Three-dimensional flower-shaped silicon-zinc selenide / cobalt selenide-carbon composite material and preparation method thereof, lithium ion battery silicon-based negative electrode and battery

A three-dimensional flower-shaped silicon@zinc selenide/cobalt selenide@carbon composite material addresses the stability and conductivity issues of silicon-based electrodes, offering high capacity and stable cycle performance.

CN119069705AActive Publication Date: 2024-12-03DAYAN SILICON ONE (ZHEJIANG) TECHNOLOGY DEVELOPMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411113659.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Traditional lithium-ion battery negative electrode materials like graphite have limited capacity and silicon-based materials suffer from poor cycle stability, volume expansion, and low conductivity, hindering their commercial use.

Method used

A three-dimensional flower-shaped silicon@zinc selenide/cobalt selenide@carbon composite material is synthesized using low-cost raw materials, with a method involving the preparation of Si@Zn(OH)2/Co(OH)2, followed by carbonization and calcination with selenium powder, forming a composite with a novel structure that alleviates volume expansion and improves conductivity.

Benefits of technology

The composite material exhibits high reversible capacity, stable cycle performance, and robust rate performance, addressing the limitations of traditional silicon-based electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069705A_ABST
    Figure CN119069705A_ABST
Patent Text Reader

Abstract

The invention provides a three-dimensional flower-shaped silicon-zinc selenide / cobalt selenide-carbon composite material and a preparation method thereof, a lithium ion battery silicon-based negative electrode and a battery, and compared with the prior art, silicon particles are firstly prepared and grow in nano flower sheets, then carbon coating is performed on the nano flower sheets, and then the nano flower sheets are put into a tube furnace to be converted into a Si-ZnSe / CoSe-C composite material by utilizing selenium powder. The flower-shaped structure not only can increase a large amount of surface active sites, but also can effectively relieve volume expansion of silicon particles, so that the cycle stability of the battery is improved, and the battery obtains extremely high specific capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicon negative electrode materials for lithium ion batteries, and specifically relates to a three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material and a preparation method thereof, a lithium ion battery silicon-based negative electrode and a battery. Background Art

[0002] In the fast-developing contemporary society, due to the depletion of fossil fuels such as coal, oil, and natural gas, and their combustion will also bring a series of environmental problems, clean energy such as solar energy, wind energy, hydropower, nuclear energy, and new electric energy has been unprecedentedly developed. Lithium-ion batteries have received extensive attention due to their long cycle life, high operating voltage, high energy density, and green environmental protection. However, traditional lithium-ion battery negative electrode materials such as graphite have limited their development due to their low theoretical capacity. Silicon has become one of the most promising negative electrode materials for lithium-ion batteries due to its extremely high capacity, but due to the large volume change during the lithiation process, silicon is easy to powderize, has poor cycle stability, and volume expansion during charging and discharging, poor conductivity, and short cycle life limit its commercial use.

[0003] The patent with the publication number CN 105070894 A published on November 18, 2015 discloses a porous silicon-based composite negative electrode material for lithium-ion batteries, a preparation method and use thereof, and discloses that the negative electrode material is a capsule structure, the capsule core is amorphous porous silicon, and the capsule wall is a conductive carbon material; the particle size of the amorphous porous silicon is 10 to 300 nm, the pore size of the amorphous porous silicon is 0.5 to 100 nm; the thickness of the capsule wall is 0.5 to 10 μm. The preparation method of the porous silicon-based composite negative electrode material for lithium-ion batteries provided by the patent is complicated and not suitable for industrial promotion. Summary of the invention

[0004] The purpose of the present invention is to provide a three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material and a preparation method thereof, wherein Si@Zn(OH)2 / Co(OH)2 is prepared using low-cost raw materials, then carbonized and calcined with selenium powder to obtain the composite material Si@ZnSe / CoSe@C. The product has a novel structure, high yield and low cost. The preparation method is simple and suitable for industrial promotion.

[0005] Another object of the present invention is to provide a lithium-ion battery silicon-based negative electrode, which is prepared using the above three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material, to improve the technical problems of poor cycle stability and easy volume expansion of silicon-based materials as electrode materials.

[0006] The last object of the present invention is to provide a battery prepared using the above-mentioned lithium-ion battery silicon-based negative electrode, which has high reversible capacity, high specific capacity, stable cycle performance and robust rate performance.

[0007] The specific technical solutions of the present invention are as follows:

[0008] A method for preparing a three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material comprises the following steps:

[0009] 1) Dispersing silicon material in a solvent to form a uniform solution, recorded as solution A; mixing cobalt salt, zinc salt and urea in water, stirring evenly, recorded as solution B; after mixing solution A and solution B evenly, reacting in a water bath to obtain flower-shaped Si@Zn(OH)2 / Co(OH)2;

[0010] 2) dispersing the Si@Zn(OH)2 / Co(OH)2 obtained in step 1) in water, adding tris(hydroxymethyl)aminomethane, adjusting the pH to 8-9 with hydrochloric acid, and then adding dopamine hydrochloride, stirring to react;

[0011] 3) calcining the product of step 2) and selenium powder to obtain a three-dimensional flower-like Si@ZnSe / CoSe@C composite material.

