Quantum dot light emitting diode device and preparation method and application thereof
By adding an inorganic metal material containing OH- into the electron transport layer of the quantum dot light-emitting diode device, the film layer inhomogeneity caused by ZnO agglomeration is solved, electron-hole injection balance is achieved, and the performance and life of the device are improved.
Patent Information
- Application Number
- CN202310626703.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing quantum dot light-emitting diode devices have uneven film layers due to the agglomeration of the electron transport layer material ZnO, which affects the efficiency and life of the device. The electron-hole injection imbalance limits the improvement of device performance.
The inorganic metal material containing OH- is added to the electron transport layer, and free conductive ions are formed by dissolving and mixing each other, covering the surface of the luminescent layer evenly, filling the ZnO uncovered area, enhancing electron transport capabilities and reducing defects, and achieving electron-hole injection balance.
It improves the overall performance of quantum dot light emitting diode devices, enhances electron transmission capabilities, reduces the fluorescence quenching of quantum dots, and improves the photoelectric conversion efficiency and service life.
Smart Images

Figure CN119072144A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of light emitting diodes, and in particular to a quantum dot light emitting diode device and a preparation method and application thereof. Background Art
[0002] Quantum dot light-emitting diode (QLED) is an active light-emitting display technology based on the principle of quantum dot electroluminescence. It has the characteristics of ultra-thin, high color gamut, flexibility, and high contrast, which can bring consumers unparalleled picture quality experience. From the perspective of color gamut, due to the extremely narrow half-peak width and the adjustable emission wavelength with size, QLED can theoretically reach 140% NTSC color gamut, which is much higher than the 100% NTSC color gamut of organic light-emitting semiconductors (OLED) and the 72% NTSC color gamut of liquid crystal displays (LCD), and can better present natural colors. In terms of contrast, since QLED and OLED are both based on self-luminous technology, they will be significantly better than traditional liquid crystal display technology (LCD) based on passive luminescence in terms of contrast, and can provide display devices with a purer black field display effect. In terms of product form, QLED technology and OLED have similar device structures, and can achieve characteristics such as ultra-thinness and flexibility. From the perspective of energy consumption, the energy consumption levels of several technologies are QLED < OLED < LCD, arranged from low to high. Compared with OLED, QLED requires a lower driving voltage at the same brightness, so the energy consumption is low. LCD is a backlight technology, and the conversion of white light into a single color of light requires filtering a large amount of other light energy, so the energy consumption is higher.
[0003] Quantum dot light-emitting diodes (QLEDs) are usually composed of five parts: an anode, a hole injection / transport layer, a quantum dot light-emitting layer, an electron injection / transport layer, and a cathode. The working principle of QLED is that under the drive of an external voltage, holes are injected from the anode and electrons are injected from the cathode. After being transported through their respective transport layers, they reach the quantum dots to form exciton recombination and luminescence. At present, ZnO is basically used as an electron transport layer in standard devices because it has good lattice structure and electrical properties. ZnO is a wide bandgap semiconductor at room temperature and has a high exciton binding energy. It has a strong hole-blocking effect when used as an electron transport layer in QLED devices, and its transmittance in the visible light region is as high as more than 90%. However, since the hole mobility of the organic semiconductor material commonly used in QLED devices is lower than the electron mobility of ZnO, the injection and transmission efficiency of electrons in the device is much greater than the injection and transmission efficiency of holes, resulting in an imbalance in electron-hole injection, thereby limiting the improvement of device efficiency. At the same time, ZnO is easy to agglomerate in the solution. After ZnO agglomerates in the solution, it will cause uneven film layer during the spin coating process. For example, there will be too many accumulated ZnO particles in some places of the film layer, while there will be no ZnO particles in some places. The obtained film layer has many surface defects, resulting in uneven electron transmission. Moreover, the bumpy surface of ZnO is in direct contact with the quantum dot layer, which will cause the fluorescence quenching of the quantum dots, thereby affecting the efficiency and life of the device.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide a quantum dot light emitting diode device and a preparation method and application thereof.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a quantum dot light-emitting diode device, comprising an anode substrate layer, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode layer stacked in sequence, wherein the material of the electron transport layer comprises ZnO and OH - Inorganic metal materials.
[0008] In a second aspect, the present invention provides a method for preparing a quantum dot light-emitting diode device as in any of the aforementioned embodiments, comprising sequentially spin-coating the material of a hole injection layer, the material of a hole transport layer, the material of a light-emitting layer and the material of an electron transport layer on the surface of an anode substrate layer, each spin coating is performed after the previous layer is formed, and then coating a cathode layer on the surface of the electron transport layer.
