlorobenzenesulfonic acid, p-chloromethylbenzenesulfonic acid, alkali metal salts of p-chloromethylbenzenesulfonic acid; optionally, the alkali metal comprises at least one of lithium, sodium and potassium;
[0125] Preferably, at least one of the following compounds is included: 1,3-propane sultone, 1,4-butane sultone, 1-methyl-1,3-propane sultone, 2-methyl-1,3-propane sultone, 3-methyl-1,3-propane sultone, 1-fluoro-1,3-propane sultone, 2-fluoro-1,3-propane sultone, 3-fluoro-1,3-propane sultone, tetrafluorosultone, 1,2,2-trifluoro-2-hydroxy-1-trifluoromethylethane sulfonic acid, 3,4,4-trifluoro-3-(perfluorobutyl)-1,2-oxathiophene 2,2-dioxo, p-bromomethylbenzenesulfonic acid, an alkali metal salt of p-bromomethylbenzenesulfonic acid, 4-(2-bromoethyl)benzenesulfonic acid, an alkali metal salt of 4-(2-bromoethyl)benzenesulfonic acid;
[0126] More preferably, at least one of the following compounds is included: 1,3-propane sultone, 1,4-butane sultone, 1-methyl-1,3-propane sultone, 3-fluoro-1,3-propane sultone, 4-(2-bromoethyl)benzenesulfonic acid, an alkali metal salt of 4-(2-bromoethyl)benzenesulfonic acid, tetrafluorosultone or 1,2,2-trifluoro-2-hydroxy-1-trifluoromethylethanesulfonic acid.
[0127] In the embodiment of the present invention, the hydroxyl group of the hydroxyl-functionalized styrene polymer as a highly active reaction site can make the grafting degree of the sulfonic acid functional group controllable. All hydroxyl groups can be reacted and grafted with sulfonic acid groups under appropriate reaction conditions, and some unreacted hydroxyl groups can be retained according to application needs. The retained hydroxyl groups, especially the phenolic hydroxyl groups directly grafted on the benzene ring, have good antioxidant properties and can improve the chemical stability of the material. Styrene polymers with clear structures can be prepared by the method of active polymerization, and further grafting modification can graft sulfonic acid side chains on all benzene rings. Since the structure of the polymer before modification is clear, the structure of the obtained sulfonic acid functionalized polymer is also clear, which can ensure the consistency of product performance and batch stability. The reaction conditions of sultone, fluorosultone, perfluoroalkyl oxygen sulfur heterocyclic compound, halogenated aryl sulfonic acid compound and hydroxyl functionalized styrene polymer are mild and controllable, the reaction process is not easy to produce cross-linking side reactions, and the ion exchange performance of the material will not be introduced into the multivalent metal cation poisoning material, so that the sulfonic acid functionalized polymer can meet the use requirements of battery separators, electrodialysis separators, water electrolysis separators, etc. Alkoxy, fluoroalkoxy, phenoxy, and phenylalkoxy as spacers between the sulfonic acid group and the main chain can improve the chemical stability and mechanical properties of the material, and can effectively control the water absorption and swelling of the low EW material, preventing excessive swelling from causing a sharp drop in dimensional stability, electrochemical properties, and mechanical strength. The fluorine substituents of the fluorinated side chains can increase the acidity of the sulfonic acid group and improve the chemical stability of the side chains. Sulfonic acid functionalized polymers with perfluoroalkoxy side chains show the best comprehensive performance.
[0128] In some embodiments, the organic medium includes at least one of a halogenated hydrocarbon, an aromatic hydrocarbon, an alkane, tetrahydrofuran, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), or dimethyl sulfoxide (DMSO);
[0129] Optionally, the organic medium includes at least one of dichloromethane, chloroform, 1,2-dichloroethane, cyclohexane, toluene, xylene, o-dichlorobenzene, DMF, DMAC, DMSO or tetrahydrofuran, preferably, includes at least one of chloroform, 1,2-dichloroethane, cyclohexane, toluene, o-dichlorobenzene, DMF, DMAC or DMSO.
[0130] In some embodiments, the molar ratio of the hydroxyl functional group in the hydroxyl functionalized styrene polymer to the sulfonating agent is 1:(0.1-30), specifically, for example, 1:0.1, 1:1, 1:2, 1:5, 1:10, 1:20 or 1:30, preferably, 1:(1-20), more preferably, 1:(2-10). In the embodiments of the present invention, the molar ratio of the hydroxyl functionalized styrene polymer to the sulfonating agent is within the above range, so that part or all of the hydroxyl functional groups in the hydroxyl functionalized styrene polymer can be grafted with sulfonic acid functional groups. If the relative amount ratio of the hydroxyl functional groups in the hydroxyl functionalized styrene polymer is too high, the grafted sulfonic acid ion groups are too few, and the ion exchange capacity of the material is poor; if the relative amount ratio of the hydroxyl functional groups is too low, it is easy to cause waste of the sulfonating agent, increase production costs and difficulty of post-processing.
[0131] In some embodiments, the molar ratio of the hydroxyl functional group and the hydrogenation agent in the hydroxyl functionalized styrene polymer is 1:0.1 to 20, specifically, for example, 1:0.1, 1:0.5, 1:1, 1:2, 1:5, 1:10, 1:15, 1:20, preferably, 1:0.5 to 5. In an embodiment of the present invention, the molar ratio of the hydroxyl functional group and the hydrogenation agent is 1:0.1 to 20. Too little hydrogenation agent will cause the hydrogen of the hydroxyl group in the polymer to be unable to be fully replaced by the alkali metal ion, and even if an excess of sulfonation agent is added, the degree of sulfonation of the product cannot be increased. On the other hand, the hydrogenation agent itself is not conducive to the dispersion of the polymer, especially the alkali metal organic compound with good solubility. Adding too much hydrogenation agent will not increase the reaction rate and reaction degree, but will cause the polymer to precipitate and agglomerate, and it will not be able to disperse the reaction evenly in the solvent.
[0132] In some embodiments, the temperature of the sulfonation reaction is 20-160° C., specifically, for example, 20° C., 30° C., 40° C., 60° C., 80° C., 100° C., 120° C., 140° C. or 160° C., preferably, 40-120° C. In the embodiment of the present invention, the temperature of the nucleophilic substitution reaction of the halogen group and the hydroxyl group is higher than that of the sulfonation reaction. In the present invention, the temperature of the sulfonation reaction is relatively low, and at this time, the cross-linking side reaction degree of the halogen group and the hydroxyl group is relatively low or does not react.