[0012] In step 1), the silicon material is dispersed in a solvent, and the amount ratio of the silicon material to the solvent is 0.05 to 0.3 mol / L, preferably 0.1 mol / L;

[0013] In step 1), the silicon material is silicon particles; the size of the silicon particles is 10-60nm; preferably 30nm;

[0014] In step 1), the solvent is anhydrous ethanol; silicon is very difficult to disperse, so the present invention can be evenly dispersed in ethanol alone, and each silicon ball can be evenly grown in the flower piece; directly adding silicon will make the silicon dispersed unevenly, so the present invention needs to first disperse the silicon material in a solvent to prepare solution A.

[0015] In step 1), the mass ratio of the cobalt salt, the zinc salt and the urea is 2.5:1.3:1.3 to 6.54:3.6:3.6;

[0016] In step 1), in solution B, the concentration of the cobalt salt in deionized water is 0.8 to 1.5 mol·L -1 , preferably 1.1 mol·L -1 ;

[0017] In step 1), the cobalt salt is cobalt nitrate hexahydrate;

[0018] In step 1), the concentration of the zinc salt in deionized water is 0.3-0.8 mol·L -1 , preferably 0.56 mol·L -1 ;

[0019] In step 1), the zinc salt is zinc nitrate hexahydrate;

[0020] In step 1), the concentration of urea in deionized water is 2.0 to 4.0 mol·L -1 , preferably 2.8 mol·L -1 ;

[0021] In step 1), the volume ratio of the solvent to deionized water is 32:15;

[0022] In step 1), the water bath reaction is carried out at 60-100° C. for 30 minutes to 2 hours; preferably at 90° C. for 1 hour.

[0023] In step 1), after the reaction is completed, the flower-shaped Si@Zn(OH)2 / Co(OH)2 is obtained by centrifugation, washing and drying;

[0024] In step 2), the mass ratio of Si@Zn(OH)2 / Co(OH)2, tris(hydroxymethyl)aminomethane and dopamine hydrochloride is 1:3:0.175 to 1:6:0.3; preferably, the mass ratio is 1:3:0.175; and the pH is adjusted to 8 to 9 with hydrochloric acid, preferably to 8.5;

[0025] In step 2), the ratio of Si@Zn(OH)2 / Co(OH)2 to deionized water is 0.003-0.005 g / mL; preferably 0.004 g / mL;

[0026] The stirring reaction in step 2) is carried out at room temperature for 20-30 hours, preferably 24 hours;

[0027] In step 2), after the reaction is completed, the product is collected by centrifugation, washing, and drying;

[0028] Step 2) preparing Si@Co(OH)2 / Zn(OH)2@PDA;

[0029] In step 3), the mass ratio of the product of step 2) to selenium powder is 1:3 to 1:8; the preferred mass ratio is 1:5; the calcination conditions are 500 to 700°C for 1 to 4 hours, and the preferred reaction conditions are 560°C for 2 hours; the calcination atmosphere is hydrogen-argon gas, which is a reducing gas and has a volume fraction of 5% hydrogen and 95% argon.

[0030] The silicon particles of the present invention grow in nano flower sheets, which are then coated with carbon and subsequently placed in a tubular furnace to be converted into a composite material of Si@ZnSe / CoSe@C using selenium powder. The flower-like structure can not only increase a large number of surface active sites but also effectively alleviate the volume expansion of silicon particles, thereby improving the cycle stability of the battery. Because the previously synthesized Zn(OH)2 / Co(OH)2 is a flower-like structure, directly adding silicon particles during the synthesis process can allow the silicon spheres to participate in the process of synthesizing nanomaterials, so that the silicon spheres grow well in the petals, so that finally a flower-like material containing silicon spheres is formed. The flower-like structure is conducive to alleviating the volume expansion of silicon, and it has a large specific surface area, thereby providing more reactive sites, which can enable the battery to obtain an extremely high specific capacity.

[0031] In the present invention, because the volume of silicon is very small, it is evenly distributed in the flowers assembled by the nanosheets, and silicon has a large specific surface area and high surface activity, these characteristics enable silicon particles to grow in the sheets of the flower. The reason why the flower-like structure is composed of sheets is that the process of self-assembly of nanoflowers to form a flower-like structure is relatively simple and easy to control. The process of self-assembly of nanosheets to form a flower-like structure involves the interaction of physical and chemical forces, which include van der Waals forces, hydrogen bonds, electrostatic effects, etc. These forces enable the nanosheets to spontaneously gather together to form a stable flower-like structure. In addition, the surface energy of the nanosheets is relatively high, which means that they have a strong tendency to gather together to reduce the surface energy, which is also a driving force for the self-assembly of the sheets into flowers. The present invention is a three-dimensional structure because the product has a three-dimensional flower-like structure.

