Aerogel for freshness monitoring and preparation method and application thereof

The pH indicator label of the porous polymer network structure prepared by Schiff alkali cross-linking technology solves the accuracy and safety of existing food freshness monitoring methods, and achieves efficient and reliable monitoring of meat food freshness.

CN119060416APending Publication Date: 2024-12-03SICHUAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411155294.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing food freshness monitoring methods have problems such as strong subjectivity, complexity, time-consuming, single indicators and limited accuracy, especially in the process of storage and transportation, which leads to food safety risks.

Method used

The aldehyde carboxymethylcellulose sodium, gelatin and anthocyanin composition are formed into a porous polymer network structure through Schiff base crosslinking technology, and a pH indicator label with high response and high sensitivity is prepared for monitoring meat Food freshness.

Benefits of technology

Real-time monitoring of the freshness of meat foods is achieved, providing high accuracy and reliability judgment on freshness, and improving the guarantee of food safety and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060416A_ABST
    Figure CN119060416A_ABST
Patent Text Reader

Abstract

The invention discloses aerogel for freshness monitoring as well as a preparation method and application of the aerogel. The aerogel comprises a porous polymer network structure formed by an anthocyanin composition, aldehyde sodium carboxymethyl cellulose and gelatin. According to the invention, aldehyde sodium carboxymethyl cellulose, gelatin and anthocyanin are cross-linked to successfully prepare the pH indication label with high response and high sensitivity. The aerogel disclosed by the invention has excellent microstructure, thermal stability, mechanical property, color reaction and storage stability, shows excellent color rendering property when the pH value is 3-12, improves the reaction capacity to decay gas, and can be used for monitoring the freshness of meat foods, so that the aerogel can be used for preparing intelligent food packaging materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of food intelligent packaging, and in particular relates to an aerogel for freshness monitoring, and a preparation method and application thereof. Background Art

[0002] In recent years, food safety has become a global concern, especially in the storage and transportation of perishable foods. According to the Food and Agriculture Organization of the United Nations (FAO), about one-third of food is wasted each year, totaling about 1.3 billion tons. Chicken accounts for about 75% of global poultry consumption and is particularly susceptible to microbial growth due to its high protein and moisture content. If freshness is not effectively monitored during storage and transportation, it will lead to serious food safety accidents and pose a huge health risk to consumers. Therefore, implementing efficient freshness monitoring is essential to ensure food safety and quality.

[0003] Traditionally, sensory evaluation, chemical analysis, and microbiological testing are used to ensure food safety. However, these methods are highly subjective, complex, time-consuming, have a single indicator, have limited accuracy, and require specialized equipment and personnel. Therefore, emerging smart packaging technologies have attracted much attention because they can monitor and track food status, quality, and safety in real time. Freshness indicators can provide qualitative or semi-quantitative information on food quality without destroying the packaging, thereby helping consumers to intuitively and scientifically judge food quality. Several aerogels for freshness indication have been developed. These materials are composed of plastics (such as polyaniline, polyimide, polyurea) and inorganic materials (such as silica). These substrates have the disadvantage of poor degradability, so recent research has focused more on sustainable polymers. Although the prospects are broad, current smart labels are still limited in performance and stability, so it is necessary to develop more efficient and reliable packaging materials. Summary of the invention

[0004] In order to solve at least some of the problems in the above-mentioned prior art, the present invention forms a porous polymer network structure of sodium aldehyde carboxymethyl cellulose, gelatin and anthocyanin composition through Schiff base crosslinking technology, and prepares a pH indicator label with high response and high sensitivity, which improves the reaction ability to corruption gas, so that it can be used to monitor the freshness of meat food, and then used to prepare food intelligent packaging materials. Specifically, the present invention includes the following contents.

[0005] In a first aspect of the present invention, an aerogel for freshness monitoring is provided, which comprises a porous polymer network structure formed by aldehyde carboxymethyl cellulose sodium, gelatin and anthocyanin composition.

[0006] In certain embodiments, according to the aerogel for freshness monitoring of the present invention, the mass ratio of the sodium aldehyde carboxymethyl cellulose, gelatin and anthocyanin composition is (2-15):(20-300):1.

[0007] In certain embodiments, according to the aerogel for freshness monitoring of the present invention, the porosity of the aerogel is 50%-80%, and the density is 0.03-0.05 g / cm 3 , the pore diameter is 150-500μm.

[0008] In a second aspect of the present invention, a method for preparing an aerogel for freshness monitoring according to the present invention is provided, which comprises the following steps:

[0009] (1) preparing sodium aldehyde carboxymethyl cellulose;

[0010] (2) extracting anthocyanin composition;

[0011] (3) dissolving the sodium aldehyde carboxymethyl cellulose and gelatin in an aqueous medium, stirring, mixing with the anthocyanin composition, and freeze-drying to obtain the aerogel.

[0012] In certain embodiments, the method for preparing aerogel for freshness monitoring according to the present invention further comprises the step of standing at 20-30° C. for 1-3 hours before freeze-drying.

[0013] In certain embodiments, according to the method for preparing aerogel for freshness monitoring of the present invention, the aldehyde carboxymethyl cellulose sodium is prepared by reacting sodium carboxymethyl cellulose and sodium periodate solution.

[0014] In certain embodiments, according to the method for preparing aerogel for freshness monitoring of the present invention, the stirring comprises stirring at 30-50° C. for 2-6 hours.

[0015] In certain embodiments, according to the method for preparing aerogel for freshness monitoring of the present invention, the freeze-drying comprises drying at -70°C to -90°C for 30-60h.

[0016] A third aspect of the present invention provides use of the aerogel for freshness monitoring according to the present invention in preparing smart food packaging materials.

[0017] A fourth aspect of the present invention provides a smart food packaging material, comprising the aerogel for freshness monitoring according to the present invention.

[0018] According to a fifth aspect of the present invention, there is provided a method for monitoring the freshness of meat products, which comprises the step of using the aerogel according to the present invention.