[0133] In some embodiments, the sulfonation reaction time is 0.5-72 h, specifically, for example, 0.5 h, 1 h, 10 h, 12 h, 20 h, 24 h, 30 h, 40 h, 50 h, 60 h, 70 h or 72 h, preferably, 1-24 h.
[0134] In some embodiments, the mass of the hydroxyl-functionalized styrene polymer, the sulfonated reagent and the hydrogenation reagent is 0.1% to 30% of the mass of the organic medium, preferably 0.5% to 25%, and more preferably 1% to 20%. In the embodiments of the present invention, the organic medium can effectively disperse the hydroxyl-functionalized styrene polymer, the sulfonated reagent and the hydrogenation reagent, which is more conducive to the reaction.
[0135] In some embodiments, the hydroxyl-functionalized styrene polymer is first dispersed in an organic medium to obtain a hydroxyl-functionalized styrene polymer dispersion, and then a hydrogenation reagent and a sulfonation reagent are added to carry out a sulfonation reaction; optionally, the concentration of the hydroxyl-functionalized styrene polymer dispersion is 1 mg / mL to 300 mg / mL, preferably 5 mg / mL to 250 mg / mL, and more preferably 5 mg / mL to 200 mg / mL.
[0136] In some embodiments, the hydroxyl-functionalized styrene polymer is first subjected to a hydrogenation reaction with a hydrogenation reagent, and then subjected to a sulfonation reaction with a sulfonating reagent; optionally, the temperature of the hydrogenation reaction is 0 to 60°C; and the time of the hydrogenation reaction is 1 min to 120 min. In the embodiment of the present invention, the hydrogenation reaction is first performed, and then the sulfonation reaction is performed, so that the hydroxyl groups of the polymer are replaced with alkali metal ions to form oxygen anions with good reaction activity, which is conducive to the nucleophilic substitution reaction with the carbon cation of the sulfonating reagent. Some sulfonating reagents are highly acidic, which is not conducive to the replacement of hydrogen of the hydroxyl groups by alkali metal ions.
[0137] In some embodiments, after the sulfonation reaction is completed, the reaction mixture is cooled to room temperature, and crushed ice, an ice-water mixture, or water is added to inactivate the hydrogenation reagent or the sulfonation reagent; optionally, the reaction mixture is then added to a poor solvent for precipitation, washed, and dried to obtain a sulfonic acid functionalized polymer solid product; optionally, the poor solvent includes at least one of water, hydrochloric acid, acetone, butanone, fatty alcohols, and esters.
[0138] In some embodiments, after the sulfonation reaction is completed, it is added to a poor solvent for precipitation, washed, and dried to obtain a sulfonic acid functionalized polymer solid product; optionally, the poor solvent includes at least one of water, hydrochloric acid, acetone, butanone, fatty alcohol, and esters.
[0139] In some embodiments, the product after the sulfonation reaction is completed and the sulfonation reagent is inactivated or the product obtained by precipitation by adding it to a poor solvent or the sulfonic acid functionalized polymer solid product is subjected to ion replacement to obtain sulfonic acid functionalized polymers with different cations;
[0140] Optionally, the ion replacement includes adding the product to an acid solution, a base solution or an alkali metal salt solution to carry out ion replacement to obtain a sulfonic acid functionalized polymer combined with different cations;
[0141] Optionally, the temperature of the ion replacement is room temperature to 100° C., preferably, room temperature to 95° C., more preferably, room temperature to 90° C.; the time of the ion replacement is 0.5 h to 72 h, preferably, 1 h to 48 h;
[0142] Optionally, the acid solution includes at least one of hydrochloric acid, nitric acid, sulfuric acid or phosphoric acid; the concentration of the acid solution is 0.1mol / L~4mol / L, preferably, 0.5mol / L~2mol / L; the alkali includes at least one of lithium hydroxide, sodium hydroxide or potassium hydroxide; the concentration of the alkali solution is 0.1mol / L~8mol / L, preferably, 0.5mol / L~2mol / L; the alkali metal salt is selected from at least one of alkali metal chloride, alkali metal bromide, alkali metal nitrate, alkali metal phosphate or alkali metal sulfate; the alkali metal is selected from at least one of Li, Na or K; the concentration of the alkali metal salt solution is 0.5mol / L~saturation concentration, preferably, 1mol / L~saturation concentration.
[0143] In the embodiment of the present invention, the ion replacement process of the alkali metal salt solution or the alkaline solution is that the metal cation replaces the cation bound to the sulfonic acid functional group on the sulfonic acid functionalized polymer; the ion replacement process in the acid solution is that the hydrogen ion of the acid replaces the cation bound to the sulfonic acid functional group on the sulfonic acid functionalized polymer. Through ion replacement, an ion exchange resin or ion exchange membrane that combines different cations can be obtained to meet the requirements for cations of the material in different application scenarios.
[0144] In order to facilitate the description of the reaction route of the sulfonic acid functionalized polymer, the compound structures of formulas (11) to (14) are simplified as follows:
[0145]
[0146] Simplify the structural formula of the hydrogen extraction reagent to M'R21 , M' is an alkali metal, R 21 is a structure other than an alkali metal in the hydrogen extraction reagent; optionally, the alkali metal is selected from at least one of Li, Na or K; M' and M + The M in are the same or different;
[0147] When the compound of formula (15) is used as a sulfonating agent in a sulfonation reaction, if M + If it is a hydrogen ion, it will react with the hydrogen-extraction reagent to produce an acid-base reaction. The cation combined with the sulfonate group is an alkali metal ion, so M' is used. + Describe the cation of the compound of formula (15) during the sulfonation reaction; M' and M + The M in are the same or different;
[0148] The reaction scheme for the synthesis of sulfonic acid functionalized polymers is as follows:
[0149]
[0150] An ion exchange membrane according to an embodiment of the present invention comprises the sulfonic acid functionalized polymer according to an embodiment of the present invention or the sulfonic acid functionalized polymer prepared by the preparation method according to an embodiment of the present invention.
[0151] In the embodiment of the present invention, the ion exchange membrane has all the advantages of the sulfonic acid functionalized polymer, which will not be described in detail here. The stability, electrochemical performance and mechanical properties of the ion exchange membrane are significantly improved, and it is more suitable for liquid flow battery diaphragms, fuel cell proton exchange membranes and proton exchange membranes for water electrolysis.