[0032] The present invention provides a three-dimensional flower-shaped silicon @ zinc selenide / cobalt selenide @ carbon composite material, which is prepared by the above method and has the following morphology: the size of the three-dimensional flower-shaped silicon @ zinc selenide / cobalt selenide @ carbon composite material is between 10-15um, Si particles are born in ZnSe / CoSe petals, and the outermost layer is a carbon layer; the particle size of the Si particles is 30±5nm, and the thickness of the nanosheet is 100±20nm. The synthesized material has a flower-like structure composed of intersecting sheets. The interlaced 'petals' produce a large number of irregular and layered pores, and there are large openings and gradient channels in the particles, so this is a special porous structure.

[0033] Due to the problems of easy expansion, poor cycle stability and weak conductivity of silicon particles, its development potential is seriously limited. In order to solve this problem, the inventors found through a large number of experimental explorations that Si is embedded in porous materials to accommodate its volume expansion through the void space in the porous framework. For this method, the three-dimensional porous nanostructure also achieves rapid ion transport by increasing the surface area in contact with the electrolyte. Therefore, the present invention composites ZnSe / CoSe with silicon particles. ZnSe and CoSe are both important members of transition metal selenides, have good conductivity and high theoretical capacity, and are considered to be excellent negative electrode materials for lithium-ion batteries. Therefore, bimetallic selenide has become the preferred material. And its assembly and compounding with silicon can make the composite material have good electrical conductivity. It can not only buffer the volume expansion of silicon, but also improve the dispersibility of silicon due to its high ductility, and can greatly improve the cycle life of silicon.

[0034] Although the composite materials of selenium, cobalt and zinc have the above advantages, there are also many difficulties that need to be overcome, such as large volume expansion during the charge and discharge process, which will cause the electrode material to break and pulverize, lose the connection with the current collector, and cause the capacity to decay rapidly, as well as difficulties such as silicon volume expansion. Therefore, the present invention adopts the porosity of the material to increase the specific surface area of ​​the material as much as possible, reduce the loss of active materials, and thus alleviate the capacity decay. At the same time, silicon is a material with extremely stable composition, and there will be no changes in the components during high-temperature selenization. Based on the above, the composite material synthesized by the present invention has the advantage of being porous. When designing the experiment, the present invention selects metal selenides with a flower-like structure, and silicon can grow in the petals of the petals, which not only maintains the advantage of the large specific surface area of ​​the nanomaterial, but also alleviates the volume expansion of the silicon particles.

[0035] The present invention provides a lithium-ion battery silicon-based negative electrode, which is prepared using the three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material.

[0036] The present invention provides a lithium-ion battery, which is prepared using the above-mentioned lithium-ion battery silicon-based negative electrode. Specifically, a three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material is used as an active material, mixed with conductive carbon black and PVDF in a mass ratio of 7:2:1, and then NMP is added dropwise, and magnetic stirring is performed for 6 to 8 hours to evenly disperse it therein, and the mixed slurry is applied on a copper foil using an applicator, and placed in a vacuum drying oven at 60 to 80°C, and after drying for 12 to 24 hours, it is pressed using a tablet press, and then cut into a small circular electrode sheet using a sheet cutter; the prepared electrode sheet is assembled into a button battery in a glove box filled with high-purity argon gas and the water oxygen value is ≤0.01ppm; the electrolyte is ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) in a volume ratio of 2:6:2 as a solvent, and the solute is LiPF6. The purity of the lithium sheet is Li ≥ 99.99%, the thickness is 0.5 mm, and it is cut into the size of the electrode sheet after rolling.

[0037] Add 1 drop of electrolyte on the positive electrode shell of the battery and place the electrode sheet, then add 1 drop of electrolyte and place the diaphragm, add 2 drops of electrolyte on the diaphragm and place the lithium sheet as the counter electrode, then put in two pieces of foamed nickel, add 1 drop of electrolyte, cover the negative electrode shell, press and seal the battery with a hydraulic press, and leave it for 6 to 12 hours.

[0038] Battery mechanism of the present invention:

[0039] The cyclic voltammetry curve of Si@ZnSe / CoSe@C anode is shown in Fig.25 During the first cathodic scan, three reduction peaks were observed at 1.70, 1.31, and 0.73 V. The weak peak at 1.70 V can be attributed to Li + Initial insertion in Si@ZnSe / CoSe@C electrode; the peak at 1.31 V may be due to Li + The intercalation reaction in Co formed LixZn(Co)Se and formed a solid electrolyte interface (SEI) film on the anode surface; at the same time, another cathode peak at 0.73 V may be due to the interaction between LixZn(Co)Se and Li +The concomitant transformation reactions between LixZn and Li2Se form Co, Zn, and Li2Se. The cathodic peak at 0.21 V is associated with the reduction of Si to LixSi alloy. In the second cycle, the reduction peak shifts to 1.41 V and a broad peak at 0.91 V, and the shift in peak position may be caused by the irreversible side reactions and activation process caused by the initial lithium insertion during the first cycle. The two high-resolution anodic peaks at 0.35 and 0.52 V match the transformation of LixSi alloy to amorphous Si. The oxidation peak at 1.36 V can be attributed to the multi-step dealloying reaction of the LixZn alloy phase and the oxidation of LiZn to ZnSe, while the oxidation peak at 2.09 V can be attributed to the reversible selenization of Co to CoSe (Co+Li2Se / LixCoSe / CoSe). Correspondingly, during the anodic scan, several small peaks in the potential range of 0.01-0.7 V are attributed to the reverse reaction between metallic Co, Zn, and Li2Se to form LixZn(Co)Se. Subsequent scans showed a constant CV curve, indicating that the conversion process of Si@ZnSe / CoSe@C is highly reversible and stable. The reaction equation of Si@ZnSe / CoSe@C is as follows:

[0040] Reduction peak

[0041] CoSe+xLi + →LixCoSe(1.31V)

[0042] LixZn(Co)Se+Li + →Co+Zn+Li2Se(0.73V)

[0043] Si+Li + →LixSi(0.35V,0.52V)

[0044] Oxidation peak

[0045] Co+Li2Se→LixCoSe→CoSe(2.09V)

[0046] LixZn→xLi + +Zn(1.36V)

[0047] Co+Zn+Li2Se→LixZn(Co)Se(0.01-0.7V)

[0048] LixSi→Si+Li + (0.21V).

[0049] In the preparation method based on the three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material provided by the present invention, cobalt salt, zinc salt and urea are used as raw materials, deionized water is used as solvent, and silicon particles are reacted in a water bath to synthesize Si@Zn(OH)2 / Co(OH)2; ethanol is selected as solvent for silicon, and the role of ethanol is to better disperse and dissolve silicon particles. Cobalt salt, zinc salt and urea select deionized water as solvent, and water plays the role of dissolving and dispersing. The present invention uses selenium powder as a selenizing agent, calcining and selenizing to generate a special three-dimensional flower-shaped Si@ZnSe / CoSe@C composite material. Its special structural material provides more active sites during the charge and discharge process, solves the problem of volume expansion, and makes the battery have better stability. In addition, the nanomaterial has the advantages of safety, environmental protection, and low price.

[0050] Compared with the prior art, the present invention has the following advantages: (1) The application of the prepared Si@ZnSe / CoSe@C composite material in lithium-ion batteries is very novel and is the first combined application; (2) The prepared composite material can well maintain the three-dimensional flower-like structure, can provide a large specific surface area, and can well inhibit the volume expansion of silicon; (3) The prepared composite material has stable performance, is not easy to denature in the air, and is easy to store; (4) The prepared composite material is used as a negative electrode material for lithium-ion batteries, and has a large specific capacity and good cycle performance; (5) The carbon matrix shortens the path of electrons / ions and reduces the strain of volume change. The Si@ZnSe / CoSe@C composite material prepared by the present invention has a good performance of 1Ag -1 After 650 cycles at the current density of 298.13 mAh g -1 The high reversible capacity, high specific capacity, stable cycling performance, and robust rate capability indicate that Si@ZnSe / CoSe@C is an excellent and promising lithium-ion anode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is the SEM image of the precursor Si@Zn(OH)2 / Co(OH)2 prepared in Example 1;

[0052] Figure 2 This is the SEM image of Si@ZnSe / CoSe@C prepared in Example 1;

[0053] Figure 3 TEM image of the three-dimensional flower-like structure Si@ZnSe / CoSe@C prepared in Example 1.

[0054] Figure 4 XRD pattern of the three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 1;

[0055] Figure 5XRD pattern of the precursor Si@Zn(OH)2 / Co(OH)2 prepared in Example 1;

[0056] Figure 6 This is the SEM image of Si@Zn(OH)2 / Co(OH)2 prepared in Example 2;

[0057] Figure 7 This is the SEM image of Si@ZnSe / CoSe@C prepared in Example 2;

[0058] Figure 8 TEM image of the three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 2;

[0059] Fig. 9 This is the SEM image of the three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 3;

[0060] Fig.10 This is the SEM image of the three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 4;

[0061] Fig.11 TEM of the three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 4;

[0062] Fig.12 This is the SEM image of the three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 5;

[0063] Fig.13 TEM image of the three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 5;

[0064] Fig.14 The three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 1 is used as a negative electrode material for lithium-ion batteries at 0.5Ag -1 The charge and discharge curve test diagram under current density;

[0065] Fig.15 The three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 1 is used as a negative electrode material for lithium-ion batteries at 0.5Ag -1 Cyclic performance test diagram under current density;

[0066] Fig.16 The three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 1 was used as a negative electrode material for lithium-ion batteries at 1.0Ag -1 Cyclic performance test diagram under current density;

[0067] Fig.17The three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 1 is used as a negative electrode material for lithium-ion batteries and is tested for cycle performance at different current densities;

