Production method of low-roughness cold-rolled strip steel for electrotinning
By designing reasonable plate and strip composition and process flow in the production of electroplating tin substrates and combining with rolls with special roughness, the problem of insufficient surface roughness control of electroplating tin substrates is solved, and the surface quality and performance after electroplating is improved. Meets T2.5/T3 material requirements.
Patent Information
- Application Number
- CN202411245003.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-06
Smart Images

Figure CN119061324A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrotin-plating sheet material processing technology, in particular to a production method of low-roughness cold-rolled strip steel for electrotin-plating. Background Art
[0002] The electroplating tin market has had a steady development trend in recent years. The application fields of electroplating tin plates are very wide, including food, beverages, medicines, paints, cosmetics and other industries. They all show the advantages of being able to keep fresh for a long time, not easy to be polluted, easy to circulate, low cost, and easy to recycle. Electroplating tin has high requirements for the surface flatness of the substrate. Substrates with poor flatness are prone to welding problems. Therefore, the flatness of the substrate must be strictly controlled during the manufacturing process. Among the mechanical properties of tin-plated substrates, hardness and elongation are more important. In the production process, the mechanical properties are ensured to meet the requirements through composition control, rolling process, annealing process, and flattening process adjustment. The surface roughness of the tin-plated substrate is particularly important for the surface quality after electroplating. Therefore, if you want to get a better surface quality after electroplating, the substrate roughness must be kept at a low level.
[0003] After searching, a tinplate and its manufacturing method disclosed in Chinese patent number CN202211264096.3 are designed with low-carbon aluminum-killed steel composition. Without increasing the alloy content and the difficulty of production control, the contents of elements such as C, Mn, Al, and N in the tinplate are designed, and the corresponding hot rolling, cold rolling, annealing, and flattening processes are matched. The strengthening effect of conventional elements carbon and manganese is fully utilized, combined with the control of hot-rolled aluminum nitride precipitation, and the appropriate cold rolling reduction rate is selected. The ferrite grain size and cementite precipitation in the steel are controlled through continuous annealing and over-aging treatment, and a specific flattening process is matched to produce tinplate with small strength and hardness fluctuations, high elongation, and short yield platform. At the same time, the amount of alloy tin is reasonably controlled to meet the requirements of aerosol can top cover for stamping formability, pressure resistance and surface gloss. The tinplate has a simple composition, a simple and easy process, and a low production cost. Patent No. CN200610026315.9 discloses a cold-rolled tinplate for easy-open ends and a production method thereof, which mainly solves the technical problems of cracking and low yield strength of the existing cold-rolled tinplate for easy-open ends during the stamping process of manufacturing the easy-open ends. The production method adopts hot metal desulfurization, converter top and bottom composite blowing, ladle bottom argon blowing or LF furnace refining, full-process Ar blowing protection casting, plate bad heating furnace heating, descaling, rough rolling, finishing rolling, coiling to obtain hot-rolled steel coils, and then re-uncoiling, pickling, cold rolling, vertical continuous annealing furnace annealing, electrotin plating, coiling to obtain finished products, the finishing rolling temperature is 820-850°C, the hot rolling coiling temperature is 630-660°C, the cold rolling reduction rate is 85%-90%, the temperature range of the hardened strip after cold rolling in the soaking section of the vertical continuous annealing furnace is 570-590°C, and the soaking time of the strip in the vertical continuous annealing furnace is 30-45s, and it is mainly used for making easy-to-open covers. Patent No. CN201410125206.7 discloses a cold-rolled tinplate for beverage can bottom covers and a production method thereof, which mainly solves the technical problems of cracking and poor performance stability of the existing cold-rolled tinplate for beverage can bottom covers during the stamping process of manufacturing beverage can bottom covers. The production method is smelting according to the components, and sequentially adopts molten iron desulfurization, converter top and bottom composite blowing, ladle bottom argon blowing or LF furnace refining, full-process Ar blowing protection casting, slab heating furnace heating, rough rolling, finishing rolling, coiling to obtain hot-rolled steel coils, and then re-uncoiling, pickling, cold rolling, vertical continuous annealing furnace annealing, electrotin plating, coiling to obtain finished products with a thickness of 0.17-0.20mm, the finishing rolling temperature is 851-879℃, the hot rolling coiling temperature is 640-660℃, the cold rolling reduction rate is 70%-79%, the temperature range of the hardened strip after cold rolling in the soaking section of the vertical continuous annealing furnace is 560-580℃, and the soaking time of the strip in the vertical continuous annealing furnace is 95-105s, and it is mainly used for making beverage can bottom covers.