[0152] In some embodiments, the ion exchange membrane also includes a reinforced membrane; the sulfonic acid functionalized polymer is loaded on the reinforced membrane, optionally, the sulfonic acid functionalized polymer is loaded on one side or both sides of the reinforced membrane along its thickness direction; optionally, in the ion exchange membrane, the mass content of the reinforced membrane is 0.1% to 90%, preferably 1% to 70%, more preferably 3% to 50%; the thickness of the reinforced membrane is 2 to 400 μm, preferably 2 to 300 μm, more preferably 2 to 180 μm; the reinforced membrane includes at least one of a polytetrafluoroethylene membrane, an ethylene-tetrafluoroethylene copolymer membrane, a polyvinylidene fluoride membrane or an aromatic polymer membrane; optionally, the aromatic polymer membrane includes at least one of a polyarylether polymer membrane and a polyimide membrane; the polyarylether polymer membrane includes at least one of a polyphenylene ether membrane, a polyarylether sulfone membrane, a polysulfone membrane, a polyethersulfone membrane, a polyaryletherketone membrane and an aromaticletherketone derivative membrane.
[0153] In some embodiments, the ion exchange membrane has a thickness of 3 to 500 μm, preferably 4 to 320 μm, and more preferably 5 to 200 μm.
[0154] In some embodiments, the IEC of the ion exchange membrane is 0.2 to 4.10 mmol / g, preferably, 0.33 to 3.90 mmol / g, and more preferably, 0.5 to 3.85 mmol / g.
[0155] The present invention provides a method for preparing an ion exchange membrane, comprising: dispersing the sulfonic acid functionalized polymer in a solvent to obtain a dispersion, forming a film from the dispersion, and drying to obtain an ion exchange membrane. The present invention has all the advantages of the sulfonic acid functionalized polymer, which will not be described in detail.
[0156] In some embodiments, the film forming method includes at least one of casting, pouring or coating; optionally, the coating includes at least one of slit coating or blade coating.
[0157] In some embodiments, the drying temperature is 20°C to 180°C, preferably 50°C to 180°C; and / or the drying time is 0.1h to 72h; and / or the ion exchange membrane also includes a reinforced membrane, and the film forming includes coating the dispersion on one side or both sides of the reinforced membrane for film forming; optionally, the coating includes at least one of slit coating or blade coating.
[0158] In some embodiments, the solvent comprises at least one of water, methanol, ethanol, isopropanol, n-propanol, toluene, xylene, tetrahydrofuran, cyclohexane, chloroform, n-hexanol, DMF, DMAC or DMSO.
[0159] In some embodiments, the mass concentration of the sulfonic acid functionalized polymer in the dispersion is 1% to 50%, preferably, 2% to 40%, and more preferably, 3% to 30%.
[0160] An application of a sulfonic acid functionalized polymer or ion exchange membrane according to an embodiment of the present invention is used in at least one of fuel cells, water electrolysis, flow batteries, chlor-alkali industry, lithium batteries, electrodialysis, osmosis, fabric coatings, packaging materials, wearable devices, biomedical devices, medical materials or antibacterial materials.
[0161] In the embodiment of the present invention, all advantages of sulfonic acid functionalized polymer or ion exchange membrane are provided, which will not be described here. In sulfonic acid functionalized polymer or ion exchange membrane, sulfonic acid functional group is connected to polymer main chain by hydrophobic spacer, and stability and mechanical properties are significantly improved, which is more conducive to application in flow battery diaphragm, fuel cell proton exchange membrane and water electrolysis proton exchange membrane, etc., and can also be used for chlor-alkali industrial diaphragm, lithium battery polyelectrolyte, electrodialysis membrane, permeation membrane. The sulfonic acid functional group in sulfonic acid functionalized polymer has broad-spectrum antibacterial property, therefore, sulfonic acid functionalized polymer and composite material comprising the polymer can also be applied to medical fabric coating, packaging material, human wearable device, biomedical equipment, medical material or antibacterial material, etc.
[0162] In some embodiments, it is used for at least one of fuel cell proton exchange membranes, water electrolyte proton exchange membranes, flow battery membranes, chlor-alkali industrial membranes, lithium battery polyelectrolytes, electrodialysis membranes, and osmotic membranes.
[0163] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0164] The test methods for conductivity, EW, IEC, tensile strength, tensile strain at break and water absorption refer to GB / T20042.3-2022 "Proton exchange membrane fuel cell part 3: proton exchange membrane test method". Among them, the test conditions for conductivity are 80℃ and relative humidity 80%.
[0165] Fuel cell polarization curve: The test method refers to GB / T20042.5-2022 "Proton Exchange Membrane Fuel Cell Part 5: Membrane Electrode Test Method", and the test conditions are 80°C and relative humidity 80%.
[0166] Free radical resistance: Soak the polymer material or ion exchange membrane in Fenton's reagent at 80°C for 8 hours, and compare the mass changes before and after soaking. The composition of Fenton's reagent: 50mL of 3% H2O2 solution, to which 0.1mL 0.01mol / L Fe 2+ The solution is the Fenton reagent. The Fenton reagent is prepared and used immediately. The greater the ratio of the remaining mass to the initial mass before immersion, the better the free radical resistance, which is expressed as the percentage of the remaining mass to the initial mass.
[0167] Liquid flow battery performance: The test method refers to NB / T42081-2016 "All-vanadium liquid flow battery single cell performance test method".
[0168] The organic medium, film-forming solvent, halomethylation agent, hydroxyl functionalization agent and hydrogenation catalyst used in the examples are all common chemical reagents; tetrafluoroethane-β-sultone, alkyl sultones and partially fluorinated alkyl sultones are from Aladdin, McLean or other chemical websites; other perfluoroalkyl oxygen-sulfur heterocyclic compounds are customized products; poly(4-methylstyrene) and poly(α-methylstyrene) are from McLean or Aladdin; polytrifluorostyrene is from San Ai Fu; SEBS is from Kraton and Asahi Chemical; poly(4-methoxystyrene) is from ACROS; styrene-b-(4-tert-butoxystyrene) diblock copolymer is from Polymer Source; polytetrafluoroethylene microporous membrane (ePTFE membrane) and ethylene-tetrafluoroethylene copolymer microporous membrane are made by conventional biaxial stretching method.
[0169] Example 1: Preparation of phenol hydroxylated styrene polymer
[0170] Weigh 2 g of poly (4-methoxystyrene) and dissolve it in 80 mL of DMAC, add 8 mL of concentrated hydrochloric acid (about 12 mol / L), heat and reflux for 12 h to acidify the methoxy group to phenolic hydroxyl group, use methanol to precipitate, wash and dry to obtain poly (p-hydroxystyrene) (PSOH-1).