[0068] Fig.18 is a graph showing the specific surface area of ​​the composite material synthesized in Example 1;

[0069] Fig.19 The pure silicon granular material of Example 6 is used as the negative electrode material of lithium ion battery at 0.1Ag -1 Cyclic performance test diagram under current density;

[0070] Fig. 20 The ZnSe material synthesized in Example 7 is used as a negative electrode material for lithium-ion batteries at 0.5Ag -1 Cyclic performance test diagram under current density;

[0071] Fig.21 The ZnSe material synthesized in Example 7 is used as a negative electrode material for lithium-ion batteries at 1.0Ag -1 Cyclic performance test diagram under current density;

[0072] Fig. 22 The CoSe material synthesized in Example 8 is used as a negative electrode material for lithium-ion batteries at 0.5Ag -1 Cyclic performance test diagram under current density;

[0073] Fig.23 The CoSe material synthesized in Example 8 is used as a negative electrode material for lithium-ion batteries at 1.0Ag -1 Cyclic performance test diagram under current density;

[0074] Fig.24 XRD pattern of the comparative material prepared in Example 9;

[0075] Fig.25 CV graph of the three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 1 as a negative electrode material for lithium-ion batteries;

[0076] Fig.26 This is the Raman image of the three-dimensional flower-like structure Si@ZnSe / CoSe@C material prepared in Example 1. DETAILED DESCRIPTION

[0077] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0078] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0079] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0080] Example 1

[0081] A method for preparing a three-dimensional flower-shaped Si@ZnSe / CoSe@C composite material comprises the following steps:

[0082] 1) Preparation of precursor Si@Zn(OH)2 / Co(OH)2:

[0083] Take 0.1g of 30nm silicon particle powder and ultrasonically disperse it in a 50mL beaker containing 32mL of anhydrous ethanol to form a uniform solution, which is recorded as solution A; weigh 4.9g Co(NO3)2·6H2O, 2.5g Zn(NO3)2·6H2O and 2.5g urea and add them to a 100mL beaker containing 15mL of deionized water, stir to form a uniform solution, and record it as solution B. Pour solution A into solution B and stir magnetically for 10min to mix it thoroughly. Then transfer it to a water bath and react at 90℃ for 1h. Cool it naturally to room temperature, wash it with deionized water by centrifugation 4 times, wash it with ethanol twice, and vacuum dry it at 60℃ for 12h, and collect the precursor Si@Zn(OH)2 / Co(OH)2 precipitate product. Its SEM picture is as follows Figure 1 As shown, it can be seen from the figure that it is a micro-nano flower of 10-15μm.

[0084] 2) Preparation of Si@ZnSe / CoSe@C:

[0085] 0.2 g Si@Zn(OH)2 / Co(OH)2 obtained in step 1) was dispersed in 50 mL of deionized water, 0.611 g of tris(hydroxymethyl)aminomethane was added to the solution, and after ultrasonication for 10 min, the pH was adjusted to 8.5 with 36% hydrochloric acid, 35 mg of dopamine hydrochloride was added, and the mixture was stirred at room temperature for 24 hours. After the reaction was completed, the product was obtained by centrifugation, washing, and drying;

[0086] 3) The obtained product was then mixed with selenium powder in a mass ratio of 1:5 and placed in two porcelain boats, and calcined in a hydrogen and argon flowing atmosphere at a heating rate of 2°C / min to a calcination temperature of 560°C for 2 hours. The calcination atmosphere was hydrogen and argon gas with a volume fraction of 5% hydrogen and 95% argon, and finally the product Si@ZnSe / CoSe@C was obtained, and its SEM image is shown as follows Figure 2 As shown in the figure, it can be seen that it is a flower-like structure. Figure 3 As shown in the figure, Si particles grow in the petals. The petals are composed of ZnSe / CoSe, and there is a carbon layer on the outermost layer.

[0087] The XRD pattern of the Si@ZnSe / CoSe@C composite material obtained in this example is shown in Figure 4 As shown, Fig.26 The D and G bands in the Raman image can verify the presence of carbon, proving that the obtained product is Si@ZnSe / CoSe@C. The XRD pattern of the Si@Zn(OH)2 / Co(OH)2 precursor material obtained in this example is as follows: Figure 5 shown.

[0088] A lithium ion battery, the preparation method is as follows: the three-dimensional flower-shaped Si@ZnSe / CoSe@C composite material prepared in Example 1 is used as an active material, and is mixed with conductive carbon black and PVDF in a ratio of 7:2:1, and then NMP is added dropwise, and the mixture is evenly dispersed therein by magnetic stirring for 8 hours, and the mixed slurry is coated on a copper foil by a coater, and the mixture is placed in a vacuum drying oven at 60°C, and after drying for 24 hours, the mixture is pressed by a tablet press, and then cut into a small circular electrode sheet by a sheet cutter; the prepared electrode sheet is assembled into a button battery in a glove box filled with high-purity argon gas and the water oxygen value is ≤0.01ppm; the electrolyte is ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) in a volume ratio of 2:6:2 as a solvent, and contains 1M LiPF6. The purity of the lithium sheet is Li≥99.99%, the thickness is 0.5mm, and the sheet is cut into the size of the electrode sheet after rolling.