[0009] In a third aspect, the present invention provides a quantum dot light-emitting diode device as in any one of the aforementioned embodiments or a quantum dot light-emitting diode device prepared by the preparation method as in any one of the aforementioned embodiments, and its application in the field of light-emitting equipment.
[0010] The present invention has the following beneficial effects:
[0011] The present invention provides a quantum dot light emitting diode device and a preparation method and application thereof, by adding OH - Inorganic metal materials, ZnO and OH - The inorganic metal materials can dissolve and mix with each other, and free conductive ions are likely to appear in the solution. These free conductive ions can evenly cover the surface of the light-emitting layer in the subsequent preparation process. The surface of the electron transport layer formed is composed of ZnO and conductive ions precipitated from the solution, and the areas not covered by ZnO are filled with conductive ions, thereby enhancing the overall electron transport capacity of the electron transport layer and improving the overall performance of the device. In addition, due to the filling effect of conductive particles, the defects on the electron transport layer are reduced, thereby reducing the quenching phenomenon of quantum dots. At the same time, it can also reduce the electron migration efficiency of the electron transport layer, making the injection of electrons and holes more balanced, thereby achieving the purpose of improving device performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0013] Figure 1 A schematic diagram of the structure of a quantum dot light emitting diode device provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0014] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0015] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0016] like Figure 1 As shown, in the first aspect, the present invention provides a quantum dot light-emitting diode device 100, comprising an anode substrate layer 110, a hole injection layer 120, a hole transport layer 130, a light-emitting layer 140, an electron transport layer 150 and a cathode layer 160 stacked in sequence, wherein the material of the electron transport layer 150 comprises ZnO and OH - Inorganic metal materials.
[0017] By adding OH - Inorganic metal materials, ZnO and OH - The inorganic metal materials can be dissolved and mixed with each other, and free conductive ions are likely to appear in the solution. These free conductive ions can evenly cover the surface of the light-emitting layer in the subsequent preparation process. The surface of the electron transport layer formed is composed of ZnO and conductive ions precipitated from the solution, and the areas not covered by ZnO are filled with conductive ions, thereby enhancing the overall electron transport capacity of the electron transport layer and improving the overall performance of the device. In addition, due to the filling effect of the conductive particles, the defects on the electron transport layer 150 are reduced, thereby reducing the quenching phenomenon of quantum dots, thereby achieving the purpose of improving device performance.
[0018] In an alternative embodiment, the OH - The inorganic metal material accounts for 2.5 to 10% of the ZnO content, preferably 3.33 to 6.67%. - The inorganic metal material content is controlled within the above range, which can take into account both the light transmittance and electron-hole injection balance of the quantum dot light-emitting diode device 100. - If the content of inorganic metal material is low, the electron-hole injection balance cannot be achieved, and the morphological defects on the electron transport layer 150 cannot be improved. - When the content of the inorganic metal material is high, the structure of the formed electron transport layer 150 is turbid, which affects the light transmittance.
[0019] Preferably, the inorganic metal material containing OH- includes any one of NaOH, Al(OH)3, KOH, and Mg(OH)2, preferably NaOH. In the above inorganic metal material containing OH-, metal ions do not have the problem of agglomeration. When they are uniformly dispersed in the alcohol solution of ZnO, they are evenly covered on the surface of the film layer by spin coating, so that the positions not covered by ZnO can also transmit electrons, thereby improving the uniformity of electron transmission.
[0020] In an optional embodiment, the material of the light-emitting layer 140 is quantum dots, and the quantum dots are Cd-based quantum dots, such as ZnCdS.
[0021] Preferably, the conductive material of the anode substrate layer 110 is an indium tin oxide substrate. A layer of In2O3 or SnO2 transparent conductive layer can also be evaporated on the surface of the indium tin oxide substrate. The anode substrate layer 110 can be composed of an anode layer and a substrate layer. For example, a layer of conductive material is coated on the surface of the substrate to simultaneously realize the function of the anode conducting and the function of the substrate supporting the overall structure.
[0022] More preferably, the resistance of the conductive material of the anode substrate layer 110 is 20 to 40 Ω / sp; for example, the resistance of the conductive material of the anode substrate layer 110 may be 20 Ω / sp, 22 Ω / sp, 24 Ω / sp, 26 Ω / sp, 28 Ω / sp, 30 Ω / sp, 32 Ω / sp, 34 Ω / sp, 36 Ω / sp, 38 Ω / sp or 40 Ω / sp.
[0023] More preferably, the thickness of the anode substrate layer 110 is 0.5-2 mm; for example, the thickness of the anode substrate layer 110 may be 0.5 mm, 1 mm, 1.5 mm or 2 mm.
[0024] Preferably, the material of the hole injection layer 120 is PE-DOT.
[0025] Preferably, the material of the hole transport layer 130 includes TFB or PMA, preferably TFB.