[0019] The present invention extracts anthocyanin compositions from peanut skin waste, and embeds the anthocyanin compositions into an aerogel having a schiff base-crosslinked sodium carboxymethyl cellulose and a porous polymer network structure of gelatin, thereby preparing a pH indicator label with high response and high sensitivity. At the same time, the aerogel of the present invention has excellent microstructure, thermal stability and mechanical properties, and exhibits excellent color development at a pH value of 3-12, thereby improving the responsiveness to corruption gases and being able to be used to monitor the freshness of meat food, so that it can be used to prepare food intelligent packaging materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 a is the color reaction of PC and DG-PC in buffer solutions with different pH values; b is the UV-visible absorption spectrum of PC in buffer solutions with different pH values; c is the molecular structure change of PC with different colors.

[0021] Figure 2 a is the Fourier transform infrared spectrum (FTIR) of CMC and DCMC; b is the Fourier transform infrared spectrum of GA and DG aerogels; c is the Fourier transform infrared spectrum of DG-PC aerogel; d is the X-ray diffraction (XRD) pattern of CMC and DCMC; e is the XRD pattern of GA and DG aerogels; f is the XRD pattern of DG-PC aerogel.

[0022] Figure 3 a and b are the thermogravimetric analysis (TGA) curve and differential thermogravimetric (DTG) curve of each substance, respectively.

[0023] Figure 4 ai are the SEM images of DCMC, GA, DG-2, DG-5, DG-10, DG-20, DG-PC1, DG-PC2 and DG-PC3 aerogels, respectively.

[0024] Figure 5 The mechanical properties of GA, DG aerogel and DG-PC aerogel are shown, where a and b are stress-strain curves; c and d are compressive strengths of each material; lowercase letters (ac) on the bars indicate significant differences between the materials (P<0.05).

[0025] Figure 6 a and b are the porosities of GA, DG aerogel and DG-PC aerogel, respectively; c is the water stability of GA, DG aerogel and DG-PC aerogel. The lowercase letters (ad) on the bars indicate significant differences between the materials (P<0.05).

[0026] Figure 7a is a schematic diagram of monitoring the freshness of chicken at 4°C based on DG-PC aerogels with different anthocyanin concentrations; b is the change in pH value of chicken during storage; ce are the changes in TVB-N, TVC and ΔE of chicken, respectively; f is a significance analysis based on the Pearson correlation coefficient; the numerical value in the figure is the size of the correlation coefficient, and × indicates insignificant (P>0.05).

[0027] In the drawings of the present invention, PC refers to anthocyanidin, CMC refers to sodium carboxymethyl cellulose, DCMC refers to sodium aldehyde carboxymethyl cellulose, GA refers to gelatin, DG refers to the cross-linked product of DCMC and gelatin Schiff base, and DG-PC means that anthocyanidin is loaded in DG. DETAILED DESCRIPTION

[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0029] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that the upper and lower limits of the scope and each intermediate value therebetween are specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art to which the invention belongs. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0031] Aerogel

[0032] In one aspect of the present invention, an aerogel for freshness monitoring is provided, which comprises a porous polymer network structure formed by an aldehyde carboxymethyl cellulose sodium, gelatin and anthocyanin composition.

[0033] The present invention utilizes Schiff base cross-linking technology to form a porous polymer network structure between sodium aldehyde carboxymethyl cellulose and gelatin, thereby enhancing the mechanical properties of the aerogel, and utilizes the hydroxyl groups of the anthocyanin composition to interact with the amino groups and hydroxyl groups in the aerogel matrix through hydrogen bonds, thereby promoting the dispersion and stability of the anthocyanin composition.

[0034] A three-dimensional aerogel with excellent mechanical properties, high stability, high porosity, low density and high specific surface area can be obtained by controlling the mass ratio of sodium aldehyde carboxymethyl cellulose, gelatin and anthocyanin within a suitable range. The amount of sodium aldehyde carboxymethyl cellulose should not be too high or too low, otherwise it will affect the porosity, density and mechanical properties of the aerogel finally prepared. In the present invention, the mass ratio of sodium aldehyde carboxymethyl cellulose and gelatin is 1:9.5 to 1:48, preferably 1:9.8 to 1:46, and preferably 1:10 to 1:45, and further preferably 1:15 to 1:25, for example 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, 1:21, 1:22, 1:23, 1:24, 1:25. In a preferred embodiment, the mass ratio of the sodium aldehyde carboxymethyl cellulose, gelatin and anthocyanin composition is (2-15): (20-300): 1, preferably (2-14): (30-280): 1, further preferably (2-13): (40-260): 1, more preferably (2-12): (50-240): 1, for example 2:50: 1, 3:50: 1, 4:50: 1, 5:50: 1, 6:50: 1, 7:50: 1, 8:50: 1, 9:50: 1, 10:50: 1, 11:50: 1, 12:50: 1, 2:95: 1, 3:95: 1, 4:95: 1, 5:95: 1, 6:95: 1 : 5:1, 7:95:1, 8:95:1, 9:95:1, 10:95:1, 11:95:1, 12:95:1, 2:190:1, 3:190:1, 4:190:1, 5:190:1, 6:190:1, 7:190:1, 8:190:1, 9:190:1, 10:190:1, 11:190:1, 12:190:1, 2:240:1, 3:240:1, 4:240:1, 5:240:1, 6:240:1, 7:240:1, 8:240:1, 9:240:1, 10:240:1, 11:240:1, 12:240:1. In a preferred embodiment, the mass ratio of the sodium aldehyde carboxymethyl cellulose, gelatin and anthocyanidin composition is 10:190:1. In another preferred embodiment, the mass ratio of the sodium aldehyde carboxymethyl cellulose, gelatin and anthocyanidin composition is 5:95:1. In another preferred embodiment, the mass ratio of the sodium aldehyde carboxymethyl cellulose, gelatin and anthocyanidin composition is 2.5:47.5:1.

