Permeable membrane for efficient oil-gas separation as well as preparation method and application of permeable membrane

By blending modified polytetrafluoroethylene with modified gas-phase silica and combining with spin coating, the penetration membrane is solved, and the problems of low breathability efficiency and insufficient mechanical properties of the existing penetration membrane are achieved, and efficient oil and gas separation and transformer oil are achieved Improved efficiency of dissolved gas analysis.

CN119075709AActive Publication Date: 2024-12-06SHANGHAI RUIKAI ELECTRIC EQUIP CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411453857.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-12-06
Estimated Expiration
2044-10-17

AI Technical Summary

Technical Problem

The existing permeable membrane has low breathability efficiency and poor mechanical properties in the analysis of dissolved gases in transformer oil, resulting in long-term and low-efficiency gas analysis, and the main component fluorosilic rubber is not resistant to heat air aging and lacks stability.

Method used

Modified polytetrafluoroethylene and modified vapor phase silica are blended, and the permeable membrane is prepared by plasma pretreatment and grafting modifier, combined with spin coating method to improve its hydrophobicity and mechanical strength, and through composite Modifiers modify gas-phase silica to enhance the mechanical properties and gas flux of the film.

Benefits of technology

It significantly improves the breathable performance and mechanical strength of the permeable membrane, delays heat shrinkage, increases gas flux, achieves efficient oil and gas separation, and improves the efficiency and accuracy of dissolved gas analysis in transformer oil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005089907770000081
    Figure BDA0005089907770000081
  • Figure BDA0005089907770000091
    Figure BDA0005089907770000091
Patent Text Reader

Abstract

The invention relates to the field of permeable membrane preparation, and particularly discloses a preparation method and application of a permeable membrane for efficient oil-gas separation, and the preparation method comprises the following steps: (1) preparing primary modified polytetrafluoroethylene; (2) preparing secondary modified polytetrafluoroethylene; and (3) preparing the permeable membrane. The permeable membrane disclosed by the invention can be used for analyzing dissolved gas in transformer oil and can realize efficient separation of oil and gas, and the air permeability and the mechanical strength are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of permeable membrane preparation, and specifically discloses a permeable membrane for high-efficiency oil-gas separation, a preparation method and application thereof. Background Art

[0002] The transformer is one of the important operating equipment in the power system, and its normal operation has a great impact on the safe operation of the power grid. The insulating oil in the transformer decomposes under the action of heat and electricity to produce 7 kinds of characteristic gases such as H2, CO, CO2, CH4, C2H2, C2H4, and C2H6, which are dissolved in the insulating oil. When there is a latent overheating or discharge fault, the above gases will be produced faster. By detecting the content of dissolved gas in the insulating oil, the type and degree of transformer fault can be analyzed in time. Oil-gas separation is an important step in the analysis of dissolved gas in transformer oil, and the permeable membrane degassing method is one of the most commonly used methods for oil-gas separation.

[0003] Membrane material is the most critical factor affecting the performance of gas separation membranes. An ideal gas separation membrane should have excellent thermochemical stability, high mechanical strength and good permeability selectivity. The more commonly used membrane materials are organic polymer membranes, such as polyvinyl chloride, polyvinylidene fluoride and polyether block amide.

[0004] The invention patent with application number 202310297489.2 discloses an oil-gas separation membrane for transformer online detection and its preparation method, including: step 1, spreading liquid fluorosilicone rubber on a flat plate and curing to form a film; step 2, mixing and dispersing HyflonAD60 and perfluoropolyether thermal fluid evenly, adding α-phase nano-alumina powder, dispersing evenly, and obtaining a casting solution; step 3, coating the casting solution on the film, standing, covering with a pressing plate, heating to 180-220°C in a drying oven, and keeping the temperature constant for 3-10 hours; step 4, standing under high pressure, when it reaches 24-48 hours, placing it in a preheated drying oven again at a constant temperature for 6-12 hours, and cooling it. The preparation method of the invention has mild conditions, the mechanical strength of the prepared oil-gas separation membrane is high, and the time to achieve oil-gas separation is short. The oil-gas separation time of the oil-gas separation membrane disclosed in the invention is short, which can significantly improve the efficiency of transformer online detection and shorten the detection cycle.