[0026] Preferably, the material of the cathode layer 160 includes either silver or aluminum; preferably, the thickness of the cathode layer 160 is 80 to 120 nm; for example, the thickness of the cathode layer 160 may be 80 nm, 90 nm, 100 nm, 110 nm or 120 nm.
[0027] In a second aspect, the present invention provides a method for preparing a quantum dot light-emitting diode device as in any of the aforementioned embodiments, comprising sequentially spin-coating the material of a hole injection layer, the material of a hole transport layer, the material of a light-emitting layer and the material of an electron transport layer on the surface of an anode substrate layer, each spin coating is performed after the previous layer is formed, and then coating a cathode layer on the surface of the electron transport layer.
[0028] The present invention adopts the spin coating method to obtain a film layer with uniform surface morphology, and the operation is simple and cost-saving.
[0029] In an optional embodiment, the material of the electron transport layer is a solution before spin coating, and the concentration of ZnO in the solution is 20-40 mg / ml, for example, the concentration of ZnO in the solution can be 20 mg / ml, 22 mg / ml, 24 mg / ml, 26 mg / ml, 28 mg / ml, 30 mg / ml, 32 mg / ml, 34 mg / ml, 36 mg / ml, 38 mg / ml or 40 mg / ml. Preferably, the concentration of ZnO is 30 mg / ml.
[0030] The concentration of the inorganic metal material containing OH- is 1-2 mg / ml; wherein the concentration of the inorganic metal material containing OH- is relative to the concentration of ZnO in the solution.
[0031] Preferably, the solvent of the material of the electron transport layer includes any one of ethanol, methanol, and isopropanol. Preferably, ethanol. At present, common ZnO solvents are all alcohol solvents. By using alcohol solvents to disperse ZnO, because ZnO is easy to agglomerate in alcohol solution, the agglomerated ZnO is prone to uneven distribution of ZnO on the surface of the film layer during the preparation of the electron transport layer. By adding an inorganic metal material containing OH-, using the principle of similar dissolving, such as NaOH can be dissolved in the alcohol solution, so that it can be evenly covered on the surface of the light-emitting layer during spin coating, thereby achieving the effect of modifying the film layer, and the inorganic metal material containing OH- can precipitate conductive ions in the alcohol solvent, and the filling of these conductive ions also increases the electron transmission capacity of the electronic conductive layer.
[0032] Preferably, the electron transport layer material is spin-coated at a speed of 2500 to 3500 rpm / min, for example, 2500 rpm / min, 2700 rpm / min, 2900 rpm / min, 3100 rpm / min, 3300 rpm / min or 3500 rpm / min. More preferably, the spin-coating speed is 3000 rpm / min.
[0033] Preferably, the spin coating time of the electron transport layer material is 30 to 50 seconds, for example, 30 seconds, 35 seconds, 40 seconds, 45 seconds or 50 seconds. Preferably, the spin coating time is 40 seconds.
[0034] Preferably, after the spin coating is completed, the quantum dot light-emitting diode device with an electron transport layer is subjected to annealing. The purpose of annealing is, on the one hand, to remove the solvent in the solution and retain the effective materials therein; on the other hand, to fix the effective materials on the surface and ensure the stability of the structure of the quantum dot light-emitting diode device.
[0035] Preferably, during the annealing process of the material of the electron transport layer, the heating temperature is 70-90° C., for example, 70° C., 75° C., 80° C., 85° C. or 90° C. More preferably, the heating temperature of the annealing process is 80° C.
[0036] Preferably, the annealing time for the material of the electron transport layer is 20 to 40 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes. Preferably, the annealing time is 30 minutes.
[0037] In an optional embodiment, the material of the light-emitting layer is a solution before spin coating, and the concentration of quantum dots in the solution is 15-25 mg / ml; for example, it can be 15 mg / ml, 17 mg / ml, 19 mg / ml, 21 mg / ml, 23 mg / ml or 25 mg / ml. Preferably, the concentration of quantum dots in the solution is 20 mg / ml.
[0038] Preferably, the solvent comprises n-octane.
[0039] Preferably, the rotation speed of the light-emitting layer material during spin coating is 2000-3000 rpm / min, for example, 2000 rpm / min, 2200 rpm / min, 2400 rpm / min, 2600 rpm / min, 2800 rpm / min or 3000 rpm / min. The spin coating time is 30-50 s, for example, 30 s, 35 s, 40 s, 42 s, 44 s, 46 s, 48 s or 50 s.
[0040] In an optional embodiment, the material of the hole transport layer is a solution before spin coating, and the concentration of the solute in the solution is 5 to 15 mg / ml. For example, it can be 5 mg / ml, 7 mg / ml, 9 mg / ml, 11 mg / ml, 13 mg / ml or 15 mg / ml. Preferably, the concentration of the solute in the solution is 10 mg / ml. Among them, the solute of the hole transport layer is an effective material such as TFB that can play a hole transport role.