[0035] In the present invention, the source of the anthocyanin composition is not particularly limited, and it can be extracted from any food industry byproduct rich in anthocyanins, examples of which include but are not limited to peanuts (especially purple seed coat or black seed coat peanuts), purple sweet potatoes, red cabbage, blueberries, mulberries, plums, black soybeans, black beans and black rice, etc. In a preferred embodiment, the anthocyanin loaded in the porous polymer network structure of the present invention is extracted from an anthocyanin mixture of peanut seed coats, and the anthocyanin composition of the present invention has different numbers of substitutions on the ring, hydroxylation sites, methylation patterns and glycosylation sites, so that the freshness of the test object can be monitored according to the differences in the chemical structures and colors of the different anthocyanins.

[0036] In the present invention, in order to make the aerogel have excellent properties (such as but not limited to mechanical properties, color development properties and thermal stability, etc.), it is necessary to control its density, porosity and pore diameter within an appropriate range. Among them, the density, porosity and pore diameter of the aerogel can be measured by methods known in the art, and there is no particular limitation on this. In a preferred embodiment, the porosity of the aerogel prepared from the above components is 50%-80%, preferably 50%-72%, and also preferably 50%-67%, such as 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%; the density is 0.03-0.05g / cm 3 , preferably with a density of 0.0394-0.0428 g / cm 3 , for example 0.039, 0.040, 0.041, 0.042 g / cm 3 The pore diameter is 150-500 μm, preferably 160-490 μm, further preferably 170-480 μm, more preferably 180-440 μm, more preferably 190-430 μm, for example 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 310, 320, 330, 340, 350, 360, 370, 380, 390, 400, 410, 420, 430 μm. In a preferred embodiment, the aerogel has a porosity of 72.56% and a density of 0.0393 g / cm 3 , the pore diameter is 189.62 μm. In another preferred embodiment, the porosity of the aerogel is 65.68% and the density is 0.0401 g / cm 3 , the pore diameter is 399.45 μm. In another preferred embodiment, the porosity of the aerogel is 67.64% and the density is 0.0429 g / cm 3 , the pore diameter is 440.98μm.

[0037] In the present invention, the aerogel prepared from the above components has significantly improved mechanical properties, especially the mechanical properties of the sodium aldehyde carboxymethyl cellulose and the gelatin porous polymer network structure are further improved after the anthocyanin composition is added, wherein the compressive stress of the pure gelatin aerogel is significantly increased to 255-271 kPa after adding 2%-20% of the sodium aldehyde carboxymethyl cellulose, and the compressive stress of the prepared aerogel is further increased to 272-300 kPa after adding the anthocyanin composition, preferably 275-280 kPa, such as 275, 276, 277, 278, 278, 280 kPa. The amount of anthocyanin composition added should not be too high or too low, because too low anthocyanin composition will affect the color development performance and reduce the pore diameter, while too high anthocyanin composition will reduce the mechanical properties of the aerogel. Therefore, the addition amount of anthocyanin composition is controlled to 0.5%-2% of the weight of sodium carboxymethyl cellulose and gelatin, preferably 0.5%-1.9%, and also preferably 0.6%-1.9%, for example 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9%. When within the above concentration range, it has significantly improved mechanical properties, higher porosity and lower density. In certain embodiments, the amount of sodium aldehyde carboxymethyl cellulose is 31-119 parts by weight, preferably 40-110, also preferably 50-100, further preferably 50-80, for example 50, 55, 60, 65, 70, 75, 80 parts by weight; the amount of gelatin is 541-587 parts by weight, preferably 550-580 parts by weight, for example 550, 555, 560, 565, 570, 575, 580 parts by weight.

[0038] Preparation method

[0039] In one aspect of the present invention, a method for preparing an aerogel for freshness monitoring according to the present invention is provided, which comprises the following steps:

[0040] (1) preparing sodium aldehyde carboxymethyl cellulose;

[0041] (2) extracting anthocyanin composition;

[0042] (3) dissolving the sodium aldehyde carboxymethyl cellulose and gelatin in an aqueous medium, stirring, mixing with the anthocyanin composition, and freeze-drying to obtain the aerogel.

[0043] In the present invention, the aldehyde-based sodium carboxymethyl cellulose can be prepared using commercially available products or methods known in the art, such as using a suitable reagent to functionalize the sodium carboxymethyl cellulose with aldehyde groups.

[0044] In a preferred embodiment, the aldehyde carboxymethyl cellulose sodium is prepared by reacting sodium carboxymethyl cellulose and sodium periodate solution. In a specific embodiment, the aldehyde carboxymethyl cellulose sodium is prepared by the following steps: 3.0-8.0g (e.g., 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0g) of CMC is dissolved in 200-400mL (preferably 220-380mL, also preferably 240-360mL, for example 240, 250, 260, 270, 280, 290, 300, 310, 320, 330, 340, 350, 360mL) of ultrapure water, and then sodium periodate solution is added dropwise under stirring, wherein the molar ratio of CMC monomer to sodium periodate is (1:0.8)-(1:1.2), for example, 1:0.8, 1:0.9, 1:1.0, 1:1.1, 1:1.2. Then, the reaction is carried out at 20-30°C, preferably 21-29°C, such as 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, in the dark for 5-10 hours, such as 5, 6, 7, 8, 9, 10 hours. Then, ethylene glycol is added to neutralize the residual sodium periodate. Finally, the product is collected by dialysis and freeze drying.

[0045] In a preferred embodiment, the anthocyanin composition is obtained by extracting black peanuts. Peanuts are roasted at high temperature, for example, at 100-200°C for 10-30 minutes, and then peeled. The peanut skins are ground, stirred at 20-30°C and defatted with a polar solvent, vacuum filtered, and the residue is collected and dried. Then, the extraction is carried out with an alcohol solvent (preferably methanol, ethanol, n-butanol, etc., and 50-90% (v / v) ethanol is also preferred) under stirring at 20-30°C, with a liquid-to-solid ratio (v / m) of 10-50:1 (preferably 20-30:1) for 20-40 hours. Then, the filtrate is concentrated using a rotary evaporator at 30-60°C. Finally, the anthocyanin composition is obtained by freeze drying. Wherein, the polar solvent is selected from at least one of n-hexane, isopropanol, and ethyl acetate.