[0004] It can be seen that the existing patents are all about the full-process production process of electrogalvanized sheets and the improvement of individual defects, and the control details of the surface roughness of electrotinned substrates are not involved. Summary of the invention
[0005] The purpose of the present invention is to provide a method for producing low-roughness cold-rolled strip steel for electrotin plating. By designing a reasonable strip composition and appropriate hot rolling, acid rolling and continuous annealing processes, an electrotin-plated substrate that meets the mechanical property requirements is obtained. At the same time, by using a roller with a special roughness surface, a lower surface roughness is obtained after flattening, so that the surface quality after electrotin plating is better, thereby solving the shortcomings of the prior art.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for producing a low-roughness cold-rolled strip steel for electroplating tin, comprising the following chemical components in mass percentage ratio: C: 0.03-0.055wt%, Si: ≤0.050wt%, Mn: 0.15-0.25wt%, Al: 0.030-0.055%, P≤0.020%, S≤0.015%, N≤0.006wt%, the balance being Fe and other inevitable impurities, and the specific production process is as follows:
[0008] Step 1: Smelting and continuous casting: LF furnace is used for slag deoxidation and desulfurization, and molten steel that meets the temperature, composition and cleanliness requirements is provided for continuous casting within a certain period of time; continuous casting is used to produce ingots, and the molten steel is formed and rapidly solidified and crystallized under the action of the crystallizer to form a slab;
[0009] Step 2: hot continuous rolling of cast slabs: austenite rolling is performed on the continuously cast slabs to obtain hot rolled coils;
[0010] Step 3: Pickling and cold rolling: Use conventional pickling process to fully remove the iron oxide scale on the surface of the strip, and then cold roll it to the required thickness specification of the finished product;
[0011] Step 4: Strip cleaning: remove impurities adhering to the surface of the strip after cold rolling, including rolling oil and iron powder;
[0012] Step 5: Continuous annealing: The cleaned steel plate is continuously annealed, the steel plate is heated to the recrystallization temperature, and after recovery, recrystallization, and grain growth processes, the annealing temperature is controlled to be 730-750°C;
[0013] Step 6: Over-aging treatment: Cool the steel plate after high-temperature continuous annealing to about 380±20℃ and keep it warm for 200-300 seconds;
[0014] Step 7: Leveling: Use a 6-roller leveler for wet leveling to improve the plate shape and eliminate the slip bands caused by dislocation deformation caused by solid solution C and N atoms.
[0015] Furthermore, during the hot rolling process in step 2, the heating temperature is controlled at 1180-1220° C., the final rolling temperature is controlled at 860-900° C., the coiling temperature is controlled at 660-690° C., and the hot rolling convexity is controlled at 0.015-0.035 mm.
[0016] Furthermore, in step 3, the cold rolling reduction rate is controlled at 80%-88%, the rolling tonnage is 500-1000 tons, the working roll roughness target of the S5 stand is 2.5 μm, the S5 stand reduction rate is ≤3%, and the working rolls of the S5 stand are chrome-plated.
[0017] Furthermore, in step 6, the strip processing speed is 100-200 m / min, the temperature in the rapid cooling section is 390-410° C., the strip temperature in the aging section is 360-400° C., and the aging time is 200-300 s.