[0041] Preferably, the solvent includes any one of chlorobenzene or 1,4-dioxane.
[0042] Preferably, the rotation speed of the hole transport layer material during spin coating is 2000-3000 rpm / min, for example, 2000 rpm / min, 2200 rpm / min, 2400 rpm / min, 2600 rpm / min, 2800 rpm / min or 3000 rpm / min. The spin coating time is 30-50 s, for example, 30 s, 35 s, 40 s, 42 s, 44 s, 46 s, 48 s or 50 s.
[0043] Preferably, after the spin coating is completed, the quantum dot light-emitting diode device with the hole transport layer is subjected to annealing treatment. Similarly, annealing can not only remove the solvent in the solution, but also make each layer structure closely connected with the previous layer structure.
[0044] Preferably, the heating temperature for annealing the hole transport layer material is 140-160° C., for example, 140° C., 145° C., 150° C., 155° C. or 160° C. More preferably, the heating temperature for annealing is 150° C.
[0045] Preferably, the annealing time of the hole transport layer material is 20 to 40 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes. Preferably, the annealing time is 30 minutes.
[0046] In an optional embodiment, the material of the hole injection layer is a solution before spin coating, and the concentration of the solute in the solution is 6-10 mg / ml, more preferably 8 mg / ml. The solute of the hole injection layer is an effective material such as PE-DOT that can play a role in injecting holes.
[0047] Preferably, the solvent is water, more preferably pure water.
[0048] Preferably, the rotation speed of the hole injection layer material during spin coating is 4000-5000 rpm / min, for example, 4000 rpm / min, 4200 rpm / min, 4400 rpm / min, 4600 rpm / min, 4800 rpm / min or 5000 rpm / min. The spin coating time is 40-60 s, for example, 40 s, 45 s, 47 s, 50 s, 52 s, 55 s, 57 s or 60 s.
[0049] Preferably, after the spin coating is completed, the quantum dot light emitting diode device with the hole injection layer is subjected to annealing treatment.
[0050] Preferably, the material of the hole injection layer is heated at a temperature of 140-160° C. during annealing, for example, 140° C., 145° C., 150° C., 155° C. or 160° C. More preferably, the heating temperature of the annealing is 150° C.
[0051] Preferably, the annealing time of the hole injection layer material during the annealing treatment is 10 to 20 minutes, for example, 10 minutes, 15 minutes or 20 minutes. Preferably, the annealing time is 15 minutes.
[0052] In an optional embodiment, before coating the cathode layer, depending on the different quantum dot light-emitting diode devices prepared, chlorobenzene is also used to erase the film layers at the edge of the anode substrate layer, such as the hole injection layer, the hole transport layer, the light-emitting layer and the electron transport layer, to expose the bottom anode layer, so that the anode and cathode of the quantum dot light-emitting diode device are conductive.
[0053] In an optional embodiment, the cathode layer is coated by evaporation; preferably, the evaporation rate is 1 to 2 A / s.
[0054] In the above preparation method, by controlling the rotation speed of spin coating, the thickness of each layer can be well controlled. The faster the spin coating rotation speed, the thinner the coating, and the slower the spin coating rotation speed, the thicker the coating.
[0055] In an optional embodiment, the quantum dot light emitting diode device is also packaged to prevent air from entering and affecting its light emitting life.
[0056] Preferably, the encapsulation includes encapsulation with ultraviolet curing glue, and after dripping the ultraviolet curing glue, curing by ultraviolet lamp irradiation. Preferably, the curing time by ultraviolet lamp irradiation can be 20 to 60 seconds.
[0057] In a third aspect, the present invention provides a quantum dot light-emitting diode device as in any one of the aforementioned embodiments or a quantum dot light-emitting diode device prepared by the preparation method as in any one of the aforementioned embodiments, and its application in the field of light-emitting equipment.
[0058] Example 1
[0059] This embodiment provides a quantum dot light-emitting diode device, which includes an anode substrate layer, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode layer stacked in sequence. The specific preparation method is as follows:
[0060] S01. The anode substrate layer uses an indium tin oxide glass substrate with a thickness of 1 mm and a resistance of 30 Ω / sp, which can be obtained commercially.
[0061] S02. The material of the hole injection layer is PE-DOT solution. Pure water is used as a solvent to dissolve PE-DOT to obtain a PE-DOT solution with a concentration of 8 mg / ml for use.
[0062] The PE-DOT solution was spin-coated on the surface of the indium tin oxide glass substrate at a spin-coating speed of 4000 rpm / min for 40 seconds. After the spin-coating, the substrate was heated at 150° C. and annealed for 15 minutes to obtain a hole injection layer.