[0046] In a preferred embodiment, the stirring in step (2) includes stirring at 30-50°C, preferably 31-49°C, also preferably 32-48°C, further preferably 33-47°C, more preferably 34-46°C, more preferably 35-45°C, such as 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C for 2-6h, preferably 2.5-5.5h, also preferably 3-5h, such as 3, 3.2, 3.4, 3.6, 3.8, 4.0, 4.2, 4.4, 4.6, 4.8, 5h. In a specific embodiment, the stirring includes stirring at 40°C for 4h.

[0047] In a preferred embodiment, the freeze drying in step (2) comprises drying at -70°C to -90°C, preferably -72°C to -88°C, also preferably -74°C to -86°C, more preferably -75°C to -85°C, such as -75°C, -76°C, -77°C, -78°C, -79°C, -80°C, -81°C, -82°C, -83°C, -84°C, -85°C for 30-60h, preferably 31-59h, also preferably 32-58h, further preferably 33-57h, more preferably 34-56h, more preferably 35-55h, such as 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55h. In a specific embodiment, the freeze drying comprises drying at -80°C for 48h.

[0048] In a preferred embodiment, the freeze-drying step further comprises standing at 20-30°C, preferably 21-29°C, such as 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C for 1-3h, preferably 1.1-2.9h, also preferably 1.2-2.8h, more preferably 1.3-2.7h, such as 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8h. In a specific embodiment, the freeze-drying step further comprises standing at 25°C for 2h.

[0049] The present invention further provides application of the aerogel for freshness monitoring in smart food packaging materials.

[0050] method

[0051] One aspect of the present invention provides a method for monitoring the freshness of meat products, comprising the step of using the aerogel for freshness monitoring according to the present invention.

[0052] In a preferred embodiment, the method for monitoring the freshness of meat food of the present invention comprises bringing the aerogel of the present invention close to the meat food to be monitored (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 cm from the meat food) for a period of time, and when the aerogel is bluish purple, it indicates that the meat food is fresh, and when the aerogel is red, it indicates that the meat food to be monitored is spoiled. The spoilage can be judged by sensory evaluation of color, or the corresponding color can be converted into a color card color number comparison table for evaluation, or the color change can be converted into a standard color value to improve the accuracy of monitoring freshness. Those skilled in the art are familiar with how to perform the corresponding conversion, and there is no particular limitation on this.

[0053] Smart food packaging materials

[0054] In one aspect of the present invention, a smart food packaging material is provided, which includes the aerogel according to the present invention. The smart food packaging material may optionally include film-forming materials, synthetic or natural high molecular polymers, nanoparticles, etc., to achieve the purpose of the present invention.

[0055] In the present invention, examples of smart food packaging materials include but are not limited to liners, labels, and the like.

[0056] Example

[0057] 1. Materials and Methods

[0058] 1. Materials

[0059] Peanuts were obtained from the Institute of Industrial Crops, Sichuan Academy of Agricultural Sciences. Chicken was purchased from a local market (Chengdu, China). Carboxymethylcellulose (CMC, MW = 250,000, DS = 0.7, viscosity = 1500-3100 mPa.s) was purchased from Aladdin Co., Ltd. Gelatin (GA, gas strength 254 g Bloom) was purchased from Sodium periodate (NaIO4), ethylene glycol, sodium hydroxide (NaOH), and magnesium oxide (MgO) were purchased from Chengdu Kelong Chemical Co., Ltd. HPLC grade methanol (MeOH) was purchased from Merck. All anthocyanin decolorization standards were purchased from isoReag. Formic acid was purchased from Sigma-Aldrich. Hydrochloric acid was purchased from Xinyang Chemical Co., Ltd. All other chemicals and solvents were of analytical grade.

[0060] 2. Preparation of anthocyanins from black peanut skins

[0061] PC was extracted from black peanuts. First, black peanuts (2500 g) were placed in an oven, baked at 180°C for 20 min, and then peeled. The peanut skins were ground, stirred at 25°C, defatted with n-hexane, vacuum filtered, and the residues were collected and dried. Then, extraction was performed with 70% (v / v) ethanol with a liquid-to-solid ratio (v / m) of 25:1 at 25°C for 24 h. The filtrate was then concentrated using a rotary evaporator at 45°C. Finally, PC powder was obtained by freeze drying.

[0062] 2.1 UV-visible spectroscopy analysis

[0063] The UV-visible spectrum of PC solution was measured by UV-visible spectrophotometer. PC powder was dissolved in the required buffer (pH 3.0-12.0, c=0.25 mg / mL) adjusted with 0.1M HCl or NaOH solution and placed in the dark for 1 min. Then the color of the solution at each pH value was recorded by taking a photo, and the absorbance of the solution was measured in the range of 450-700 nm.

[0064] 2.2 HPLC-MS analysis

[0065] PC was characterized by liquid chromatography-quadrupole time-of-flight mass spectrometry. 50 mg of powder was weighed and extracted with 0.5 mL of methanol / water / hydrochloric acid (500:500:1, v / v / v). The extract was then vortexed for 5 min, sonicated for 5 min, and centrifuged at 12,000 g for 3 min at 4 °C. The supernatant was collected and filtered. The sample extract was analyzed by UPLC-ESI-MS / MS system. UPLC analysis conditions were as follows: chromatographic column: Waters ACQUITY BEH C18 (1.7 μm, 2.1 mm×100 mm); solvent system: water (0.1% formic acid) and methanol (0.1% formic acid); gradient program: 0 min 95:5 v / v, 6 min 50:50 v / v, 12 min 5:95 v / v, hold 2 min, 14 min 95:5 v / v, hold 2 min; flow rate 0.35 mL / min; temperature 40°C; injection volume 2 μL. ESI+ source conditions included: source temperature 550°C, ion spray voltage (IS) 5500 V, curtain gas (CUR) set to 35 psi. Linear ion trap (LIT) and triple quadrupole (QQQ) scans were obtained.

[0066] 3. Preparation of sodium carboxymethyl cellulose

[0067] First, 5.0 g of CMC was dissolved in 300 mL of ultrapure water, and then sodium periodate solution was added dropwise under stirring. The molar ratio of CMC monomer to sodium periodate was 1:1. Then, the reaction was carried out at 25 °C in the dark for 8 h. Then, ethylene glycol was added to neutralize the residual sodium periodate. Finally, the product was collected by dialysis and freeze drying.