[0089] The specific method of assembling the battery is: add 1 drop of electrolyte on the positive electrode shell of the battery and place the electrode sheet, then add 1 drop of electrolyte and place the diaphragm, add 2 drops of electrolyte on the diaphragm and place the lithium sheet as the counter electrode, then put in two pieces of foam nickel, add 1 drop of electrolyte, cover the negative electrode shell, press and seal the battery with a hydraulic press, and leave it for 12 hours.

[0090] Then at 0.5Ag -1 , 1Ag -1 The cycle performance and charge-discharge performance of the button battery were tested at a current of Fig.14 , Fig.15 , Fig.16 As shown: Fig.14 The three-dimensional flower-like structure Si@ZnSe / CoSe@C material is used as a negative electrode material for lithium-ion batteries at 0.5Ag -1 The charge and discharge curve test diagram under current density; Fig.15 Its Si@ZnSe / CoSe@C material as anode material for lithium-ion batteries at 0.5Ag -1 Cyclic performance test diagram under current density, which is 0.5Ag -1 After 300 cycles at the current density, the specific capacity is 501.18 mAh g -1 . Fig.16 Si@ZnSe / CoSe@C materials as negative electrode materials for lithium-ion batteries at 1Ag -1 Cyclic performance test diagram under current density, which is 1Ag -1 After 650 cycles at the current density, the specific capacity is 298.13 mAh g -1 , and the Coulomb efficiency is 99.66%. Fig.17 The three-dimensional flower-like structure Si@ prepared in Example 1

[0091] The rate performance test diagram of ZnSe / CoSe@C material as anode material for lithium-ion batteries at 0.1, 0.2, 0.3, 0.4, and 0.5Ag -1 The specific capacities at different current densities are 1308.26, 1083.16, 906.82, 744.64 and 691.12 mAh g -1 . Fig.18 The specific surface area of ​​the Si@ZnSe / CoSe@C prepared in Example 1, the ZnSe prepared in Example 7, and the CoSe prepared in Example 8 was tested. Before the BET test, the samples were degassed in a vacuum at 120°C for 12 h to remove the water adsorbed on the surface. Then, the physical adsorption isotherm (adsorption-desorption branch) was recorded using a specific surface area tester (ASAP Micromeritics Tristar 2460). The results were: Fig.18 The specific surface area of ​​Si@ZnSe / CoSe@C is 56.93 m 2 g -1 , higher than ZnSe (38.20m 2 g -1 ) and the specific surface area of ​​CoSe (4.26 m 2 g -1 ). The large specific surface area and rich porous structure can reduce the diffusion path and increase the active sites. It further proves that the synthesized Si@ZnSe / CoSe@C composite material has excellent performance. It provides a shuttle channel for the transfer of lithium ions, thereby increasing the storage capacity of lithium ions.

[0092] Example 2 (for comparison)

[0093] A method for preparing a three-dimensional flower-shaped Si@ZnSe / CoSe@C composite material comprises the following steps:

[0094] 1) Preparation of precursor Si@Zn(OH)2 / Co(OH)2:

[0095] Take 0.1g of 30nm silicon particle powder and ultrasonically disperse it in a 50mL beaker containing 32mL of anhydrous ethanol to form a uniform solution, which is recorded as solution A; weigh 4.9g Co(NO3)2·6H2O, 2.5g Zn(NO3)2·6H2O and 2.5g urea and add them to a 100mL beaker containing 15mL of deionized water, stir vigorously to form a uniform solution, which is recorded as solution B. Pour solution A into solution B and stir magnetically for 10min to mix it thoroughly. Then transfer it to a water bath and heat it at 90℃ Reaction 3h Cool naturally to room temperature, wash with deionized water 4 times by centrifugation, wash with ethanol 2 times, dry under vacuum at 60℃ for 12h, and collect the precursor Si@Zn(OH)2 / Co(OH)2 precipitation product. Its SEM picture is as follows Figure 6 As shown, it can be seen that the composite material structure is incomplete.

[0096] 2) Preparation of Si@ZnSe / CoSe@C:

[0097] 0.2 g Si@Zn(OH)2 / Co(OH)2 obtained in step 1) was dispersed in 50 mL of deionized water, 0.611 g of tris(hydroxymethyl)aminomethane was added to the solution, and after ultrasonication for 10 min, the pH was adjusted to 8.5 with hydrochloric acid, 35 mg of dopamine hydrochloride was added, and the mixture was stirred at room temperature for 24 hours. After the reaction was completed, the product was obtained by centrifugation, washing, and drying;

[0098] 3) The obtained product was then mixed with selenium powder in a mass ratio of 1:5 and placed in two porcelain boats, and calcined in a hydrogen and argon flowing atmosphere at a heating rate of 2°C / min to a calcination temperature of 560°C for 2 hours. The calcination atmosphere was hydrogen and argon gas with a volume fraction of 5% hydrogen and 95% argon, and finally the product Si@ZnSe / CoSe@C was obtained, and its SEM image is shown as follows Figure 7 As shown in the figure, it can be seen that the morphology of the composite material is not good and no flowers are formed. Figure 8 shown.