[0171] Example 2: Preparation of phenol hydroxylated styrene polymer
[0172] Different from Example 1, the raw material for the reaction is styrene-b-(4-tert-butoxystyrene) diblock copolymer, and styrene-b-(4-hydroxystyrene) diblock copolymer (PSOH-2) is obtained. The chemical structure of PSOH-2 is as follows:
[0173]
[0174] Example 3: Preparation of Chloromethylated Styrene Polymers
[0175] A certain amount of styrene polymer (containing about 50 mmol of repeating unit A1) was weighed and dispersed in chloroform, and 200 mmol of 1,4-dichloromethoxybutane was used as a chloromethylation reagent and 100 mmol of anhydrous tin tetrachloride was used as a catalyst to prepare a chloromethylated styrene polymer. The molar ratio of chloromethyl to benzene ring is defined as the chloromethylation degree, and the chloromethylation degree of all chloromethylated styrene polymers is 100%. The numbers of the chloromethylated styrene polymers and the styrene polymers are shown in Table 2.
[0176] Table 2
[0177] Chloromethylated styrene polymers Styrene polymers X-PS-3 <![CDATA[Poly(α-methylstyrene) (M w ~300000)]]> X-PS-4 Polytrifluorostyrene X-PS-5 SEBS (Asahi Kasei H1043, styrene content 67%) X-PS-6 SEBS (Kraton G1652H, styrene content 30%) X-PS-7 SEBS (Kraton G1536H, styrene content 42%)
[0178] Example 4: Preparation of bromomethylated styrene polymer
[0179] Weigh 7.08 g of poly (4-methylstyrene) (Sigma-Aldrich, M w ~72000), dispersed in dichloromethane, using 60mmol of N-bromosuccinimide as bromination agent, to obtain bromomethylated styrene polymer X-PS-8. The molar ratio of bromomethyl to benzene ring is defined as bromomethylation degree, and the bromomethylation degree of X-PS-8 is 11.0%.
[0180] Example 5: Preparation of hydroxymethylated styrene polymers
[0181] Weigh 2 g of the halomethylated styrene polymer or PVBC in Example 3 and Example 4, dissolve and disperse in 80 mL of toluene, add 5 g of sodium acetate and 10 mL of an aqueous solution of 0.5 g of tetrabutylammonium bromide, stir and react at 100° C. for 96 h, and pour into methanol to precipitate to obtain an esterified polymer solid. Dissolve 1.5 g of the esterified polymer solid in 100 mL of toluene, add 4 g of KOH and 5 mL of an aqueous solution of 0.8 g of tetrabutylammonium bromide, stir and react at 40° C. for 96 h, precipitate the product in methanol, and vacuum dry to obtain a hydroxymethylated styrene polymer.
[0182] The halomethylated styrene polymer raw materials and the corresponding hydroxymethylated styrene polymer products are shown in Table 3. In Table 3, PVBC is poly (vinyl benzyl chloride) (from Sigma-Aldrich, referred to as "PVBC", M n ~55000,M w ~100000, a 60 / 40 mixture of 3-isomer and 4-isomer). The halomethyl groups of the halomethylated styrene polymer can be completely converted into hydroxymethyl groups, and the hydroxymethyl groups in the hydroxymethylated styrene polymer can further react with a sulfonating agent to obtain a sulfonic acid functionalized polymer.
[0183] Table 3
[0184] Halomethylated styrene polymers Hydroxymethylated styrene polymers X-PS-3 PSOH-3 X-PS-4 PSOH-4 X-PS-5 PSOH-5 X-PS-6 PSOH-6 X-PS-7 PSOH-7 X-PS-8 PSOH-8 PVBC PSOH-9
[0185] Example 6: Preparation of sulfonic acid functionalized polymer
[0186] 1.20 g of PSOH-1 in Example 1 was weighed and dissolved in 15 mL of anhydrous toluene, and then 0.36 g of sodium hydride was added, and the mixture was stirred at 40 ° C for 0.5 h for hydrogen extraction reaction. Then 1 g of 1-methyl-1,3-propane sultone was added as a sulfonation reagent for sulfonation reaction, and the sulfonation reaction temperature was 100 ° C and the reaction time was 6 h. After the reaction was completed, 3 mL of water was added to terminate the reaction, and the reaction system was poured into 100 mL of acetone to precipitate the precipitated polymer solid product, and the solid product was washed with acetone and vacuum dried at 45 ° C for 48 h to obtain the sulfonic acid functionalized polymer SPS-1.
[0187] The EW of SPS-1 is 452.1 g / mol, and the structural formula is:
[0188]
[0189] Example 7: Preparation of sulfonic acid functionalized polymer
[0190] Different from Example 6, the phenol hydroxylated styrene polymer is the block copolymer PSOH-2 in Example 2, and the sulfonating agent is 2.3 g of 1,2,2-trifluoro-2-hydroxy-1-trifluoromethylethane sulfonic acid to obtain the sulfonic acid functionalized polymer SPS-2. The EW of SPS-2 is 631.6 g / mol, and the structural formula is:
[0191]
[0192] Figure 3 This is the infrared spectrum of the sulfonic acid functionalized polymer SPS-2. -1 The broad and smooth vibration peak near the hydroxyl group is the stretching vibration of the sulfonic acid group. This characteristic peak comes from the bound water of the sulfonic acid group; 1100-1200cm -1 The characteristic peak at 1000 cm is attributed to the stretching vibration of O=S=O in the sulfonic acid group; -1 The characteristic peaks at around 671cm are attributed to the stretching vibration of CF in the polymer side chain -CF3; -1 and 577cm -1 The characteristic peaks of 3000cm-1 are attributed to the swing vibration and stretching vibration of FCF. The molecule of SPS-2 contains a benzene ring. -1 The characteristic peaks nearby are the CH stretching vibrations on the benzene ring.
[0193] Example 8: Preparation of sulfonic acid functionalized polymer
[0194] Weigh 1.49g of PSOH-3 in Example 5, dissolve and disperse in 30mL of anhydrous DMAC to obtain a hydroxymethylated styrene polymer solution. Add 0.24g of lithium hydride to the polymer solution and stir at 50°C for 0.5h to perform a hydrogen extraction reaction. Add 4.2g of 3-fluoro-1,3-propane sultone as a functionalizing agent for a functionalization reaction, the functionalization reaction temperature is 90°C, and the reaction time is 8h. After the reaction is completed, add 5mL of water to terminate the reaction, pour the reaction system into 120mL of acetone to precipitate the precipitated polymer solid product, wash the solid product with tetrahydrofuran and acetone, and vacuum dry at 45°C for 48h to obtain a sulfonic acid functionalized polymer SPS-3.