[0068] 4. Preparation of indicator labels

[0069] DCMC (0, 12, 30, 60, 120 mg) and GA (600, 588, 570, 540, 480 mg) were added to 20 mL of ultrapure water, stirred continuously for 4 h at 40 °C to make them uniformly dispersed, and then allowed to stand at 25 °C for 2 h. After the prepared aerogels were solidified at 105 °C for 2 h, they were named GA, DG-2, DG-5, DG-10, and DG-20.

[0070] The exemplary preparation method of the pH-responsive anthocyanin smart indicator label is as follows: 75 mg DCMC and 1425 mg GA were added to 50 mL ultrapure water and stirred at 40°C for 4 h (equivalent to the concentration of DG-5). Then 0.5% (7.5 mg), 1% (15 mg) and 2% (30 mg) PC were added respectively, mixed well and allowed to stand at 25°C for 2 h, then pre-frozen at -80°C and freeze-dried for 48 h, and named DG-PC1, DG-PC2 and DG-PC3 respectively.

[0071] 5. Structure and performance determination

[0072] 5.1 FTIR

[0073] Fourier transform infrared spectroscopy was performed at room temperature in transmission mode (32 scans, step size: 4 cm -1 ) Collect 4000-600cm -1 Fourier transform infrared spectroscopy in the range.

[0074] 5.2XRD

[0075] The crystal structure of the aerogel was recorded using an X-ray diffractometer equipped with a copper sealed tube, a voltage of 40 kV, a current of 40 mA, an angle range of 5°-70° (2θ), and a speed of 5° / min.

[0076] 5.3 Thermogravimetric analysis

[0077] Thermogravimetric analysis was performed using a thermal analyzer under a nitrogen atmosphere. The sample (5.0 mg) was placed in a crucible and heated from 50°C to 600°C at a rate of 10°C / min.

[0078] 5.4 Microstructure

[0079] The microstructure of the aerogels was characterized by scanning electron microscopy at a magnification of 400× and an accelerating voltage of 5.00 kV. Before observation, all aerogels were fractured with liquid nitrogen to obtain cross-sections and gold-sprayed under vacuum.

[0080] 5.5 Color Characteristics

[0081] Aerogel color parameters (L * -Brightness, a * -Redness and b * -yellowness) was measured by a benchtop spectrophotometer. The color parameters were calibrated against a white plate. Three aerogels were selected from each group and randomly selected from multiple locations for testing. ΔE (total color difference) was determined by the following formula:

[0082]

[0083] in, is the initial color measurement of the aerogel, and L * , a * , b * It is the measured value of color after storage period.

[0084] 5.6 Density and porosity

[0085] The dimensions (length and diameter) and mass of the aerogel were measured using a digital caliper and an analytical balance, and the density was then calculated. The dry aerogel was soaked in ethanol to achieve adsorption saturation and then removed. Excess ethanol was wiped off with filter paper. The wet aerogel was reweighed. The porosity was calculated using the following formula:

[0086] Porosity(%)=(M2-M1) / ρV×100%;

[0087] Where M1 is the weight of dry aerogel, M2 is the weight of wet aerogel after soaking in ethanol (g), and V is the volume of dry aerogel (cm 3 ), ρ is the density of ethanol (0.785 g / cm 3 ).

[0088] 5.7 Mechanical properties

[0089] Each cylindrical aerogel (0.80 cm×1.30 cm) was compressed to 50% of the maximum deformation at a speed of 1 mm / min using a rheometer to obtain a stress-strain curve.

[0090] 6. Application of DG-PC in monitoring the freshness of chicken

[0091] To monitor the freshness of the chicken, 30 g of chicken was placed in a sealed container (the D×H size of the culture dish was 90 mm×15 mm), and then DG-PC (thickness: 4.0 mm±0.2 mm, diameter: 13 mm) was attached to the inside of the packaging cover without contacting the chicken ( Figure 7 ). The package was sealed and stored at 4°C. The color change of DG-PC was recorded after storage for 0, 1, 3, 5 and 7 days.

[0092] 6.1 pH

[0093] The chicken meat was cut with scissors, and 5.0 g of each sample was mixed with ultrapure water at a ratio of 1:10 (weight ratio) using a high-speed homogenizer, and then the pH value was measured at room temperature.

[0094] 6.2 Total Volatile Base Nitrogen (TVBN)

[0095] The chicken (5.0 g) in each sample was ground and stirred with ultrapure water (50 mL) for 30 min. Then, 5.0 mL of the supernatant obtained by centrifugation (8000 × g, 10 min, 4 ° C) was added to an equal volume of magnesium oxide suspension (10 g / L). The mixture was distilled using a semi-micro nitrogen fixation device. The distillate was then absorbed with 10 mL of H3BO3 solution containing methyl red (1 g / L) and bromocresol green (1 g / L). The absorption solution was then titrated with 0.01M HCl solution. The calculation formula for TVB-N (mg / 100g) is as follows:

[0096]

[0097] Wherein, X is the content of total volatile basic nitrogen in the sample (mg / 100g), V1 is the volume of standard hydrochloric acid solution consumed by the sample (mL), V2 is the volume of standard hydrochloric acid solution consumed by the blank control group (mL), C is the concentration of standard hydrochloric acid solution (mol / L), M is the mass of the sample (g), V is the volume of the filtrate (mL), and V0 is the total volume of the sample solution (mL).

[0098] 6.3 Total bacterial colony count (TVBN)

[0099] The mixture was treated and serially diluted 10-fold, and 50 μL of the dilutions were spread on plate count agar and incubated at 37°C for 48 h.

[0100] 7. Data Analysis

[0101] All experiments were repeated three times in parallel, and the results were expressed as mean ± standard deviation. One-way ANOVA and Duncan test were performed by software to calculate significant differences (P < 0.05, n = 3).