[0099] Figure 6It can be seen that the reaction time for synthesizing Si@Zn(OH)2 / Co(OH)2 in Example 2 is 3h, which is too long and leads to poor morphology. Therefore, the preferred reaction time of the present invention is 1 hour at 90°C.

[0100] Example 3 (for comparison)

[0101] A method for preparing a three-dimensional flower-shaped Si@ZnSe / CoSe@C composite material comprises the following steps:

[0102] 1) The preparation of the precursor is the same as in Example 1;

[0103] 2) Preparation of Si@ZnSe / CoSe@C:

[0104] The obtained 0.2 g Si@Zn(OH)2 / Co(OH)2 was dispersed in 50 mL of deionized water. 1.6g Tris(hydroxymethyl)aminomethane was added to the solution, and after ultrasonication for 10 min, the pH was adjusted to 8.5 with hydrochloric acid, and then added 85mg Dopamine hydrochloride was stirred at room temperature for 24 hours, and the product was obtained after centrifugation, washing and drying after the reaction was completed;

[0105] 3) The obtained product was then mixed with selenium powder in a mass ratio of 1:5 and placed in two porcelain boats, and calcined in a hydrogen and argon flowing atmosphere at a heating rate of 2°C / min to a calcination temperature of 560°C for 2 hours. The calcination atmosphere was hydrogen and argon gas with a volume fraction of 5% hydrogen and 95% argon, and the product Si@ was finally obtained.

[0106] The SEM image of ZnSe / CoSe@C is shown in Fig. 9 As shown, it can be seen from the figure that it is a spherical structure.

[0107] from Fig. 9 It can be seen from the figure that the amount of reagent added during carbon coating increases, resulting in thicker carbon coating, thus destroying the flower-like morphology. Therefore, the composite material synthesized according to Example 1 has the best effect.

[0108] Example 4 (for comparison)

[0109] A method for preparing a three-dimensional flower-shaped Si@ZnSe / CoSe@C composite material comprises the following steps:

[0110] 1) The preparation of the precursor is the same as in Example 1;

[0111] 2) 0.2 g of Si@Zn(OH)2 / Co(OH)2 was dispersed in 50 mL of deionized water, 0.611 g of tris(hydroxymethyl)aminomethane was added to the solution, and after ultrasonication for 10 min, the pH was adjusted to 8.5 with hydrochloric acid, 35 mg of dopamine hydrochloride was added, and the mixture was stirred at room temperature for 24 hours. After the reaction was completed, the product was obtained by centrifugation, washing, and drying;

[0112] 3) Then the obtained product is mixed with selenium powder according to the mass ratio 1:10 They were placed in two porcelain boats and calcined in a hydrogen and argon flowing atmosphere at a heating rate of 2°C / min until the calcination temperature was 560°C. The calcination time was 2h. The calcination atmosphere was hydrogen and argon gas with a volume fraction of 5% hydrogen and 95% argon. Finally, the product Si@ZnSe / CoSe@C was obtained. Its SEM image is shown in Fig.10 As shown in the figure, it can be seen that it is a flower ball structure, and the TEM image is as follows Fig.11 As shown, the flower-like flakes cannot be formed. It is further highlighted that the mass ratio of Example 1 is 1:5, which is the best example.

[0113] Example 5 (for comparison)

[0114] A method for preparing a three-dimensional flower-shaped Si@ZnSe / CoSe@C composite material comprises the following steps:

[0115] 1) The preparation of the precursor is the same as in Example 1;

[0116] 2) 0.2 g of Si@Zn(OH)2 / Co(OH)2 was dispersed in 50 mL of deionized water, 0.611 g of tris(hydroxymethyl)aminomethane was added to the solution, and after ultrasonication for 10 min, the pH was adjusted to 8.5 with hydrochloric acid, 35 mg of dopamine hydrochloride was added, and the mixture was stirred at room temperature for 24 hours. After the reaction was completed, the product was obtained by centrifugation, washing, and drying;

[0117] 3) The obtained product was then mixed with selenium powder in a mass ratio of 1:5 and placed in two porcelain boats, and calcined in a hydrogen and argon flowing atmosphere at a heating rate of 2°C / min until the calcination temperature was 800℃ , calcination time 2h, calcination atmosphere is hydrogen argon gas, volume fraction 5% hydrogen and 95% argon, the final product is still Si@ZnSe / CoSe@C, its SEM picture is as follows Fig.12 As shown in the TEM image Fig.13 shown.

[0118] After increasing the calcination temperature, although the XRD of the composite material is basically the same as that of Example 1, the flower-like structure collapses.