[0195] The EW of SPS-3 is 304.4 g / mol, and the structural formula is:
[0196]
[0197] Example 9: Preparation of sulfonic acid functionalized polymer
[0198] Weigh 1.89g of PSOH-4 in Example 5, dissolve and disperse in 30mL DMSO to obtain a polymer solution. Add 2.24g of potassium carbonate to the polymer solution and stir at 50°C for 0.5h to carry out hydrogen extraction reaction. Add 5.74g of sodium 4-(2-bromoethyl)benzenesulfonate as a sulfonating agent to carry out sulfonation reaction, the sulfonation reaction temperature is 130°C, and the reaction time is 12h. After the reaction is completed, pour the reaction system into 150mL of ethyl acetate to precipitate the precipitated polymer solid product, wash the solid product with acetone, and vacuum dry at 45°C for 48h to obtain sulfonic acid sulfonated polymer SPS-4.
[0199] The EW of SPS-4 is 731.1 g / mol, and the structural formula is:
[0200]
[0201] Sodium 4-(2-bromoethyl)benzenesulfonate is used as the sulfonation reagent. The side chain of the polymer grafting has a large steric hindrance, and only part of the hydroxyl groups participate in the reaction to graft the sulfonic acid functional groups.
[0202] Example 10: Preparation of sulfonic acid functionalized polymer
[0203] Weigh 1.3g of PSOH-8 in Example 5, dissolve and disperse in 30mL DMF to obtain a polymer solution. Add 1.56g of potassium tert-butoxide to the polymer solution and stir at 40°C for 0.5h to carry out hydrogen extraction reaction. Then add 0.61g of 1,3-propane sultone as a sulfonating agent for sulfonation reaction. The sulfonation reaction temperature is 60°C and the reaction time is 8h. After the reaction is completed, pour the reaction system into 150mL of ethyl acetate to precipitate the precipitated polymer solid product, wash the solid product with acetone, and vacuum dry at 45°C for 48h to obtain the sulfonic acid functionalized polymer SPS-8.
[0204] The EW of SPS-8 is 1212.6 g / mol, and the structural formula is:
[0205]
[0206] Example 11: Preparation of Sulfonic Acid Functionalized Polymer
[0207] Weigh 1.49g of PSOH-9 in Example 5, dissolve and disperse in 20mL of anhydrous DMAC to obtain a polymer solution. Add 0.72g of sodium hydride to the polymer solution and stir at 40°C for 0.5h to perform hydrogen extraction reaction. Add 4.88g of 1,3-propanesulfonic acid lactone as a sulfonation reagent for sulfonation reaction, the sulfonation reaction temperature is 60°C, and the reaction time is 24h. After the reaction is completed, add 10mL of ice water to terminate the reaction, pour the reaction system into 150mL of ethyl acetate to precipitate the precipitated polymer solid product, wash the solid product with acetone, and vacuum dry at 45°C for 48h to obtain the sulfonic acid functionalized polymer SPS-9.
[0208] The EW of SPS-9 is 257.3 g / mol, and the structural formula is:
[0209]
[0210] Example 12: Preparation of Sulfonic Acid Functionalized Polymer
[0211] Weigh 1.5g of PSOH-5 in Example 5, dissolve and disperse in 40mL of anhydrous toluene to obtain a polymer solution. Add 0.72g of sodium hydride to the polymer solution and stir at 40°C for 0.5h to carry out hydrogen extraction reaction. Then add 5.45g of 1,4-butanesulfonate as a sulfonation reagent for sulfonation reaction. The sulfonation reaction temperature is 60°C and the reaction time is 16h. After the reaction is completed, add 3mL of ice water to terminate the reaction, pour the reaction system into 150mL of ethyl acetate to precipitate the precipitated polymer solid product, wash the solid product with acetone, and vacuum dry at 45°C for 48h to obtain the sulfonic acid functionalized polymer SPS-5.
[0212] The EW of SPS-5 is 339.8 g / mol, and the structural formula is:
[0213]
[0214] Figure 4 This is the infrared spectrum of the sulfonic acid functionalized polymer SPS-5. -1 The broad and smooth vibration peak near 2924cm is the stretching vibration of the hydroxyl group. This characteristic peak comes from the bound water of the sulfonic acid group. -1 and 2854cm -1 The symmetric stretching vibration and asymmetric stretching vibration of methylene come from the main chain of the polymer and the side chain of alkyl sulfonic acid. The intensity of the symmetric stretching vibration peak is greater than that of the asymmetric stretching vibration peak, indicating that the methylene is in a more polar environment. This also verifies that the polymer molecule introduces a highly polar functional group (sulfonic acid group); 1035-1181cm -1 The characteristic peak at is attributed to the stretching vibration of O=S=O in the sulfonic acid group.
[0215] Example 13: Preparation of Sulfonic Acid Functionalized Polymer
[0216] Weigh 0.50g of PSOH-6 in Example 5 and dissolve it in 15mL of anhydrous toluene, then add 0.24g of sodium hydride, and stir at 40°C for 0.5h to carry out hydrogen extraction reaction. Then add 1.8g of tetrafluorosulfone as a sulfonation reagent to carry out sulfonation reaction, the sulfonation reaction temperature is 100°C, and the reaction time is 10h. After the reaction is completed, add 4mL of ice water to terminate the reaction, pour the reaction system into 60mL of acetone to precipitate the precipitated polymer solid product, use hydrochloric acid to acidify the solid product to replace the cation bound to the sulfonic acid functional group with hydrogen ions, wash the solid product with acetone, and vacuum dry it at 45°C for 48h to obtain the sulfonic acid functionalized polymer SPS-6.