[0005] However, the main component of the disclosed oil-gas separation membrane, fluorosilicone rubber, is not resistant to hot air aging, and has insufficient stability and durability. In addition, the gas separation capacity of the oil-gas separation membrane still has room for further improvement. At the same time, the existing permeable membrane materials also have problems such as low air permeability efficiency and low mechanical properties, which directly lead to long duration and low efficiency of gas analysis, as well as cracking and oil leakage of the permeable membrane after long-term operation. The oil-gas separation link of dissolved gas analysis in transformer oil urgently needs a degassing membrane with better air permeability and mechanical properties.

[0006] In view of this, it is particularly important to disclose a permeable membrane for efficient oil and gas separation in the present invention. Summary of the invention

[0007] In view of the defects of the prior art, the present invention discloses a permeable membrane for efficient oil-gas separation and its preparation method and application. The permeable membrane disclosed in the present invention can be used for analysis of dissolved gas in transformer oil, which can achieve efficient oil-gas separation, and the air permeability and mechanical strength are significantly improved.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] In one aspect, the present invention provides a method for preparing a permeable membrane for efficient oil-gas separation, comprising the following steps:

[0010] (1) Preparation of primary modified polytetrafluoroethylene: polytetrafluoroethylene is pretreated with plasma to obtain primary modified polytetrafluoroethylene;

[0011] (2) Preparation of secondary modified polytetrafluoroethylene: Mix the primary modified polytetrafluoroethylene and an organic solvent, add a grafting modifier, a crosslinking agent and an initiator, heat to 50-70°C, react for 2-5 hours, wash and dry to obtain the secondary modified polytetrafluoroethylene;

[0012] (3) Preparation of permeable membrane: Add secondary modified polytetrafluoroethylene and organic solvent into a reactor, stir and mix for 1 to 3 hours, then add modified fumed silica, stir and mix for 2 to 4 hours to obtain a mixed solution, place the mixed solution in an oven for degassing, and then spin-coat the mixed solution onto a dry and smooth substrate to form a film, and dry at room temperature to obtain the permeable membrane.

[0013] Preferably, in step (3), the spin coating is performed by dripping glue while rotating at a speed of 200 to 800 r / min. After completion, the speed is increased to 1000 to 2000 r / min and the rotation is performed for 30 seconds to 1 minute.

[0014] In some embodiments of the present invention, in step (1), the plasma pretreatment is performed by setting the discharge distance to 8 mm, the discharge power to 10000 Hz, the voltage to 30-50 V, the current to 1-3 A, and the treatment time to 2-10 min.

[0015] In some embodiments of the present invention, in step (2), the grafting modifier is polysilazane.

[0016] In some embodiments of the present invention, in step (2), the mass ratio of the primary modified polytetrafluoroethylene to the grafting modifier is 10:(2-3).

[0017] Preferably, in step (2), the mass ratio of the primary modified polytetrafluoroethylene to the grafting modifier is 10:2.5.

[0018] In some embodiments of the present invention, in step (3), the amount of modified fumed silica added is 0.3-1% of the mass of the secondary modified polytetrafluoroethylene.

[0019] Preferably, in step (3), the amount of modified fumed silica added is 0.6% of the mass of the secondary modified polytetrafluoroethylene.

[0020] In some embodiments of the present invention, the preparation steps of the modified fumed silica are as follows:

[0021] 1) Add water, ethanol and a modifier into a reactor, adjust the pH to 5-7, stir for 20-30 minutes, then add fumed silica, stir for 1-3 hours at room temperature, centrifuge, wash and dry to obtain pretreated fumed silica;

[0022] 2) Adding fumed silica and the pretreated fumed silica in step 1) into a reactor, stirring and mixing, thereby obtaining modified fumed silica.

[0023] In some embodiments of the present invention, in step 1), the modifier is a composite of KH-570 and hexamethyldisilazane.

[0024] Preferably, in step 1), the mass ratio of KH-570 to hexamethyldisilazane is (1-3):1.

[0025] Further preferably, in step 1), the mass ratio of KH-570 to hexamethyldisilazane is 2:1.