[0018] Furthermore, in step 7, the rolling force of the leveling mill is controlled at 4500-5500 kN, and the leveling elongation does not exceed 1.4%.
[0019] Furthermore, the roller diameter of the leveling machine is 460-480 mm, the surface roughness of the roller is 0.8-1.0 μm, the rolling tonnage of the leveling machine is 200-800 tons, the roller diameter difference between the upper and lower rollers of the leveling machine is controlled within 50 μm, and the roller shifting amount of the middle roller of the leveling machine is set to +20 mm.
[0020] Furthermore, the leveling elongation control parameters of the leveling machine include: Leveling machine inlet / outlet tension requirements: Leveling machine inlet tension target value (kN) = strip thickness (mm) × strip width (mm) × 0.08 (kN / mm 2 ), the target value of the tension at the leveling machine outlet (kN) = strip thickness (mm) × strip width (mm) × 0.09 (kN / mm 2 ); The height difference between the inlet anti-wrinkle roller and the outlet anti-trembling roller of the leveling machine is maintained at 50mm, the outlet anti-trembling roller is higher than the inlet anti-wrinkle roller, and the surface roughness Ra of the inlet anti-wrinkle roller and the outlet anti-trembling roller is controlled at 0.8-1.6μm.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The production method of low-roughness cold-rolled strip steel for electrotin plating of the present invention obtains an electrotin-plated substrate that meets the mechanical property requirements by designing reasonable strip composition and appropriate hot rolling, acid rolling and continuous annealing processes. At the same time, by using rollers with special roughness surfaces, a lower surface roughness is obtained after leveling, so that the surface quality after electrotin plating is better, the plate shape is good, and the performance meets the T2.5 / T3 material requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a production process flow chart of the present invention. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] In an embodiment of the present invention, a method for producing a low-roughness cold-rolled strip steel for electroplating tin is provided, comprising the following chemical components in mass percentage ratio: C: 0.03-0.055wt%, Si: ≤0.050wt%, Mn: 0.15-0.25wt%, Al: 0.030-0.055%, P≤0.020%, S≤0.015%, N≤0.006wt%, and the balance is Fe and other inevitable impurities; wherein the specific principle of determining the chemical composition is as follows:
[0026] C: is the most effective strengthening element and also the most economical strengthening element. When the C content is low, its formability and welding performance are better, but a low C content will lead to low mechanical properties and hardness of the product, while an excessively high C content will lead to a significant decrease in its formability and elongation. Therefore, the C content in the present invention is controlled at 0.03-0.055wt%.
[0027] Si: has a strong strengthening effect in steel, but Si is easily enriched and oxidized on the surface, which is not conducive to the surface quality of the product after pickling and annealing, and also reduces the coating and plating properties of the steel plate. Therefore, the present invention adds a small amount of Si or no Si is added, which is controlled below 0.05wt%.
[0028] Mn: It plays a role of solid solution strengthening in steel, which can increase the strength and hardness of the material. At the same time, it reacts with S in steel to reduce the hot brittleness of the steel. However, too high Mn content will increase the cost of raw materials. Therefore, in the present invention, Mn mainly improves the strength and hardness of the material and reduces the hot brittleness. Its content is controlled in the range of 0.15-0.25%.
[0029] Al: It mainly plays a deoxidizing role in steel. At the same time, Al can also form AlN precipitation, fix the N element, improve the aging of the material, and play a certain role in refining the grains. A small amount of Al can improve the material performance, but if the Al content is too high, the crystallizer is easily blocked, the castability deteriorates, and the cost is increased. Therefore, the weight percentage of Al in the present invention is controlled at 0.030%-0.055%.
[0030] P: is easy to segregate, reducing the formability and plasticity of the material, and has adverse effects on the stamping performance, cold brittleness, secondary processing brittleness, etc. of the steel. In the present invention, the P content is controlled to be below 0.020wt%.