[0217] The EW of SPS-6 is 576.4 g / mol, and the structural formula is:
[0218]
[0219] Example 14: Preparation of Sulfonic Acid Functionalized Polymer
[0220] Weigh 1.5g of PSOH-7 in Example 5, dissolve and disperse in 30mL of anhydrous toluene to obtain a polymer solution. Add 0.72g of sodium hydride to the polymer solution and stir at 40°C for 0.5h to carry out hydrogen extraction reaction. Add 2.85g of sodium 4-(2-bromoethyl)benzenesulfonate as a sulfonating reagent for sulfonation reaction, the sulfonation reaction temperature is 105°C, and the reaction time is 12h. Take a small amount of sample to determine the EW of the intermediate product to be 734.5g / mol. Add 2.32g of 1,4-butanesulfonic acid lactone as a sulfonating reagent to the reaction system to continue the sulfonation reaction, the sulfonation reaction temperature is 60°C, the reaction time is 12h, and 10mL of ice water is added after the reaction is completed to terminate the reaction. The reaction system was poured into 150 mL of ethyl acetate to precipitate a solid polymer product. The solid product was acidified with hydrochloric acid to replace the cations bound to the sulfonic acid functional group with hydrogen ions. The solid product was washed with acetone and vacuum dried at 45° C. for 48 h to obtain a sulfonic acid functionalized polymer SPS-7.
[0221] The EW of SPS-7 is 460.2 g / mol, and the structural formula is:
[0222]
[0223] Sodium 4-(2-bromoethyl)benzenesulfonate is used as a sulfonation reagent. The side chain of the polymer grafting has a large steric hindrance. Only part of the hydroxyl groups participate in the reaction of grafting sulfonic acid functional groups. After adding 1,4-butanesulfonic acid lactone, the unreacted hydroxyl groups further react to graft butanesulfonic acid to achieve complete reaction of the hydroxyl groups. Since the reaction activity of sodium 4-(2-bromoethyl)benzenesulfonate is low, it basically does not react at 60°C. According to the EW values of the intermediate product and SPS-7, it can be inferred that (x7+x7') / (w7+w7')=0.53:0.47.
[0224] Example 15: Preparation of Sulfonic Acid Functionalized Polymer
[0225] Different from Example 13, the sulfonating agent is 1.36 g of 1-methyl-1,3-propane sultone, and the sulfonic acid functionalized polymer SPS-6A is obtained. The EW of SPS-6A is 532.6 g / mol.
[0226] Example 16: Preparation of Sulfonic Acid Functionalized Polymer
[0227] Different from Example 13, the sulfonating agent is 2.30 g of 1,2,2-trifluoro-2-hydroxy-1-trifluoromethylethanesulfonic acid, and the sulfonic acid functionalized polymer SPS-6B is obtained. The EW of SPS-6B is 626.4 g / mol.
[0228] Example 17: Preparation of Sulfonic Acid Functionalized Polymer
[0229] Different from Example 13, the sulfonating agent is 1.40 g of 1-fluoro-1,3-propane sultone, and the sulfonic acid functionalized polymer SPS-6C is obtained. The EW of SPS-6C is 536.4 g / mol.
[0230] Example 18: Preparation of ion exchange membrane
[0231] The sulfonic acid functionalized polymer SPS-4 in Example 9 was dissolved and dispersed in DMSO to obtain a polymer solution with a concentration of 5%, which was cast in an ultra-flat petri dish and dried at 80° C. for 24 h to obtain an ion exchange membrane PEM-1 with an average thickness of 200 μm. The IEC of PEM-1 was 1.33 mmol / g.
[0232] Example 19: Preparation of ion exchange membrane
[0233] The SPS-8 in Example 10 was dissolved in a mixed solvent of water and n-propanol to obtain a polymer solution with a concentration of 25%, and the mass ratio of water to n-propanol was 9:1. The dispersion was obtained by slit coating on a release film, and dried at 100° C. for 10 min to obtain an ion exchange membrane PEM-8 with a thickness of 5 μm. The IEC of PEM-8 was 0.82 mmol / g.
[0234] Example 20: Preparation of ion exchange membrane
[0235] The SPS-9 in Example 11 was dissolved in a mixed solvent of water and methanol to obtain a polymer solution with a concentration of 30%, and the mass ratio of water to methanol was 95:5. The solution was cast in an ultra-flat petri dish and dried at 45°C for 24 hours to obtain an ion exchange membrane PEM-9 with an average thickness of 100 μm. The IEC of PEM-9 was 3.89 mmol / g.
[0236] Example 21: Preparation of ion exchange membrane
[0237] The SPS-5 in Example 12 was dissolved in a mixed solvent of water and ethanol to obtain a polymer solution with a concentration of 15%, and the mass ratio of water to ethanol was 2:3. The solution was coated on both sides of an ethylene-tetrafluoroethylene microporous membrane (thickness 22-28 μm, porosity 72%, pore size distribution 202-507 nm) by a doctor blade, dried at 60° C. for 15 min, heated to 100° C. for 5 min, and finally heat treated at 140° C. for 5 min to obtain an ion exchange membrane PEM-5 with an average thickness of 50 μm containing an ethylene-tetrafluoroethylene reinforcement layer.
[0238] The IEC of PEM-5 is 2.94 mmol / g, and the water absorption rate is 113.5%. Compared with D-PEM-5 of Comparative Example 2, PEM-5 still maintains a complete film morphology and has better dimensional stability.
[0239] Example 22: Preparation of ion exchange membrane
[0240] The SPS-6 in Example 13 was dissolved in a mixed solvent of o-dichlorobenzene and n-hexanol, with the volume ratio of o-dichlorobenzene to n-hexanol being 85:15, to obtain a polymer solution with a concentration of 10%, which was cast in an ultra-flat culture dish, dried at 50°C for 6h, and heated to 120°C for 15min to obtain an ion exchange membrane PEM-6 with an average thickness of 45μm.
[0241] Example 23: Preparation of ion exchange membrane
[0242] Different from Example 22, the sulfonic acid functionalized polymer is SPS-6A in Example 15, and the ion exchange membrane PEM-6A with an average thickness of 45 μm is obtained.
[0243] Example 24: Preparation of ion exchange membrane
[0244] Different from Example 22, the sulfonic acid functionalized polymer is SPS-6B in Example 16, and the ion exchange membrane PEM-6B with an average thickness of 45 μm is obtained.
[0245] Example 25: Preparation of ion exchange membrane
[0246] The difference from Example 22 is that the sulfonic acid functionalized polymer is SPS-6C in Example 17, and the ion exchange membrane PEM-6C with an average thickness of 45 μm is obtained.
[0247] Example 26: Preparation of ion exchange membrane
[0248] The SPS-7 in Example 14 was dissolved in a mixed solvent of toluene and n-hexanol in a volume ratio of 80:20 to obtain a polymer solution with a concentration of 15%. The solution was coated on both sides of the ePTFE membrane (thickness 8-10 μm, porosity 76%, pore size distribution 190-280 nm) with a scraper, dried at room temperature for 5 min, dried at 80°C for 10 min, and then heat treated at 140°C for 5 min to obtain an ion exchange membrane PEM-7 containing an ePTFE membrane reinforcement layer with an average thickness of 12 μm.