[0119] Example 6 (for comparison)

[0120] The 30nm Pure silicon particles in batteries (The silicon particles are the same as those used in Example 1, and the process of assembling the battery is the same as the process of assembling the battery with the materials in Example 1). The battery was assembled in the same manner as above, and tested in the same manner and with the same parameters. Fig.19 It can be seen that pure silicon particles at 0.1Ag -1 At a current density of , the cycle performance is poor and decays faster than that of the composite material in Example 1.

[0121] Example 7 (for comparison)

[0122] The same method as in Example 1 was used except that No silicon particles and cobalt nitrate hexahydrate were added. The ZnSe nanomaterials were synthesized separately and assembled into batteries according to the same method as above, and tested according to the same method and parameters. Fig. 20 , Fig.21 It can be found that it is 0.5, 1Ag -1 Under the conditions of low specific capacity and poor cycle performance.

[0123] Example 8 (for comparison)

[0124] The same method as in Example 1 was used except that no Add silicon particles and zinc nitrate hexahydrate, The CoSe nanomaterials were synthesized separately and the batteries were assembled according to the same method as above and tested according to the same method and parameters. Fig. 22 , Fig.23 It can be found that it is 0.5, 1Ag -1 Under the conditions of low specific capacity and poor cycle performance.

[0125] Example 9 (for comparison)

[0126] According to the same preparation method as Example 1, The silicon particles are simply replaced with Fe3O4 pellets, which are commercially available Product , particle size is 20nm, from Fig.24 It can be found from the XRD diagram in that Fe3O4@ZnSe / CoSe@C cannot be synthesized, which further verifies the stability of the silicon particles. Even during selenization, the composition of the silicon particles remains unchanged, reflecting the superiority and particularity of the composite material synthesized by the present invention.

[0127] The underlined data above do not meet the requirements of the present invention.

[0128] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A method for preparing a three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material, characterized in that: The preparation method comprises the following steps: 1) Dispersing silicon material in a solvent to form a uniform solution, recorded as solution A; mixing cobalt salt, zinc salt and urea in water, stirring evenly, recorded as solution B; after mixing solution A and solution B evenly, reacting in a water bath to obtain flower-shaped Si@Zn(OH)2 / Co(OH)2; 2) dispersing the Si@Zn(OH)2 / Co(OH)2 obtained in step 1) in water, adding tris(hydroxymethyl)aminomethane, adjusting the pH to 8-9 with hydrochloric acid, and then adding dopamine hydrochloride, stirring to react; 3) calcining the product of step 2) and selenium powder to obtain a three-dimensional flower-like Si@ZnSe / CoSe@C composite material.

2. The preparation method according to claim 1, characterized in that: In step 1), the amount ratio of silicon material to solvent is 0.05-0.3 mol / L; the solvent is anhydrous ethanol.

3. The preparation method according to claim 1, characterized in that: In step 1), the mass ratio of the cobalt salt, the zinc salt and the urea is 2.5:1.3:1.3 to 6.54:3.6:3.

6.

4. The preparation method according to claim 1 or 3, characterized in that: In step 1), the volume ratio of the solvent to deionized water is 32:

15.

5. The preparation method according to claim 1, characterized in that: In step 1), the water bath reaction is carried out at 60-100° C. for 30 minutes to 2 hours.

6. The preparation method according to claim 1, characterized in that: In step 2), the mass ratio of Si@Zn(OH)2 / Co(OH)2, tris(hydroxymethyl)aminomethane and dopamine hydrochloride is 1:3:0.175 to 1:6:0.

3.

7. The preparation method according to claim 1, characterized in that: In step 3), the mass ratio of the product of step 2) to selenium powder is 1:3-1:8; the calcination conditions are 500-700°C for 1-4 hours, and the calcination atmosphere is hydrogen-argon gas, which is 5% hydrogen and 95% argon by volume.

8. A three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material has a size between 10-15um, Si particles are grown in ZnSe / CoSe petals, the outermost layer is a carbon layer, the particle size of the Si particles is 30±5nm, and the thickness of the nanosheet is 100±20nm.

9. A lithium-ion battery silicon-based negative electrode, characterized in that: The three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material is prepared using the three-dimensional flower-shaped silicon@zinc selenide / cobalt selenide@carbon composite material described in claim 8.

10. A lithium ion battery, characterized in that: It is prepared using the lithium-ion battery silicon-based negative electrode described in claim 9.

Citation Information

Patent Citations

  • Preparation method and application of cobalt selenide / zinc selenide@nitrogen doped porous carbon nanotubes

    CN110492081A

  • Flower-like zinc selenide-manganese / carbon composite material as well as preparation method and application thereof

    CN114725334A

  • Core-shell silicon, selenium tin sulfide and carbon nanosphere structure material, preparation method of core-shell silicon, selenium tin sulfide and carbon nanosphere structure material, lithium ion battery silicon-based negative electrode and battery

    CN118486791A