[0031] N: mainly causes yield effect and strain aging, and is a harmful impurity. Therefore, the upper limit of N content is strictly controlled. In the present invention, N is controlled below 0.006wt%.
[0032] S: is an inevitable harmful impurity in steel, which has an adverse effect on the isotropy, hot brittleness, stamping performance, cold bending performance, flanging forming performance, etc. of the steel. Strictly controlling the S content in the steel will increase the smelting cost of the steel. Therefore, in the present invention, the upper limit of the S content is controlled at 0.015%.
[0033] The balance is Fe and unavoidable impurity elements. The less impurity elements there are, the better without increasing additional costs.
[0034] like Figure 1 As shown, based on the ratio of the above chemical components, the production process of the present invention includes: smelting → continuous casting → hot rolling → pickling and cold rolling → cleaning → continuous annealing → flattening → finished product, which is specifically as follows:
[0035] Step 1: Smelting and continuous casting: LF furnace is used for slag deoxidation and desulfurization, and molten steel that meets the temperature, composition and cleanliness requirements is provided for continuous casting within a certain period of time; continuous casting is used to produce ingots, and the molten steel is formed and rapidly solidified and crystallized under the action of the crystallizer to form a slab;
[0036] Step 2: Hot rolling of ingot: austenite rolling is performed on the continuous casting ingot to obtain hot rolled coils; during the hot rolling process, a relatively low temperature is used for rolling. A higher heating temperature will cause an increase in scale oxide, coarsening of grains, and dissolution of AlN, which will increase the solid solution N. Therefore, the heating temperature is controlled at 1180-1220°C; to avoid rolling in the two-phase zone, the final rolling temperature is controlled at 860-900°C; to ensure that the performance of the steel plate meets the requirements, low-temperature coiling is adopted, and too low a temperature is not conducive to the precipitation of solid solution N. The coiling temperature is controlled at 660-690°C. A smaller convexity can obtain a smaller difference with the same plate, but a too small convexity is difficult to control in hot rolling, which may easily lead to an excessively large wedge shape. Therefore, the hot rolling convexity is controlled at 0.015-0.035mm;
[0037] Step 3: Pickling and cold rolling: conventional pickling process is adopted to fully remove the iron oxide scale on the surface of the strip, and then cold rolling is carried out to the required thickness specification of the finished product. In order to obtain finer grains and ensure certain mechanical properties, a higher reduction rate is required, but too high a reduction rate will cause instability in the production process, and the yield platform will be extended after recovery and recrystallization, which is not conducive to stamping. The cold rolling reduction rate is controlled at 80%-88%. In order to ensure the surface roughness range of the finished product, the production of electroplated tin substrates has special requirements for the acid rolling tonnage, the roughness of the working roll of the S5 stand and the reduction rate. The rolling tonnage is required to be 500-1000 tons, the roughness target of the working roll of the S5 stand is 2.5μm, and the reduction rate of the S5 stand is required to be ≤3%. In order to ensure that the decay rate of the plate surface roughness is low, the working roll of the S5 stand must be chrome-plated;
[0038] Step 4: Strip cleaning: remove impurities adhering to the surface of the strip after cold rolling, such as rolling oil and iron powder, to improve the cleanliness of the strip surface and obtain better surface quality;
[0039] Step 5: Continuous annealing: Continuous annealing of the cleaned steel plate is a key process for controlling the structure and performance of the steel plate. The steel plate is heated to the recrystallization temperature, and after recovery, recrystallization, grain growth and other processes, a structure with a certain grain size and appropriate performance is obtained. Too high annealing temperature will lead to coarse material structure and obvious orange peel on the surface after stamping, so the annealing temperature is controlled to 730-750℃;