[0249] Example 27: Preparation of ion exchange membrane
[0250] Different from Example 26, the sulfonic acid functionalized polymer is SPS-4 in Example 9, and an ion exchange membrane PEM-4 having an average thickness of 12 μm containing an ePTFE membrane reinforcement layer is obtained. PEM-4 is acidified in a 1 mol / L hydrochloric acid solution at 80° C. for 24 h to obtain a proton exchange membrane PEM-4H in which the cation is a hydrogen ion.
[0251] Comparative Example 1: Preparation of sulfonated styrene polymers
[0252] Sulfonated styrene polymers were prepared by using acetosulfonate as a sulfonating agent and carrying out a sulfonation reaction with the styrene polymer in Example 3. The styrene polymer, the sulfonated styrene polymer number, EW value and side chain structure are shown in Table 4.
[0253] Table 4
[0254]
[0255] Comparative Example 2: Preparation of ion exchange membrane
[0256] Different from Example 21, the ion exchange resin used to prepare the ion exchange membrane is D-SPS-5 in Comparative Example 1, and the obtained ion exchange membrane D-PEM-5 has an average thickness of 50 μm and contains an ethylene-tetrafluoroethylene reinforcement layer.
[0257] The IEC of D-PEM-5 was 2.92 mmol / g. The ion exchange resin dissolved and broke in water, and the water absorption rate could not be determined.
[0258] Comparative Example 3: Preparation of ion exchange membrane
[0259] The difference from Example 22 is that the ion exchange resin used to prepare the ion exchange membrane is D-SPS-6 in Comparative Example 1. An ion exchange membrane D-PEM-6 with an average thickness of 45 μm is obtained.
[0260] Comparative Example 4: Preparation of ion exchange membrane
[0261] The difference from Example 26 is that the ion exchange resin used to prepare the ion exchange membrane is D-SPS-7 in Comparative Example 1. The obtained ion exchange membrane D-PEM-7 has an average thickness of 12 μm and contains an ePTFE membrane reinforcement layer.
[0262] Comparative Example 5: Preparation of Sulfonic Acid Functionalized Polymer by Alkylation Reaction
[0263] Weigh 2g of SEBS (Kraton G1652H) in Example 3 and disperse it in 25mL of 1,2-dichloroethane and 25mL of cyclohexane at room temperature. Add 2g of anhydrous aluminum chloride and stir and disperse for 10min. Add 2.5g of 1-methyl-1,3-propane sultone, heat to 70°C, and stir to react for 8h. After the reaction is completed, cool to room temperature and add 20g of crushed ice to deactivate the catalyst. Pour the reactant into 300mL of 2mol / L hydrochloric acid solution and precipitate. Filter to obtain a solid and wash it with pure water until neutral. Vacuum dry at 45°C for 24h to obtain a dry solid product D-SPS-6A.
[0264] The repeating unit structure of the grafted sulfonic acid group of D-SPS-6A is:
[0265]
[0266] Wherein, M1 is a hydrogen ion or an aluminum ion.
[0267] Comparative Example 6: Preparation of Sulfonic Acid Functionalized Polymer by Alkylation
[0268] Different from Comparative Example 5, the sulfonating agent involved in the reaction is 3.2 g of 1,2,2-trifluoro-2-hydroxy-1-trifluoromethylethanesulfonic acid, and a dry solid product D-SPS-6B is obtained.
[0269] The repeating unit structure of the grafted sulfonic acid group of D-SPS-6B is:
[0270]
[0271] Wherein, M1 is a hydrogen ion or an aluminum ion.
[0272] Comparative Example 7: Preparation of ion exchange membrane
[0273] Different from Example 23, the sulfonic acid functionalized polymer is D-SPS-6A in Comparative Example 5, and the obtained ion exchange membrane D-PEM-6A has an average thickness of 45 μm.
[0274] Comparative Example 8: Preparation of ion exchange membrane
[0275] Different from Example 24, the sulfonic acid functionalized polymer is D-SPS-6B in Comparative Example 6, and the obtained ion exchange membrane D-PEM-6B has an average thickness of 45 μm.
[0276] The IEC, water absorption, conductivity, tensile strength and free radical resistance of the ion exchange membranes in the examples and comparative examples are shown in Table 5.
[0277] Table 5
[0278]
[0279]
[0280] Compared with D-PEM-6, PEM-6 has similar IEC, but PEM-6 containing hydrophobic spacers has lower water absorption. This is because the introduction of hydrophobic spacers reduces the content of free water in the membrane material, reduces the water absorption and swelling of the material, and improves the dimensional stability of the ion exchange membrane. This low water absorption can increase the number of ionic groups per unit volume and improve the conductivity of the ion exchange membrane. The introduction of hydrophobic spacers also increases the tensile strength of the membrane and the free radical resistance of the material, which is beneficial to the application of ion exchange membranes in fuel cells, flow batteries, water electrolysis and electrodialysis. PEM-7 and D-PEM-7 contain microporous membrane reinforcement layers with high tensile strength. The key properties of PEM-7 containing hydrophobic spacers are better than those of D-PEM-7.
[0281] Compared with D-PEM-6A, PEM-6A has the same alkyl sulfonic acid structure in the side chain. Since the reactivity of hydroxyl group is much higher than that of benzene ring, SPS-6A has a higher degree of grafting and PEM-6A has a higher IEC. Another reason for the difference in IEC is that the catalyst of D-SPS-6A is aluminum chloride. A small amount of catalyst will remain in the soft segment (ethylene-butene segment) of the polymer or become the cation of the sulfonic acid group, which will lead to a decrease in the IEC of the ion exchange membrane. Due to the high degree of side reactions of D-SPS-6A prepared by alkylation reaction and the cross-linking effect of multivalent cations, the molding quality of D-PEM-6A is not as good as PEM-6A, which is manifested as lower tensile strength and higher water absorption. At the same time, in the free radical resistance test, the residual transition metal cations will enhance the ability of Fenton reagent to generate free radicals, accelerate material degradation, and show higher mass loss after Fenton reagent treatment. The difference in conductivity performance is mainly affected by the poisoning of multivalent metal cations and molding quality. PEM-6A with good molding quality and no multivalent metal ion impurities has higher conductivity. The perfluoroalkyl sulfonic acid structure of the side chain of PEM-6B and D-PEM-6B is the same. PEM-6B has higher IEC, conductivity and tensile strength, as well as lower water absorption and mass loss. Its core performance indicators are better than those of D-PEM-6B. PEM-4H has the best free radical resistance, which is due to its fluorocarbon main chain. By optimizing the appropriate polymer main chain chemical structure, side chain chemical structure and ion exchange membrane composite structure, an ion exchange membrane with controllable water absorption, high conductivity, high tensile strength and good chemical stability can be prepared.