[0102] 2. Results and Discussion

[0103] 1. Analysis of the main components of PC

[0104] In the natural environment, free anthocyanins are not common and are usually combined with glucose, galactose, arabinose or rhamnose to form glycosides through glycosidic bonds. Table 1 lists the identification results of the main components of anthocyanins extracted from black peanut skins. Ten major substances were identified in the analysis, including six cyanidin derivatives, two pelargonidin derivatives and two peonyin derivatives: cyanidin-3-O-galactoside, cyanidin-3-O-xyloside, cyanidin-3-O-sophoroside, pelargonidin-3-O-sambubioside, peonyin-3-O-rutinoside, cyanidin-3-O-sambubioside-5-O-glucoside, pelargonidin-3-O-glucoside, cyanidin-3-O-(6-O-malonyl-β-D-glucoside), peonyin-3-O-glucoside, and cyanidin-3-O-sambubioside-glucoside. The changes in the number of substitutions on different rings, hydroxylation sites, methylation patterns and glycosylation sites lead to differences in the chemical structure and color of different anthocyanins. In general, anthocyanins show higher stability at lower temperatures and acidic conditions. In addition, under acidic conditions, the color development of anthocyanins is enhanced, and the color can be stabilized by complexation with metal ions. The structural composition of anthocyanins shows that they have both acidic and basic groups, which endows them with solubility in polar solvents such as water and methanol-ethanol. Therefore, the significant color development ability and water solubility of anthocyanins under different pH environments provide potential for the preparation of smart aerogel sensors for monitoring freshness.

[0105] Table 1 Analysis of the main components of PC in black peanut skin

[0106]

[0107]

[0108] 2. pH sensitivity of PC

[0109] In order to verify the sensitivity of PC to pH, the color changes of PC solution and DG-PC aerogel at different pH values ​​were measured, such as Figure 1 The UV-visible spectrum ( Figure 1 b) and the four main structural changes of anthocyanins ( Figure 1c). At pH 3.0, anthocyanins exist in the form of yellow salt cations (red) with an absorption peak at 520nm. From pH 3.0 to 6.0, the absorption peak intensity gradually weakens and the red color of the solution becomes lighter, which is due to the conversion of yellow salt cations into colorless quinone bases. At pH 7.0, the solution turns light purple, the yellow salt cations almost disappear, and the maximum absorption wavelength of anthocyanins red-shifts. At pH 8.0, the maximum absorption wavelength of the solution shifts to 580nm, and the absorption wavelength is enhanced due to the conversion of anthocyanins into blue quinone groups. From pH 9.0 to 10.0, no obvious characteristic peaks appear in the range of 450-700 nanometers, indicating that anthocyanins may have been degraded. This color change trend is consistent with previous studies. At pH 11.0-12.0, the solution turns yellow-green and the absorption peak at a wavelength of 600nm decreases, because the quinone structure of anthocyanins in a strong alkaline environment is unstable and chalcone is formed. Therefore, the pH sensitivity of PC can change the color from red to blue, purple and yellow-green, facilitating the real-time monitoring of food freshness.

[0110] 3. Material Characterization and Analysis

[0111] 3.1 FTIR analysis

[0112] The functional groups of CMC, DCMC, and GA and their combinations, as well as the possible PC interactions in DG aerogels were investigated by Fourier transform infrared spectroscopy ( Figure 2 For CMC( Figure 2 a), 3448.7cm -1 The broad absorption bands at 2927.9, 1627.9 and 1155.4 cm correspond to OH stretching vibrations. -1 The absorption bands at 1720.5 and 837.1 cm-1 are attributed to CH stretching vibration, OH bending vibration, and COC asymmetric stretching vibration, respectively. It is worth noting that the absorption bands at 1720.5 and 837.1 cm-1 are observed in the DCMC spectrum. -1 There are new absorption bands at , which are attributed to the carbonyl group and hemiacetal bond, respectively, indicating the formation of aldehyde group.

[0113] The spectrum of GA ( Figure 2 b) shows 3410.4cm -1 The absorption peak at (amide A), 1683.9 cm -1 The absorption peak at 1535.3 cm is attributed to C=O stretching vibration (amide I). -1 The absorption peak at 1244.1 cm is attributed to NH bending and CN coupling (amide II). -1The absorption peaks at 1683.9 cm-1 are attributed to CN stretching and NH bending (amide III). In the Fourier transform infrared spectrum of DG aerogel, both DCMC and GA retain prominent typical bands, but some peaks are shifted. For example, the hydrogen bonds formed between DCMC and GA cause the amide A band of DG aerogel to shift compared with GA. In addition, the GA peak at 1683.9 cm-1 after crosslinking is not significantly different from that at 1683.9 cm-1. -1 The peak at 1535.3 cm-1 was shifted to a lower wavelength, and the characteristic peak of the amide II band was shifted from 1535.3 cm-1 to 1535.3 cm-1. -1 The shift to higher wavelengths is attributed to the imide bands generated by the reaction of aldehyde groups with amino functional groups. In particular, DCMC has a peak at 1720.5 cm -1 The characteristic peak at disappeared because the CN stretching vibration of the Schiff base overlaps with the amide I band of GA. These results indicate that aldehyde depletion and Schiff base bond formation occur during the cross-linking process of DCMC and GA. In addition, compared with DG-5, the addition of PC leads to a decrease in the wave number and increase in the intensity of the amide A band. This may be due to the interaction of the hydroxyl groups of anthocyanins with the amino and hydroxyl groups in the hydrogel matrix through hydrogen bonds, which promotes the dispersion and stabilization of anthocyanins. This shows that the aerogel forms a stable network structure and good intermolecular physical composite ( Figure 2 c).

[0114] 3.2 XRD analysis

[0115] Figure 2 The XRD spectra shown in df analyzed the crystal structure of the prepared aerogel. Figure 2 In the d, the characteristic diffraction peaks of CMC appear at 2θ = 11.1° and 21.2°, which are attributed to the (110) and (200) crystal planes of cellulose type I crystals. However, in DCMC, the diffraction peak intensity at 2θ = 21.2° decreases and the diffraction peak intensity at 2θ = 11.1° disappears, indicating that the oxidation reaction destroys the crystal structure of cellulose. Figure 2 The e shows that GA has a peak at 2θ = 7.5° associated with the triple helical crystal structure and a broad amorphous peak at 2θ = 20.0°. In contrast, DG aerogels show diffraction peaks at 7.2°-7.8° and 19.9°-20.3°, indicating that the Schiff base reaction changes the crystal structure of the sample. In addition, the peak intensity of DG aerogels increases with the increase of DCMC concentration. Figure 2 f, PC does not affect the amorphous structure of the aerogel, which indicates that DG-PC has good biocompatibility, but compared with DG-5, its peak intensity first increases and then decreases, which confirms the existence of hydrogen bonds.