[0063] S03. The material of the hole transport layer is TFB solution. Chlorobenzene is used as a solvent to dissolve TFB to obtain a TFB solution with a concentration of 10 mg / ml for use.
[0064] The TFB solution was spin-coated on the surface of the hole injection layer obtained in step S02 at a spin-coating speed of 3000 rpm / min for 30 seconds. After the spin-coating, the layer was heated at 150° C. and annealed for 30 minutes to obtain a hole transport layer.
[0065] S04. The material of the light-emitting layer is a ZnCdS quantum dot solution. Pyridone glycolate is used as a solvent to dissolve the ZnCdS quantum dots to obtain a ZnCdS quantum dot solution with a concentration of 20 mg / ml for use.
[0066] The surface of the hole transport layer obtained in step S03 was spin-coated with a ZnCdS quantum dot solution at a spin-coating speed of 3000 rpm / min for 30 seconds to obtain a light-emitting layer.
[0067] S05. The material of the electron transport layer is a mixed solution of ZnO and NaOH. Ethanol is used as a solvent to dissolve ZnO and NaOH to obtain a mixed solution of ZnO and NaOH with a ZnO concentration of 30 mg / ml and a NaOH concentration of 1 mg / ml for later use.
[0068] The surface of the light-emitting layer obtained in step S04 is spin-coated with a mixed solution of ZnO and NaOH at a spin-coating speed of 3000 rpm / min for 40 seconds. After the spin-coating, it is heated at 80° C. and annealed for 30 minutes to obtain an electron transport layer.
[0069] S06, preparation of cathode layer: wipe the edge of the material obtained in step S05. Use chlorobenzene to wipe the hole injection layer, hole transport layer, light-emitting layer and electron transport layer at the edge of the indium tin oxide glass substrate to expose the indium tin oxide anode layer at the bottom, and then place it in an evaporation device to evaporate the Ag electrode at a rate of 1.5A / s. The thickness of the evaporated Ag electrode is 100nm.
[0070] S07, Packaging
[0071] A UV curing glue was dripped onto the coated side of the indium tin oxide glass substrate, and a cover glass was placed on the substrate. The substrate was irradiated with a UV lamp for 30 seconds for curing, thereby obtaining a quantum dot light emitting diode device.
[0072] Example 2
[0073] This embodiment provides a quantum dot light-emitting diode device, which includes an anode substrate layer, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode layer stacked in sequence. The specific preparation method is as follows:
[0074] S01. The anode substrate layer uses an indium tin oxide glass substrate with a thickness of 1 mm and a resistance of 30 Ω / sp, which can be obtained commercially.
[0075] S02. The material of the hole injection layer is PE-DOT solution. Pure water is used as a solvent to dissolve PE-DOT to obtain a PE-DOT solution with a concentration of 8 mg / ml for use.
[0076] The PE-DOT solution was spin-coated on the surface of the indium tin oxide glass substrate at a spin-coating speed of 4000 rpm / min for 40 seconds. After the spin-coating, the substrate was heated at 150° C. and annealed for 15 minutes to obtain a hole injection layer.
[0077] S03. The material of the hole transport layer is TFB solution. Chlorobenzene is used as a solvent to dissolve TFB to obtain a TFB solution with a concentration of 10 mg / ml for use.
[0078] The TFB solution was spin-coated on the surface of the hole injection layer obtained in step S02 at a spin-coating speed of 3000 rpm / min for 30 seconds. After the spin-coating, the layer was heated at 150° C. and annealed for 30 minutes to obtain a hole transport layer.
[0079] S04. The material of the light-emitting layer is a ZnCdS quantum dot solution. Pyridone glycolate is used as a solvent to dissolve the ZnCdS quantum dots to obtain a ZnCdS quantum dot solution with a concentration of 20 mg / ml for use.
[0080] The surface of the hole transport layer obtained in step S03 was spin-coated with a ZnCdS quantum dot solution at a spin-coating speed of 3000 rpm / min for 30 seconds to obtain a light-emitting layer.
[0081] S05. The material of the electron transport layer is a mixed solution of ZnO and NaOH. Ethanol is used as a solvent to dissolve ZnO and NaOH to obtain a mixed solution of ZnO and NaOH with a ZnO concentration of 30 mg / ml and a NaOH concentration of 1 mg / ml for later use.
[0082] The surface of the light-emitting layer obtained in step S04 is spin-coated with a mixed solution of ZnO and NaOH at a spin-coating speed of 3000 rpm / min for 40 seconds. After the spin-coating, it is heated at 80° C. and annealed for 30 minutes to obtain an electron transport layer.