[0040] Step 6: Over-aging treatment: After the continuous annealing steel plate is rapidly cooled, a large amount of supersaturated carbon remains, which is not conducive to stamping. After rapid cooling, an over-aging process is used to promote the precipitation of a large number of C atoms. The over-aging treatment is to cool the steel plate that has undergone high-temperature continuous annealing to about 380±20°C and then keep it warm for 200-300 seconds. Since rapid cooling increases the precipitation power of carbon, maintaining heating can promote the precipitation of carbon, thereby ensuring that the product has good stamping and anti-aging performance. Therefore, the strip speed of the present invention is 100-200m / min, the temperature of the rapid cooling section is 390-410°C, the strip temperature of the aging section is 360-400°C, and the aging time is 200-300s;
[0041] Step 7: Leveling: The leveling process uses 6-roll wet leveling, which mainly improves the plate shape, eliminates the slip band (yield platform) caused by the deformation of dislocation caused by the solid solution C and N atoms, avoids tensile strain marks in the later processing, adjusts the mechanical properties of the material after annealing, and transfers different surface structures and roughness of the strip. Using a larger rolling force is beneficial to eliminating the yield platform and reducing the yield elongation, but too much rolling force is not conducive to the control of strip shape and roughness, so the rolling force of the leveler is controlled at 4500-5500kN; for low-carbon aluminum-killed steel, as the leveling elongation increases, the yield strength of the steel plate first decreases and then increases. The leveling elongation reaches about 1.0%-1.2%, which can eliminate the yield platform of 0.25-0.35mm thick annealed steel plate. At the same time, the yield strength reaches the lowest point. Continuing to increase the leveling elongation can lead to dislocation strengthening in the organization, increase the yield strength and hardness of the steel plate, reduce processing performance, and increase the load of the leveler. Reduced operating stability, therefore, the leveling elongation of thin-gauge products should not exceed 1.4%.
[0042] In the above embodiment, in order to ensure that the surface quality of the plate meets the requirements after tin plating, the roughness of the base material must be low enough, so the leveling process adopts smooth roller rolling, and the resulting plate and strip has a roughness of less than 0.6μm. In order to reduce the rolling force of the leveling machine and achieve smooth rolling, a 6-roller leveling machine is used to further reduce the diameter of the working roller. The roller diameter is required to be 460-480mm during production. The working roller adopts a ground surface and is not roughened. The surface roughness of the roller is controlled to be in the range of 0.8-1.0μm. In order to control the roughness range of the plate surface, the rolling tonnage of the leveling machine is required to be 200-800 tons. The plate shape of the electroplated tinned substrate is required to be relatively high. To ensure that no warping occurs, the difference in roller diameters between the upper and lower rollers of the leveling machine must be controlled within 50μm. In order to improve the plate shape control ability of the leveling machine and reduce harmful contact, the middle roller of the leveling machine must be shifted, and the shifting amount is set to +20mm.
[0043] In order to avoid the surface twill defects of the 6-roller leveler under large elongation, it is necessary to specially control the leveler entrance / exit tension and the leveler entrance anti-wrinkle roller / exit anti-vibration roller. The leveler entrance / exit tension requirements are as follows: Leveler entrance tension target value (kN) = strip thickness (mm) × strip width (mm) × 0.08 (kN / mm 2 ), the target value of the tension at the leveling machine outlet (kN) = strip thickness (mm) × strip width (mm) × 0.09 (kN / mm 2 ); For example: when producing 0.3mm thick and 1000mm wide strip steel, the target value of the tension at the leveling mill entrance is set to 0.3mm×1000mm×0.08kN / mm 2 That is 24kN, the target value of the tension at the exit of the leveling machine is set to 0.3mm×1000mm×0.09kN / mm 2That is 27kN, the height difference between the inlet anti-wrinkle roller / exit anti-trembling roller of the leveling machine is maintained at 50mm, the exit anti-trembling roller is higher than the inlet anti-wrinkle roller, and the surface roughness Ra of the inlet anti-wrinkle roller / exit anti-trembling roller needs to be controlled in the range of 0.8-1.6μm.
