Preparation method of biomass pyrolytic carbon for ironmaking
Through the methods of soaking, solid-liquid separation and pyrolysis carbonization, the problems of high energy consumption of biomass carbon and difficulty in removing alkali metals are solved, and biomass pyrolysis carbon with high calorie value and low alkalinity are prepared, realizing the replacement of blast furnace fuel and the effective utilization of resources reduces production costs and carbon emissions.
Patent Information
- Application Number
- CN202411098129.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-12-03
AI Technical Summary
When using biomass to prepare iron-smelting fuel, the prior art has problems such as high energy consumption, difficulty in effectively removing alkali metal content, complicated process steps and waste of energy, resulting in the quality of biomass carbon not meeting the standards and cannot effectively replace traditional fossil fuels.
The biomass is pretreated by dipping, solid-liquid separation and pyrolysis carbonization. The alkali metal elements are removed by stirring and dipping, and the alkali metal content is reduced, and the alkali metal content is pyrolysis carbonization is carried out in a high-temperature vertical furnace to generate high calorific value. Low alkalinity, low ash biomass pyrolysis carbon.
The high-quality preparation of biomass pyrolytic carbon is achieved, which can partially replace traditional fossil fuels in blast furnaces, reduce carbon emissions, reduce production costs, and use the circulating process water for fertilizer use, with high resource utilization.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of iron and steel metallurgy and biomass energy resource utilization, and specifically relates to a method for preparing biomass pyrolytic carbon for iron making. Background Art
[0002] The steel industry is the cornerstone of modern industry, and its importance is self-evident. It provides key materials for many fields and supports infrastructure construction, manufacturing development, etc. However, the steel production process consumes a lot of energy and emits pollutants. Energy conservation and emission reduction are particularly necessary at this moment. This will not only help ease the energy shortage and reduce damage to the environment, but also promote the sustainable development of the steel industry. By adopting advanced technologies and management methods, reducing dependence on traditional energy such as coal, optimizing the energy structure, reducing energy waste and pollutant emissions, and actively practicing the concept of energy conservation and emission reduction, the steel industry can continue to play an important role in the future while coexisting harmoniously with the ecological environment.
[0003] As a renewable carbon-neutral carbon source, biomass can be used in blast furnace ironmaking to effectively reduce carbon emissions from blast furnaces and reduce dependence on traditional fossil energy. However, biomass has low fixed carbon content and capacity density, and is relatively tough. In particular, agricultural straw, which is rich in resources in my country, including corn straw, has excessive alkali metal content due to the addition of potassium fertilizer during its growth, and cannot be directly used in blast furnace ironmaking. Therefore, the biomass must be pretreated before it can be used in blast furnace ironmaking.
[0004] CN110358599A discloses a method for dealkalization carbonization of agricultural and forestry wastes based on hydrothermal reaction. By controlling the raw materials and reaction conditions of the hydrothermal reaction, agricultural and forestry wastes with low calorific value and high alkali metal content with low utilization value are converted into high-quality hydrothermal carbon with high calorific value and low alkali metal content. However, the carbonization reaction requires a high temperature and high pressure environment, with high energy consumption, and the composition of the generated hydrothermal carbon is close to that of lignite, and the quality cannot reach the bituminous coal and anthracite currently used in blast furnaces; CN117778074A discloses a method and system for preparing biomass fuel for metallurgy. The biomass fuel prepared by drying, pyrolysis, washing, digestion, distillation, pelletizing and carbonization has the characteristics of low volatile matter (<10wt%), low combustion rate, low alkali metal, high energy density and high strength. However, the method is relatively complicated, and washing after drying and pyrolysis will cause a certain degree of energy waste, and the tar generated after pyrolysis will have a certain impact on the subsequent washing to remove alkali metals, and the biomass alkali metal effect is not ideal.