[0116] 3.3 Thermogravimetric analysis

[0117] The thermal stability and thermodynamic degradation behavior of the composite aerogels were analyzed using TGA and DTG curves. Figure 3 ).exist Figure 3 In a, DCMC has a lower degradation temperature than CMC due to oxidation destroying the ordered structure of highly crystalline cellulose. The initial weight loss (50-130°C) is attributed to water evaporation. The subsequent stage (160°C) marks the decomposition of DCMC. The critical third stage (250°C) indicates the cleavage of peptide bonds in GA. DTG curve ( Figure 3 b) shows that the DCMC peaks are at 220°C and 293°C, reflecting the dehydration of glucuronic acid and glucose units, respectively. Correspondingly, this feature is also evident in DG-10 and DG-20 due to residual DCMC. The weight loss in the fourth stage (360-500°C) indicates further degradation of the amino acid residues in the gel.

[0118] To further evaluate the thermal stability of the composite aerogels, the following table records the mass loss (T5 wt% 、T 20 wt% ) corresponding to the temperature and the maximum mass loss rate temperature (T max ) and the residual weight at 600℃ (W red ). Compared with GA, the T5 wt% 、T 20 wt% 、T max and W red This indicates that the covalent cross-linking of DCMC and GA improves thermal stability. This enhancement is due to the aldehyde groups of DCMC and the amine groups of GA, which are conducive to the formation of a cross-linked network and larger molecular chains. In addition, the T max Equivalent to DG-5, but W red higher, which indicates that PC does not impair the thermal properties of DG aerogels, which may be due to the lower PC addition or the destruction of the interaction at high temperature.

[0119] Table 2 Thermogravimetric analysis data of DCMC and all aerogels

[0120]

[0121] 3.4 SEM image analysis

[0122] Figure 4 The cross-sectional SEM images of DCMC, GA and aerogel are shown. Pure DCMC is disordered flakes ( Figure 4 a), while pure GA aerogel has a sheet-like structure ( Figure 4 b). In contrast, the DG composite aerogel showed a highly porous structure with an interconnected network ( Figure 4 The ci of the aerogels was ascribed to the enhanced three-dimensional continuous network structure due to cross-linking. Except for DG-2 and DG-PC1, the other aerogels had uniform shapes, multiple pores, and smooth pore walls. It is noteworthy that the DG-2 aerogel had the largest number of pores, and the increase in DCMC / PC content was associated with an increase in interlayer spacing and pore size.

[0123] Lower density and higher porosity are usually ideal conditions for developing colorimetric indicators. Table 3 lists the porosity, density, and pore size of aerogels. Figure 6 The ab shows the difference in porosity of each group of aerogels. Compared with GA (76.50% and 0.0369 g / cm 3 ), DG-2 aerogel exhibited similar porosity (73.37%) and density (0.0413 g / cm 3 With the increase of DCMC addition, the porosity of DG-5, DG-10 and DG-20 decreased significantly to 68.61%, 57.94% and 53.68% (P<0.05), and the density became 0.0396, 0.0401 and 0.0404 g / cm, respectively. 3 After cross-linking with DCMC, the pore size of GA aerogels decreased significantly from 382.51 μm to 61.75 μm (P < 0.05), indicating that the pores were more dense. However, excessive addition of DCMC resulted in an increase in pore size, which was confirmed by SEM images ( Figure 4 It is noteworthy that low concentration anthocyanin addition (DG-PC1) significantly reduced the pore size compared with DG-5 (P<0.05), while medium and high concentration additions resulted in larger and more uniform pores. This is because there are many free phenolic hydroxyl groups in PC, which can interact with the aerogel matrix through hydrogen bonding and electrostatic attraction.

[0124] Table 3 Porosity, density and pore diameter of GA, DG aerogel and DG-PC aerogel

[0125]

[0126] The values ​​in the table are the mean ± standard error of three replicates. Lowercase letters (af) indicate significant differences between different materials (P < 0.05).

[0127] 3.5 Mechanical properties analysis

[0128] In practical applications, the strong load-bearing capacity of aerogel can effectively protect indicator labels from damage caused by external pressure. Figure 5 The mechanical properties of GA and aerogel are shown. Stress-strain curves ( Figure 5Figure 1 ab) shows that the initial stress rises rapidly (about 10%), then slows down, and rises rapidly again after about 40% strain. This is because the high stress in the aerogel destroys the honeycomb structure and the tight network skeleton. Figure 5 As shown in the cd, the compressive stress of pure GA aerogel (247.09 kPa) increased significantly to varying degrees after adding 2% to 20% DCMC, reaching 258.96, 276.88, 258.14 and 270.15 kPa, respectively (P<0.05). Similar mechanical enhancements have been observed in previous studies, which are due to the covalent cross-linked network structure between DCMC and GA, which restricts the movement of gelatin molecular chains, thereby improving the deformation resistance of DG aerogels. It is worth noting that among all DG composite aerogels, DG-5 showed the highest compressive stress, which was attributed to its lower packing density and dense polymer domains. At the same time, compared with GA, DG-PC aerogels still exhibited higher compressive stress and superior mechanical properties (as shown in the table below). In addition, the stability of each aerogel immersed in ultrapure water at 25°C was tested, and the results showed that all aerogels were more stable than GA. After 24 hours, only GA showed obvious swelling and rupture ( Figure 6 c). Therefore, the comprehensive analysis results show that DG-5 has a uniform microstructure, lower density, higher porosity and stronger thermal stability, and is the most suitable modification scheme in this embodiment.