[0044] In order to further better explain the embodiment of the present invention, based on the above method, the following specific fact case parameters are also provided for illustration:
[0045] Steelmaking and continuous casting: The molten steel is smelted in a converter, refined by HR or LF, and then continuously cast into slabs. The chemical composition of the slabs is shown in Table 1:
[0046] Table 1 Chemical composition / %
[0047] Serial number C Si Mn P S Als N Example 1 0.043 0.005 0.180 0.014 0.012 0.031 0.0017 Example 2 0.044 0.020 0.190 0.014 0.006 0.051 0.0018 Example 3 0.048 0.019 0.174 0.015 0.008 0.045 0.0018 Example 4 0.044 0.021 0.185 0.010 0.004 0.043 0.0024 Comparative Example 1 0.040 0.016 0.222 0.014 0.006 0.050 0.0022 Comparative Example 2 0.043 0.007 0.202 0.012 0.009 0.051 0.0022 Comparative Example 3 0.054 0.004 0.199 0.017 0.017 0.034 0.0024 Comparative Example 4 0.056 0.017 0.183 0.009 0.006 0.044 0.0018
[0048] Hot rolling of cast slab: The continuous casting slab is heated, rough rolled, finished rolled, laminar cooled and rolled to obtain a hot rolled steel coil with a thickness of 2 mm. The specific hot rolling process parameters are shown in Table 2:
[0049] Table 2 Hot rolling process
[0050]
[0051] Pickling and cold rolling: The hot rolled steel coil is sequentially uncoiled, pickled, trimmed, cold rolled, and rolled to obtain a cold hardened coil with a thickness of 0.25-0.35 mm. The specific hot rolling process parameters are shown in Table 3.
[0052] Table 3 Pickling reduction control
[0053] Serial number Hot coil thickness / mm Thickness of hard rolled coil / mm Reduction rate / % Example 1 2 0.25 0.875 Example 2 2 0.35 0.825 Example 3 2 0.35 0.825 Example 4 2 0.25 0.875 Comparative Example 1 2.8 0.5 0.821 Comparative Example 2 3.2 0.7 0.781 Comparative Example 3 5 1.5 0.700 Comparative Example 4 5 1.8 0.640
[0054] Continuous annealing and leveling: The cold-hardened coil is sequentially subjected to uncoiling, degreasing and cleaning, annealing, leveling, trimming, and coiling to obtain the cold-rolled annealed steel coil. The specific process parameters are shown in Tables 4 and 5.
[0055] Table 4 Continuous Annealing Process
[0056]
[0057] Table 5 Leveling process
[0058]
[0059] The actual performance is shown in Table 6:
[0060] Table 6 Performance
[0061]
[0062] As can be seen from the examples, using appropriate hot rolling and annealing processes can produce cold-rolled strip with good performance, meeting T2.5 / T3 requirements. Using low-roughness work roll rolling, as well as appropriate tension, rolling force and roll stringing, can produce cold-rolled strip with low surface roughness and good plate shape, which meets the requirements according to customer trial feedback.