[0083] S06, preparation of cathode layer: wipe the edge of the material obtained in step S05. Use chlorobenzene to wipe the hole injection layer, hole transport layer, light-emitting layer and electron transport layer at the edge of the indium tin oxide glass substrate to expose the indium tin oxide anode layer at the bottom, and then place it in an evaporation device to evaporate the Ag electrode at a rate of 1.5A / s. The thickness of the evaporated Ag electrode is 100nm.
[0084] S07, Packaging
[0085] A UV curing glue was dripped onto the coated side of the indium tin oxide glass substrate, and a cover glass was placed on the substrate. The substrate was irradiated with a UV lamp for 30 seconds for curing, thereby obtaining a quantum dot light emitting diode device.
[0086] Example 3
[0087] This embodiment provides a quantum dot light-emitting diode device, which includes an anode substrate layer, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode layer stacked in sequence. The specific preparation method is as follows:
[0088] S01. The anode substrate layer uses an indium tin oxide glass substrate with a thickness of 1 mm and a resistance of 30 Ω / sp, which can be obtained commercially.
[0089] S02. The material of the hole injection layer is PE-DOT solution. Pure water is used as a solvent to dissolve PE-DOT to obtain a PE-DOT solution with a concentration of 8 mg / ml for use.
[0090] The PE-DOT solution was spin-coated on the surface of the indium tin oxide glass substrate at a spin-coating speed of 4000 rpm / min for 40 seconds. After the spin-coating, the substrate was heated at 150° C. and annealed for 15 minutes to obtain a hole injection layer.
[0091] S03. The material of the hole transport layer is TFB solution. Chlorobenzene is used as a solvent to dissolve TFB to obtain a TFB solution with a concentration of 10 mg / ml for use.
[0092] The TFB solution was spin-coated on the surface of the hole injection layer obtained in step S02 at a spin-coating speed of 3000 rpm / min for 30 seconds. After the spin-coating, the layer was heated at 150° C. and annealed for 30 minutes to obtain a hole transport layer.
[0093] S04. The material of the light-emitting layer is a ZnCdS quantum dot solution. Pyridone glycolate is used as a solvent to dissolve the ZnCdS quantum dots to obtain a ZnCdS quantum dot solution with a concentration of 20 mg / ml for use.
[0094] The surface of the hole transport layer obtained in step S03 was spin-coated with a ZnCdS quantum dot solution at a spin-coating speed of 3000 rpm / min for 30 seconds to obtain a light-emitting layer.
[0095] S05. The material of the electron transport layer is a mixed solution of ZnO and NaOH. Ethanol is used as a solvent to dissolve ZnO and NaOH to obtain a mixed solution of ZnO and NaOH with a ZnO concentration of 30 mg / ml and a NaOH concentration of 1 mg / ml for later use.
[0096] The surface of the light-emitting layer obtained in step S04 is spin-coated with a mixed solution of ZnO and NaOH at a spin-coating speed of 3000 rpm / min for 40 seconds. After the spin-coating, it is heated at 80° C. and annealed for 30 minutes to obtain an electron transport layer.
[0097] S06, preparation of cathode layer: wipe the edge of the material obtained in step S05. Use chlorobenzene to wipe the hole injection layer, hole transport layer, light-emitting layer and electron transport layer at the edge of the indium tin oxide glass substrate to expose the indium tin oxide anode layer at the bottom, and then place it in an evaporation device to evaporate the Ag electrode at a rate of 1.5A / s. The thickness of the evaporated Ag electrode is 100nm.
[0098] S07, Packaging
[0099] A UV curing glue was dripped onto the coated side of the indium tin oxide glass substrate, and a cover glass was placed on the substrate. The substrate was irradiated with a UV lamp for 30 seconds for curing, thereby obtaining a quantum dot light emitting diode device.
[0100] Example 4
[0101] This embodiment provides a quantum dot light-emitting diode device, which includes an anode substrate layer, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode layer stacked in sequence. The specific preparation method is as follows:
[0102] S01. The anode substrate layer uses an indium tin oxide glass substrate with a thickness of 1 mm and a resistance of 30 Ω / sp, which can be obtained commercially.
[0103] S02. The material of the hole injection layer is PE-DOT solution. Pure water is used as a solvent to dissolve PE-DOT to obtain a PE-DOT solution with a concentration of 8 mg / ml for use.
[0104] The PE-DOT solution was spin-coated on the surface of the indium tin oxide glass substrate at a spin-coating speed of 4000 rpm / min for 40 seconds. After the spin-coating, the substrate was heated at 150° C. and annealed for 15 minutes to obtain a hole injection layer.
[0105] S03. The material of the hole transport layer is TFB solution. Chlorobenzene is used as a solvent to dissolve TFB to obtain a TFB solution with a concentration of 10 mg / ml for use.