[0005] In addition, for different types of biomass, due to the difference in raw materials, the processing methods and process sequences will have a great impact on the quality of the finished product. The present invention is aimed at typical agricultural and forestry waste biomass with relatively abundant resources in my country, and proposes a method for preparing high-quality biomass charcoal fuel, which improves the quality of biomass by removing alkali metal elements from biomass through soaking, solid-liquid separation, and pyrolysis and carbonization of biomass. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing biomass pyrolytic carbon for ironmaking. The biomass pyrolytic carbon is prepared by soaking, solid-liquid separation, and pyrolysis and carbonization of biomass. The prepared biomass pyrolytic carbon has the characteristics of high calorific value, high energy density, low alkalinity and low ash content, and can be used to partially replace traditional fossil fuels in blast furnace ironmaking, greatly reducing the demand for fossil fuels in blast furnace ironmaking.
[0007] To achieve the above object, the present invention adopts the following technical solutions: A method for preparing biomass pyrolytic carbon for ironmaking, comprising the following steps: (1) Cut the biomass into pieces of 1-50 mm in length, put them into a blender, add a certain amount of water, and perform a stirring and soaking treatment; (2) separating the washed biomass into solid and liquid; (3) The biomass obtained by solid-liquid separation is subjected to pyrolysis and carbonization to obtain.
[0008] Furthermore, the biomass in step (1) of the present invention includes one or a mixture of agricultural straw, wheat straw, waste wood, municipal garden prunings.
[0009] Furthermore, the stirring and immersion time in step (1) of the present invention is 1-8 hours.
[0010] Furthermore, the water in step (1) of the present invention is pure water.
[0011] Furthermore, in step (1) of the present invention, the ratio of biomass to water added is m:v in the range of 5g-10g:1L.
[0012] Furthermore, in step (2) of the present invention, the mixing ratio of process water to pure water is 1:10-10:1.
[0013] Furthermore, the process water filtered out by solid-liquid separation in step (2) of the present invention can be mixed with pure water in a certain proportion and used as water for washing the biomass in step (1).
[0014] Furthermore, the mixing ratio of the process water and the pure water in the present invention is 1:10-10:1.
[0015] Furthermore, the process water in step (2) of the present invention is circulated 2-10 times. After a certain number of cycles, the content of alkali metal elements in the solution becomes high, and it is not suitable for continued use as a solution for leaching, and can be discharged as fertilizer for irrigating farmland.
[0016] Furthermore, the specific operation of the pyrolysis carbonization in step (3) of the present invention is: placing the washed and filtered biomass into a high-temperature vertical furnace, pyrolyzing it at a temperature of 400-800° C. for 0.5-3 h in an oxygen-free environment, and the obtained solid is biomass pyrolysis carbon.
[0017] Furthermore, the biomass pyrolysis charcoal in step (3) of the present invention has a dry basis fixed carbon content greater than 55%, a dry basis ash content less than 4.5%, a dry basis volatile matter less than 42%, a dry basis carbon content greater than 65%, a dry basis hydrogen content greater than 3.00%, and a dry basis higher calorific value greater than 25 MJ / kg.
[0018] Furthermore, the K content in the biomass pyrolysis charcoal in step (3) of the present invention is 0.05-0.40%, and the Na content is 0.01-0.03%.
[0019] The inventive principle of the present invention is: The method of the present invention has a better effect in removing alkali metals. The principle is that K and Na, which are relatively high in biochar, are soluble alkali metal elements, and most of them can be removed by leaching. Moreover, studies have shown that the effect of leaching is significantly better than that of ordinary leaching, because biomass has a porous structure, and alkali metals such as K and Na are easily soluble in water. Therefore, after leaching, the alkali metal content in biomass is greatly reduced. If pyrolysis is performed and then washed with water, K, Na, and Zn will be enriched after pyrolysis treatment, which is due to the inert atmosphere of the reaction environment. Biomass itself cannot effectively remove ash. As the temperature increases, its volatile matter is removed and condensed into tar, which adheres to the pores on the surface of the biomass, further hindering the removal of ash, resulting in unsatisfactory removal of alkali metals by subsequent leaching.