[0129] Table 4 Compressive stress of GA and DG aerogels

[0130]

[0131] 4. Chicken freshness detection effect

[0132] like Figure 7 As shown in Figure 2, DG-5 aerogels containing 0.50-2.00wt% PC were used to monitor the freshness of raw chicken. During the 7-day storage period, the quality of the chicken meat decreased significantly. In the smart tag, blue-purple indicates freshness and red indicates spoilage. On the first day at 4°C ( Figure 7a), all three groups of smart aerogel labels showed slight changes, indicating that they were beginning to deteriorate. At the end of the third day of storage, all groups of aerogel smart labels turned red, indicating that the chicken had deteriorated and was not suitable for consumption. Among them, when 1wt% of anthocyanin (DG-PC2) was added, the label showed obvious color changes in different buffer solutions. In the chicken freshness test, the material changed color significantly after one day of storage at 4°C (P<0.05), and the change on the third day was the most obvious, indicating that the chicken had deteriorated. The experimental results show that these color changes are perceptible to the naked eye and are significantly correlated with the physical and chemical indicators of chicken deterioration (P<0.05). Therefore, the colorimetric porous aerogel label of this embodiment can be applied to food intelligent packaging systems.

[0133] like Figure 7 As shown in Figure b, the pH value of chicken increased from 6.02 to 6.38 during storage and significantly increased to 6.14 after 3 days (P<0.05). This increase is attributed to the metabolism of nitrogenous compounds in food by microorganisms such as Acetobacter, converting them into alkaline substances. It is worth noting that the TVB-N value of chicken increased rapidly throughout the storage period (P<0.05), from 5.13 mg / 100 g to 29.87 mg / 100 g ( Figure 7 c), exceeding the national standard limit for fresh meat (25mg / 100g). This rise is attributed to microbial proliferation, decomposing sugar and protein nutrients, and producing biogenic amines and ammonia. By day 3, TVB-N exceeded the limit of 15mg / 100g, indicating that consumption is not recommended, which is consistent with the color change time on the smart aerogel label. In addition, according to Figure 7 On the 3rd day, the TVC of chicken meat increased significantly (P<0.05), reaching a peak of 7.60 lg CFU / g on the 7th day. It is worth noting that on the 3rd day, the TVC rose to 6.96 lg CFU / g, and it was considered deteriorated when it exceeded 6 lg CFU / g.

[0134] like Figure 7 As shown in the figure, the ΔE values ​​of the smart labels showed a trend of first increasing and then decreasing during the storage of chicken. It is worth noting that from the first day, the ΔE values ​​on all labels exceeded 4.00, indicating that the human eye can recognize obvious color changes, which is consistent with the Figure 7 In addition, from the third to the fifth day, DG-PC2 and DG-PC3 showed obvious changes in ΔE, indicating that they were more sensitive to changes in TVB-N levels. Considering Table 2 and Figure 4 , Figure 5 It can be seen from the bd that DG-PC2 has a more uniform microstructure, higher compressive stress and better thermal stability, and is therefore particularly suitable for chicken freshness monitoring. Figure 7The f shows a significant positive correlation between the total color difference of the three DG-PC aerogels and the pH, TVC, and TVBN levels of chicken. These results demonstrate the accuracy and feasibility of the developed aerogel smart responsive label for real-time monitoring of chicken freshness and highlight the potential of DG-PC aerogel labels for smart packaging of protein-rich foods.

[0135] Conclusion

[0136] In this embodiment, sodium aldehyde carboxymethyl cellulose and gelatin are cross-linked by Schiff base bonds to successfully prepare an aerogel with a porous polymer network structure, which has good structural properties, stronger thermal stability and higher mechanical strength. The DG-5 composite aerogel has the best effect, and the aerogel has a higher porosity and a smaller pore size. After adding anthocyanins, the aerogel of the present invention exhibits excellent color rendering at a pH value of 3-12. In addition, after adding 1.00% anthocyanins to the aerogel label (DG-PC2), it has broad application prospects in the monitoring of the freshness of meat food due to its higher compressive stress, thermal stability and responsiveness to total volatile base nitrogen (TVB-N).

[0137] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An aerogel for freshness monitoring, characterized in that: The invention comprises a porous polymer network structure formed by anthocyanin composition, sodium aldehyde carboxymethyl cellulose and gelatin.

2. The aerogel for freshness monitoring according to claim 1, characterized in that: The mass ratio of the sodium aldehyde carboxymethyl cellulose, gelatin and anthocyanin composition is (2-15): (20-300):

1.

3. The aerogel for freshness monitoring according to claim 1, characterized in that: The porosity of the aerogel is 50%-80% and the density is 0.03-0.05 g / cm 3 , the pore diameter is 150-500μm.

4. The method for preparing aerogel for freshness monitoring according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) preparing sodium aldehyde carboxymethyl cellulose; (2) extracting anthocyanin composition; (3) dissolving the sodium aldehyde carboxymethyl cellulose and gelatin in an aqueous medium, stirring, mixing with the anthocyanin composition, and freeze-drying to obtain the aerogel; Preferably, the freeze-drying step further comprises a step of standing at 20-30°C for 1-3 hours.

5. The method for preparing aerogel for freshness monitoring according to claim 4, characterized in that: The aldehyde carboxymethyl cellulose sodium is prepared by reacting carboxymethyl cellulose sodium and sodium periodate solution.

6. The method for preparing aerogel for freshness monitoring according to claim 4, characterized in that: The stirring includes stirring at 30-50° C. for 2-6 hours.

7. The method for preparing aerogel for freshness monitoring according to claim 4, characterized in that: The freeze drying comprises drying at -70°C to -90°C for 30-60h.

8. Use of the aerogel for freshness monitoring according to any one of claims 1 to 3 in preparing smart food packaging materials.

9. A smart food packaging material, characterized in that: It comprises the aerogel for freshness monitoring according to any one of claims 1 to 3.

10. A method for monitoring the freshness of meat products, characterized in that: It comprises the step of using the aerogel according to any one of claims 1-3.

Citation Information

Cited By

  • Reversible response type MOF confinement colorimetric sensing patch and preparation method thereof

    CN122306787A