[0106] The TFB solution was spin-coated on the surface of the hole injection layer obtained in step S02 at a spin-coating speed of 3000 rpm / min for 30 seconds. After the spin-coating, the layer was heated at 150° C. and annealed for 30 minutes to obtain a hole transport layer.
[0107] S04. The material of the light-emitting layer is a ZnCdS quantum dot solution. Pyridone glycolate is used as a solvent to dissolve the ZnCdS quantum dots to obtain a ZnCdS quantum dot solution with a concentration of 20 mg / ml for use.
[0108] The surface of the hole transport layer obtained in step S03 was spin-coated with a ZnCdS quantum dot solution at a spin-coating speed of 3000 rpm / min for 30 seconds to obtain a light-emitting layer.
[0109] S05. The material of the electron transport layer is a mixed solution of ZnO and NaOH. Ethanol is used as a solvent to dissolve ZnO and NaOH to obtain a mixed solution of ZnO and NaOH with a ZnO concentration of 30 mg / ml and a NaOH concentration of 1 mg / ml for later use.
[0110] The surface of the light-emitting layer obtained in step S04 is spin-coated with a mixed solution of ZnO and NaOH at a spin-coating speed of 3000 rpm / min for 40 seconds. After the spin-coating, it is heated at 80° C. and annealed for 30 minutes to obtain an electron transport layer.
[0111] S06, preparation of cathode layer: wipe the edge of the material obtained in step S05. Use chlorobenzene to wipe the hole injection layer, hole transport layer, light-emitting layer and electron transport layer at the edge of the indium tin oxide glass substrate to expose the indium tin oxide anode layer at the bottom, and then place it in an evaporation device to evaporate the Ag electrode at a rate of 1.5A / s. The thickness of the evaporated Ag electrode is 100nm.
[0112] S07, Packaging
[0113] A UV curing glue was dripped onto the coated side of the indium tin oxide glass substrate, and a cover glass was placed on the substrate. The substrate was irradiated with a UV lamp for 30 seconds for curing, thereby obtaining a quantum dot light emitting diode device.
[0114] Comparative Example 1
[0115] This comparative example provides a quantum dot light-emitting diode device, which is different from Example 1 only in that the electron transport layer contains only ZnO and no NaOH.
[0116] Comparative Example 2
[0117] This comparative example provides a quantum dot light-emitting diode device, which is different from Example 2 only in that the electron transport layer contains only ZnO and no NaOH.
[0118] Comparative Example 3
[0119] This comparative example provides a quantum dot light-emitting diode device, which is different from Example 3 only in that the electron transport layer contains only ZnO and no NaOH.
[0120] Comparative Example 4
[0121] This comparative example provides a quantum dot light-emitting diode device, which is different from Example 4 only in that the electron transport layer contains only ZnO and no NaOH.
[0122] Comparative Example 5
[0123] This comparative example provides a quantum dot light-emitting diode device, the structure of which is the same as that of Example 1, except that the concentration of NaOH in the material of the electron transport layer is 0.5 mg / ml.
[0124] Comparative Example 6
[0125] This comparative example provides a quantum dot light-emitting diode device, the structure of which is the same as that of Example 1, except that the concentration of NaOH in the material of the electron transport layer is 3 mg / ml.
[0126] Test Example 1
[0127] The quantum dot light emitting diode devices prepared in Examples 1 to 4 and Comparative Examples 1 to 6 were tested. The photoelectric conversion efficiency (EQE) and service life thereof were tested respectively, and the results shown in Table 1 were obtained.
[0128] Table 1 Performance of quantum dot light-emitting diode devices
[0129]
[0130]
[0131] As can be seen from Table 1, the embodiment of the present invention uses - The electron transport layer prepared by compounding the inorganic metal material with ZnO is used in the quantum dot light-emitting diode device. Since the electron-hole injection balance is achieved, the photoelectric conversion efficiency (EQE) of the quantum dot light-emitting diode device is significantly improved. Moreover, the improved electron transport layer has fewer surface defects, which will not cause fluorescence quenching of quantum dots, thereby increasing the service life of the quantum dot light-emitting diode device. In addition, Comparative Examples 5 and 6 change the concentration of the inorganic metal material containing OH-. Comparative Example 5 reduces the concentration of the inorganic metal material containing OH-, and the surface defects of the electron transport layer are difficult to cover, and the photoelectric conversion efficiency and service life are reduced. Comparative Example 6 increases the concentration of the inorganic metal material containing OH-, resulting in turbidity of the solution for preparing the electron transport layer, which deteriorates the state of the film layer and reduces the performance of the device.