[0020] The beneficial technical effects of the technical solution of the present invention are: (1) Using waste biomass as raw material to prepare high-quality ironmaking fuel, biomass is a carbon-neutral fuel. When used in blast furnace ironmaking, it can reduce carbon dioxide emissions and at the same time, waste biomass can be used as a resource.
[0021] (2) The water generated during the biomass soaking process can be mixed with pure water and recycled in the subsequent soaking process, thus reducing costs.
[0022] (3) After a certain number of cycles, the process water is rich in potassium and sodium, which can be used as fertilizer for farmland irrigation without causing waste of resources.
[0023] (4) By soaking the biomass before pyrolysis, the drying step can be omitted. It has been verified that the water after soaking has evaporated completely in the early stage of pyrolysis, which will not have a significant impact on the pyrolysis effect. In addition, soaking before pyrolysis can remove the alkali metal content such as K and Na in the biomass to the greatest extent.
[0024] (4) The present invention has a simple process, is easy to operate, and has low energy consumption and production costs. It is an excellent method for producing high-quality biomass fuel for blast furnace ironmaking. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below in conjunction with the embodiments, so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more explicit definition of the protection scope of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention. Example 1
[0026] In this embodiment, corn stalks are used to prepare ironmaking fuel, and the preparation method is as follows: (1) Cut 20 g corn stalks into 1-10 mm segments and place them in a magnetic stirrer. Add 4 L of pure water and start magnetic stirring to soak for 3 h.
[0027] (2) After the soaking is completed, the solid-liquid mixture is poured into a suction filter for filtration. The process water obtained by filtration can be mixed with pure water and used for subsequent biomass soaking.
[0028] (3) The washed and filtered biomass was placed in a high-temperature vertical pyrolysis furnace for pyrolysis carbonization. The high-temperature vertical furnace was heated to 600°C at a heating rate of 10°C / min and kept warm for 3 h. Inert gas was introduced throughout the process for protection. The biomass was then cooled to room temperature to obtain corn straw pyrolysis carbon.
[0029] The corn straw pyrolysis carbon prepared in this embodiment was subjected to component analysis, calorific value and alkali metal content detection. The test results show that the corn straw pyrolysis carbon prepared in this embodiment has a fixed carbon content of 78.60% on a dry basis, an ash content of 2.02% on a dry basis, a volatile content of 24.38% on a dry basis, a carbon content of 75.36% on a dry basis, a hydrogen content of 3.78% on a dry basis, a nitrogen content of 1.03% on a dry basis, a sulfur content of 0.03% on a dry basis, an oxygen content of 17.78% on a dry basis, a high calorific value of 28.87 MJ / kg on a dry basis, a K content of 0.38%, and a Na content of 0.03%; it can partially replace pulverized coal for injection in blast furnace ironmaking. Example 2
[0030] In this embodiment, wheat straw is used to prepare ironmaking fuel, and the preparation method is as follows: (1) Cut 30 g of wheat straw into 40-50 mm segments and place them in a magnetic stirrer. Pour 5 L of pure water into the magnetic stirrer and turn on the magnetic stirring to soak for 4 h.
[0031] (2) After the soaking is completed, the solid-liquid mixture is poured into a suction filter for filtration. The process water obtained by filtration can be mixed with pure water for subsequent biomass soaking.
[0032] (3) The washed and filtered biomass was placed in a high-temperature vertical pyrolysis furnace for pyrolysis carbonization. The high-temperature vertical furnace was heated to 400°C at a heating rate of 10°C / min and kept warm for 2 h. Inert gas was introduced throughout the process for protection. The biomass was then cooled to room temperature to obtain wheat straw pyrolysis carbon.