[0063] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for producing low-roughness cold-rolled steel strip for electroplating tin, characterized in that: The chemical composition includes the following mass percentage ratio: C: 0.03-0.055wt%, Si: ≤0.050wt%, Mn: 0.15-0.25wt%, Al: 0.030-0.055%, P≤0.020%, S≤0.015%, N≤0.006wt%, and the balance is Fe and other inevitable impurities. The specific production process is as follows: Step 1: Smelting and continuous casting: LF furnace is used for slag deoxidation and desulfurization, and molten steel that meets the temperature, composition and cleanliness requirements is provided for the continuous casting process within a certain period of time; continuous casting is used to produce ingots, and the molten steel is formed and rapidly solidified and crystallized under the action of the crystallizer to form a slab; Step 2: hot continuous rolling of cast slabs: austenite rolling is performed on the continuously cast slabs to obtain hot rolled coils; Step 3: Pickling and cold rolling: Use conventional pickling process to fully remove the iron oxide scale on the surface of the strip, and then cold roll it to the required thickness specification of the finished product; Step 4: Strip cleaning: remove impurities adhering to the surface of the strip after cold rolling, including rolling oil and iron powder; Step 5: Continuous annealing: The cleaned steel plate is continuously annealed, the steel plate is heated to the recrystallization temperature, and after recovery, recrystallization, and grain growth processes, the annealing temperature is controlled to be 730-750°C; Step 6: Over-aging treatment: Cool the steel plate after high-temperature continuous annealing to about 380±20℃ and keep it warm for 200-300 seconds; Step 7: Leveling: Use a 6-roller leveler for wet leveling to improve the plate shape and eliminate the slip bands caused by dislocation deformation caused by solid solution C and N atoms.
2. The method for producing a low-roughness cold-rolled steel strip for electrotinning according to claim 1, characterized in that: During the hot rolling process in step 2, the heating temperature is controlled at 1180-1220° C., the final rolling temperature is controlled at 860-900° C., the coiling temperature is controlled at 660-690° C., and the hot rolling convexity is controlled at 0.015-0.035 mm.
3. The method for producing a low-roughness cold-rolled steel strip for electrotinning according to claim 1, characterized in that: In step 3, the cold rolling reduction rate is controlled at 80%-88%, the rolling tonnage is 500-1000 tons, the working roll roughness target of the S5 stand is 2.5 μm, the S5 stand reduction rate is ≤3%, and the working roll of the S5 stand is chrome-plated.
4. The method for producing a low-roughness cold-rolled steel strip for electrotinning according to claim 1, characterized in that: In step 6, the strip processing speed is 100-200 m / min, the temperature in the rapid cooling section is 390-410°C, the strip temperature in the aging section is 360-400°C, and the aging time is 200-300s.
5. The method for producing a low-roughness cold-rolled steel strip for electrotinning according to claim 1, characterized in that: In step 7, the rolling force of the leveling mill is controlled at 4500-5500 kN, and the leveling elongation does not exceed 1.4%.
6. The method for producing a low-roughness cold-rolled steel strip for electro-tinning according to claim 5, characterized in that: The roller diameter of the leveling machine is 460-480mm, the surface roughness of the roller is 0.8-1.0μm, the rolling tonnage of the leveling machine is 200-800 tons, the roller diameter difference between the upper and lower rollers of the leveling machine is controlled within 50μm, and the roller shifting amount of the middle roller of the leveling machine is set to +20mm.
7. The method for producing a low-roughness cold-rolled steel strip for electrotinning according to any one of claim 5, characterized in that: The leveling elongation control parameters of the leveling machine include: Leveling machine inlet / outlet tension requirements: Leveling machine inlet tension target value (kN) = strip thickness (mm) × strip width (mm) × 0.08 (kN / mm 2 ), the target value of the tension at the leveling machine outlet (kN) = strip thickness (mm) × strip width (mm) × 0.09 (kN / mm 2 ); The height difference between the inlet anti-wrinkle roller and the outlet anti-trembling roller of the leveling machine is maintained at 50mm, the outlet anti-trembling roller is higher than the inlet anti-wrinkle roller, and the surface roughness Ra of the inlet anti-wrinkle roller and the outlet anti-trembling roller is controlled at 0.8-1.6μm.
Citation Information
Patent Citations
Production method for tinned plate cold-rolled substrate
CN112126854A
High-hardness cold-rolled electrotinning substrate and production method thereof
CN114250410A
Tin-plated plate and manufacturing method thereof
CN115341155A
Cold-rolled electroplated tin steel plate for deep drawing cover and manufacturing method of cold-rolled electroplated tin steel plate
CN116770166A
Manufacture of al killed cold rolled steel sheet excellent in surface property by continuous annealing
JP1992247826A