[0132] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A quantum dot light emitting diode device, characterized in that: The invention comprises an anode substrate layer, a hole injection layer, a hole transport layer, a light emitting layer, an electron transport layer and a cathode layer which are stacked in sequence, wherein the material of the electron transport layer comprises ZnO and an inorganic metal material containing OH-.
2. The quantum dot light emitting diode device according to claim 1, characterized in that: The OH - The inorganic metal material accounts for 2.5-10% of the ZnO content, preferably 3.33-6.67%; Preferably, the OH - The inorganic metal material includes any one of NaOH, Al(OH)3, KOH, and Mg(OH)2, preferably NaOH.
3. The quantum dot light emitting diode device according to claim 1, characterized in that: The material of the light-emitting layer is quantum dots, and the quantum dots are Cd-based quantum dots; Preferably, the conductive material of the anode substrate layer is indium tin oxide; more preferably, the resistance of the conductive material of the anode substrate layer is 20 to 40 Ω / sp; more preferably, the thickness of the anode substrate layer is 0.5 to 2 mm; Preferably, the material of the hole injection layer is PE-DOT; Preferably, the material of the hole transport layer includes any one of TFB or PMA; Preferably, the material of the cathode layer includes either silver or aluminum; preferably, the thickness of the cathode layer is 80-120 nm.
4. A method for preparing a quantum dot light-emitting diode device according to any one of claims 1 to 3, characterized in that: The method includes sequentially spin coating the material of the hole injection layer, the material of the hole transport layer, the material of the light emitting layer and the material of the electron transport layer on the surface of the anode substrate layer, each spin coating is performed after the previous layer is formed, and then the cathode layer is coated on the surface of the electron transport layer.
5. The preparation method according to claim 4, characterized in that: The material of the electron transport layer is a solution before spin coating, the concentration of ZnO in the solution is 20-40 mg / ml, and contains OH - The concentration of the inorganic metal material is 1-2 mg / ml; preferably, the concentration of ZnO is 30 mg / ml; Preferably, the solvent of the material of the electron transport layer includes any one of ethanol, methanol, and isopropanol; Preferably, the material of the electron transport layer is spin-coated at a speed of 2500 to 3500 rpm / min, and the spin-coating time is 30 to 50 s; more preferably, the spin-coating speed is 3000 rpm / min, and the spin-coating time is 40 s; Preferably, after the spin coating is completed, the quantum dot light-emitting diode device having the electron transport layer is subjected to annealing treatment; Preferably, the heating temperature of the annealing treatment is 70-90° C., and the annealing time is 20-40 min. More preferably, the heating temperature of the annealing treatment is 80° C., and the annealing time is 30 min.
6. The preparation method according to claim 4, characterized in that: The material of the light-emitting layer is a solution before spin coating, and the concentration of quantum dots in the solution is 15-25 mg / ml; preferably, the concentration of quantum dots in the solution is 20 mg / ml; Preferably, the solvent is n-octane; Preferably, the rotation speed of the material of the light-emitting layer during spin coating is 2000-3000 rpm / min, and the spin coating time is 30-50 s.
7. The preparation method according to claim 4, characterized in that: The material of the hole transport layer is a solution before spin coating, and the concentration of the solute in the solution is 5 to 15 mg / ml; preferably, the concentration of the solute in the solution is 10 mg / ml; Preferably, the solvent comprises any one of chlorobenzene or 1,4-dioxane; Preferably, the rotation speed of the hole transport layer material during spin coating is 2000-3000 rpm / min, and the spin coating time is 30-50 s; Preferably, after the spin coating is completed, the quantum dot light-emitting diode device having the hole transport layer is subjected to annealing treatment; Preferably, the heating temperature of the annealing treatment is 140-160° C., and the annealing time is 20-40 min. More preferably, the heating temperature of the annealing treatment is 150° C., and the annealing time is 30 min.
8. The preparation method according to claim 4, characterized in that: The material of the hole injection layer is a solution before spin coating, and the concentration of the solute in the solution is 6-10 mg / ml; Preferably, the solvent is water; Preferably, the rotation speed of the hole injection layer material during spin coating is 4000-5000 rpm / min, and the spin coating time is 40-60 s; Preferably, after the spin coating is completed, the quantum dot light-emitting diode device having the hole injection layer is subjected to an annealing treatment; Preferably, the heating temperature of the annealing treatment is 140-160° C., and the annealing time is 10-20 min. More preferably, the heating temperature of the annealing treatment is 150° C., and the annealing time is 15 min.
9. The preparation method according to claim 4, characterized in that: The cathode layer is coated by evaporation; preferably, the evaporation rate is 1-2 A / s.
10. Use of the quantum dot light emitting diode device as claimed in any one of claims 1 to 3 or the quantum dot light emitting diode device prepared by the preparation method as claimed in any one of claims 4 to 9 in the field of light emitting equipment.