[0033] The wheat straw pyrolysis carbon prepared in this embodiment was subjected to component analysis, calorific value and alkali metal content detection. The test results show that the wheat straw pyrolysis carbon prepared in this embodiment has a fixed carbon content of 55.31% on a dry basis, an ash content of 2.89% on a dry basis, a volatile content of 41.80% on a dry basis, a carbon content of 65.43% on a dry basis, a hydrogen content of 4.97% on a dry basis, a nitrogen content of 0.97% on a dry basis, a sulfur content of 0.02% on a dry basis, an oxygen content of 25.72% on a dry basis, a high calorific value of 25.96 MJ / kg on a dry basis, a K content of 0.30%, and a Na content of 0.02%; it can partially replace pulverized coal for injection in blast furnace ironmaking. Example 3
[0034] In this embodiment, wheat straw is used to prepare ironmaking fuel, and the preparation method is as follows: (1) Cut 30 g of wheat straw into 20-30 mm segments and place them in a magnetic stirrer. Mix 2 L of once-circulated process water and 3 L of pure water and pour them into the magnetic stirrer. Turn on the magnetic stirring and soak for 4 h.
[0035] (2) After the soaking is completed, the solid-liquid mixture is poured into a suction filter for filtration. The process water obtained by filtration can be mixed with pure water for subsequent biomass soaking.
[0036] (3) The washed and filtered biomass was placed in a high-temperature vertical pyrolysis furnace for pyrolysis carbonization. The high-temperature vertical furnace was heated to 800°C at a rate of 10°C / min and kept warm for 1 h. Inert gas was introduced throughout the process for protection. The biomass was then cooled to room temperature to obtain wheat straw pyrolysis carbon.
[0037] The wheat straw pyrolysis carbon prepared in this embodiment was subjected to component analysis, calorific value and alkali metal content detection. The test results show that the wheat straw pyrolysis carbon prepared in this embodiment has a fixed carbon content of 79.31% on a dry basis, an ash content of 4.39% on a dry basis, a volatile content of 16.30% on a dry basis, a carbon content of 81.62% on a dry basis, a hydrogen content of 3.83% on a dry basis, a nitrogen content of 1.05% on a dry basis, a sulfur content of 0.02% on a dry basis, an oxygen content of 9.09% on a dry basis, a high calorific value of 31.96 MJ / kg on a dry basis, a K content of 0.40%, and a Na content of 0.03%; it can partially replace pulverized coal for injection in blast furnace ironmaking. Example 4
[0038] In this embodiment, municipal garden prunings are used to prepare ironmaking fuel, and the preparation method is as follows: (1) Cut 50 g of municipal garden prunings into small pieces of 2-10 mm and put them into a container. Add 7 L of pure water and turn on the magnetic stirrer to stir and soak for 6 h.
[0039] (2) After immersion and washing, filter.
[0040] (3) The washed and filtered biomass was placed in a high-temperature vertical furnace for pyrolysis and carbonization. The high-temperature vertical furnace was heated to 800°C at a heating rate of 10°C / min and kept warm for 30 min. Inert gas was introduced throughout the process for protection. The biomass was then cooled to room temperature with the furnace to obtain municipal garden pruning material pyrolysis carbon.
[0041] The composition analysis, calorific value and alkali metal content of the municipal garden pruning pyrolytic carbon prepared in this embodiment were tested. The test results show that the fixed carbon content of the municipal garden pruning pyrolytic carbon prepared in this embodiment is 83.21% on a dry basis, the ash content is 1.79% on a dry basis, and the volatile content is 15.00% on a dry basis. The dry basis carbon content is 85.43%, the dry basis hydrogen content is 3.97%, the dry basis nitrogen content is 1.03%, the dry basis sulfur content is 0.02%, the dry basis oxygen content is 7.76%, the dry basis high calorific value is 33.65MJ / kg, the K content is 0.17%, and the Na content is 0.02%; it can partially replace coal powder for injection in blast furnace ironmaking. Example 5
[0042] In this embodiment, waste wood is used to prepare ironmaking fuel, and the preparation method is as follows: (1) 4 L of deionized water was mixed with 1 L of process water after three immersion cycles, and then added to a magnetic stirrer. 50 g of waste wood with a length of 8-10 mm was added thereto for stirring and immersion for 8 h.
[0043] (2) After the immersion is completed, filter.