[0282] PEM-6 is used in flow battery separators at a current density of 120 mA / cm 2 Under the conditions of , the coulombic efficiency of the flow battery single cell is 95.4%, the voltage efficiency is 88.5%, and the energy efficiency is 82.7%, which has a high flow battery efficiency. Due to the severe swelling of D-PEM-6 due to water absorption and low mechanical properties, it was damaged during the assembly and circulation of the flow battery, and the flow battery efficiency was not measured.
[0283] Figure 1 This is the cross-sectional SEM image of PEM-7. The sulfonic acid functionalized polymer SPS-7 and the ePTFE membrane reinforcement layer are evenly compounded, and the film-forming effect is good.
[0284] Figure 2 This is the polarization curve of a single cell of a PEM-7 fuel cell. The results show that the power density of PEM-7 at 0.65V is 1678.4mA / cm 2 Since D-PEM-7 has a high water absorption rate and low mechanical strength, wrinkles and damage occurred during the membrane electrode preparation process, and the single cell performance test was not carried out.
[0285] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0286] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.
Claims
1. A sulfonic acid functionalized polymer, characterized in that The sulfonic acid functionalized polymer comprises a repeating unit A0 represented by formula (1): Wherein, R1 is selected from H or F; R2 is selected from H, F or CH3; a is selected from an integer of 0 to 12; and R3 is selected from an alkyl sulfonic acid, a fluoroalkyl sulfonic acid or an aryl sulfonic acid.
2. The sulfonic acid functionalized polymer according to claim 1, characterized in that R3 is selected from at least one of the following structural formulas: Among them, M + is selected from cations; b is selected from integers of 0 to 6; c is selected from integers of 0 to 12; R4~R 17 Each independently selected from H, F, C1-C6 alkyl, C1-C6 perfluoroalkyl or C6-C 12 The aromatic group.
3. The sulfonic acid functionalized polymer according to claim 1, characterized in that The sulfonic acid functionalized polymer further comprises repeating units A1: wherein R1 is selected from H or F; R2 is selected from H, F or CH3; R 18 Selected from H, C1-C12 alkyl, C1-C6 perfluoroalkyl or C6-C 12 The aromatic group; and / or, the sulfonic acid functionalized polymer further comprises a repeating unit A2, wherein the repeating unit A2 comprises at least one of -C(CH3)2CH-, -CH2CH2-, -CH(CH3)CH2- or -CH(CH2CH3)CH2-; And / or, the sulfonic acid functionalized polymer further comprises repeating unit A3: wherein R1 is selected from H or F; R2 is selected from H, F or CH3; a is selected from an integer of 0 to 12; R 19 An alkoxy group selected from -OH, -F, -Cl, -Br, -I or C1-C4.
4. The sulfonic acid functionalized polymer according to claim 1, characterized in that The molar percentage of the repeating unit A0 in the benzene ring-containing repeating unit of the sulfonic acid functionalized polymer is defined as the sulfonation degree of the sulfonic acid functionalized polymer, and the sulfonation degree is ≥ 0.1%; and / or, the sulfonic acid functionalized polymer has a n 30,000 to 1,000,000; and / or, the sulfonic acid functionalized polymer has a w 30,000 to 1,500,000; And / or, the EW of the sulfonic acid functionalized polymer is 244 to 5000 g / mol.
5. A method for preparing a sulfonic acid functionalized polymer according to any one of claims 1 to 4, characterized in that: include: The hydroxyl functionalized styrene polymer is subjected to a sulfonation reaction with a hydrogen extraction agent and a sulfonation agent to obtain a sulfonic acid functionalized polymer.
6. The method for preparing a sulfonic acid functionalized polymer according to claim 5, characterized in that: The hydrogen extraction agent includes at least one of alkali metal oxides, alkali metal hydrides, alkali metal peroxides, alkali metal hydroxides, alkali metal carbonates or alkali metal organic compounds; And / or, the sulfonated reagent comprises at least one of the following structural formulas: Among them, R4~R 17 Each independently selected from H, F, C1-C6 alkyl, C1-C6 perfluoroalkyl or C6-C 12 b is an integer selected from 0 to 6; c is an integer selected from 0 to 12; M + is selected from cations; and X is selected from halogens.
7. The method for preparing a sulfonic acid functionalized polymer according to claim 5, characterized in that: The molar ratio of the hydroxyl functional group in the hydroxyl functionalized styrene polymer to the sulfonated reagent is 1:0.1-30; and / or, the molar ratio of the hydroxyl functional group in the hydroxyl functionalized styrene polymer to the hydrogen extraction agent is 1:0.1-20; And / or, the temperature of the sulfonation reaction is 20-160°C; And / or, the sulfonation reaction time is 0.5-72h.
8. An ion exchange membrane, characterized in that: The invention comprises the sulfonic acid functionalized polymer described in any one of claims 1 to 4 or the sulfonic acid functionalized polymer prepared by the preparation method described in any one of claims 5 to 7.
9. The ion exchange membrane according to claim 8, characterized in that The thickness of the ion exchange membrane is 3 to 500 μm; and / or, the IEC of the ion exchange membrane is 0.2 to 4.10 mmol / g; And / or, the ion exchange membrane further comprises a reinforcement membrane, and the sulfonic acid functionalized polymer is supported on the reinforcement membrane.
10. A method for preparing an ion exchange membrane according to claim 8 or 9, characterized in that: include: The sulfonic acid functionalized polymer is dispersed in a solvent to obtain a dispersion, and the dispersion is subjected to film formation and drying to obtain an ion exchange membrane.
11. Use of the sulfonic acid functionalized polymer according to any one of claims 1 to 4 or the ion exchange membrane according to claim 8 or 9, characterized in that: At least one of fuel cells, water electrolysis, flow batteries, chlor-alkali industry, lithium batteries, electrodialysis, osmosis, fabric coatings, packaging materials, wearable devices, biomedical devices, medical materials or antibacterial materials.