[0044] (3) The washed and filtered biomass is placed in a high-temperature vertical furnace for pyrolysis and carbonization. The high-temperature vertical furnace is heated to 700°C at a heating rate of 10°C / min and kept warm for 1 hour. Inert gas is introduced throughout the process for protection. The biomass is then cooled to room temperature to obtain waste wood pyrolysis charcoal.
[0045] The waste wood pyrolysis charcoal prepared in this embodiment was subjected to component analysis, calorific value and alkali metal content testing. The test results show that the waste wood pyrolysis charcoal prepared in this embodiment has a fixed carbon content of 81.31% on a dry basis, an ash content of 1.65% on a dry basis, and a volatile content of 17.04% on a dry basis. The dry basis carbon content is 84.45%, the dry basis hydrogen content is 3.00%, the dry basis nitrogen content is 1.05%, the dry basis sulfur content is 0.02%, the dry basis oxygen content is 9.84%, the dry basis high calorific value is 31.94 MJ / kg, the K content is 0.05%, and the Na content is 0.01%.
[0046] The waste wood pyrolysis charcoal prepared in this embodiment can partially replace coal powder for injection in blast furnace ironmaking; it can be used as blast furnace injection fuel, sintering fuel, coking raw material and carbon-containing pellet reducing agent, etc.
[0047] The above description is only an illustrative embodiment of the present invention and is not any formal or substantial limitation of the present invention. It should be pointed out that a number of improvements and supplements made by ordinary technicians in this technical field without departing from the method of the present invention should also be regarded as the protection scope of the present invention; at the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention still fall within the protection scope of the present invention.
Claims
1. A method for preparing biomass pyrolytic carbon for ironmaking, characterized in that: The method comprises the following steps: (1) Cut the biomass into pieces of 1-50 mm in length, put them into a blender, add a certain amount of water, and perform a stirring and soaking treatment; (2) separating the washed biomass into solid and liquid; (3) The biomass obtained by solid-liquid separation is subjected to pyrolysis carbonization to obtain biomass pyrolysis charcoal.
2. The method for preparing biomass pyrolytic carbon for ironmaking according to claim 1, characterized in that: The biomass in step (1) includes one or a mixture of agricultural straw, wheat straw, waste wood, municipal garden prunings.
3. The method for preparing biomass pyrolytic carbon for ironmaking according to claim 1, characterized in that: The stirring and immersion time in step (1) is 1-8 hours.
4. The method for preparing biomass pyrolytic carbon for ironmaking according to claim 1, characterized in that: The water in step (1) is pure water.
5. The method for preparing biomass pyrolytic carbon for ironmaking according to claim 1, characterized in that: The addition ratio of biomass to water in step (1) is m:v 5g-10g:1L.
6. The method for preparing biomass pyrolytic carbon for ironmaking according to claim 1, characterized in that: The process water filtered out during the solid-liquid separation in step (2) can be mixed with pure water in a certain proportion and used as water for washing the biomass in step (1).
7. The method for preparing biomass pyrolytic carbon for ironmaking according to claim 6, characterized in that: The mixing ratio of the process water to the pure water is 1:10-10:
1.
8. The method for preparing biomass pyrolytic carbon for ironmaking according to claim 1, characterized in that: The specific operation of the pyrolysis carbonization in step (3) is: putting the washed and filtered biomass into a high-temperature vertical furnace, pyrolyzing it at a temperature of 400-800°C for 0.5-3h in an oxygen-free environment, and the obtained solid is biomass pyrolysis carbon.
9. The method for preparing biomass pyrolytic carbon for ironmaking according to claim 1, characterized in that: The biomass pyrolysis charcoal in step (3) has a dry basis fixed carbon content greater than 55%, a dry basis ash content less than 4.5%, a dry basis volatile matter less than 42%, a dry basis carbon content greater than 65%, a dry basis hydrogen content greater than 3.00%, and a dry basis higher calorific value greater than 25 MJ / kg.
10. The method for preparing biomass pyrolytic carbon for ironmaking according to claim 1, characterized in that: The K content in the biomass pyrolysis charcoal in step (3) is 0.05-0.40%, and the Na content is 0.01-0.03%.