[0026] In some embodiments of the present invention, in step 1), the mass ratio of the modifier to the fumed silica is (1-1.5):1.

[0027] Preferably, in step 1), the mass ratio of the modifier to the fumed silica is 1.3:1.

[0028] In some embodiments of the present invention, in step 2), the mass ratio of the fumed silica to the pretreated fumed silica is 1:(0.5-1).

[0029] Preferably, in step 2), the mass ratio of the fumed silica to the pretreated fumed silica is 1:0.75.

[0030] Preferably, in step 2), the average particle size of the fumed silica is 100 to 300 nm.

[0031] Further preferably, in step 2), the average particle size of the fumed silica is 200 nm.

[0032] Among many polymers, polytetrafluoroethylene has strong comprehensive properties and is an ideal organic substrate for preparing high-performance permeable membranes. However, it has a high thermal expansion coefficient and poor resistance when encountering overheating environments. When heated, its fiber-node structure will shrink, resulting in a decrease in the comprehensive performance of the permeable membrane. When used as a permeable membrane for transformer diagnosis and analysis, its fatigue resistance is obviously insufficient and it is prone to failure.

[0033] The present invention first pre-treats polytetrafluoroethylene with plasma, then grafts it with a grafting modifier, and finally blends it with modified fumed silica to obtain a mixed solution, and obtains a permeable membrane by spin coating. The present invention introduces a grafting modifier to further improve the hydrophobicity of the permeable membrane, which accelerates the dissolution rate of the gas in the membrane during oil and gas separation; at the same time, the tolerance and dimensional stability of polytetrafluoroethylene after film formation are also effectively improved, effectively delaying the thermal shrinkage of the permeable membrane under high-pressure overheating environment. The possible reason is that the specific modified fumed silica is deposited and filled in the fiber-node structure of polytetrafluoroethylene, and the hydrophobic chain segment grafted thereon cooperates to prevent the shrinkage phenomenon.

[0034] In the field of permeable membranes, since there is always an upper limit effect between the permeability and selectivity of permeable membranes, inorganic matrices are often mixed into the preparation process of organic membranes and used as dispersed phases in order to introduce the unique advantages of inorganic particles in gas adsorption and separation, such as large flux and good mechanical strength, to solve the defects of existing organic polymer permeable membranes in this regard. However, most of the existing technologies use physical blending, and the inorganic matrix is ​​only wrapped by the polymer, and the interaction force is not strong, resulting in insufficient utilization. There is still room for improvement in the utilization effect of the inorganic matrix.

[0035] Based on this, the present invention first adds a composite modifier to hydrophobically modify the fumed silica, then blends it with the fumed silica of the same nanometer level, and then composites it with polytetrafluoroethylene. On the one hand, the poor modification effect of the commonly used modifier on the fumed silica is solved. When the addition amount increases, it still has the problem of uneven dispersion in the polymer system. At this time, the mixed fumed silica and polytetrafluoroethylene are blended to prepare a permeable membrane for oil and gas separation. When subjected to external stress impact, the fumed silica migrates and absorbs or buffers the impact energy at the same time; on the other hand, the introduction of KH-570 and hexamethyldisilazane composite modified fumed silica hinders the movement of the polytetrafluoroethylene chain to a certain extent, and jointly plays the role of toughening and enhancing the mechanical strength of the permeable membrane, and further increases the specific surface area of ​​the fumed silica, increases the volume of the amorphous region between it and the polymer, and further increases the gas flux.

[0036] Another aspect of the present invention further provides a permeable membrane for efficient oil-gas separation obtained by the above preparation method, wherein the thickness of the permeable membrane is 40-70 μm.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The present invention pre-treats polytetrafluoroethylene with plasma, grafts it with a grafting modifier, and finally blends it with modified fumed silica to obtain a mixed solution. The mixed solution is then spin-coated to obtain a permeable membrane, which can be used for analysis of dissolved gases in transformer oil to achieve efficient separation of oil and gas, and its air permeability and mechanical strength are significantly improved.

[0039] (2) The present invention introduces a grafted modifier to further improve the hydrophobicity of the permeable membrane, thereby accelerating the dissolution rate of the gas in the membrane during oil-gas separation; at the same time, the tolerance and dimensional stability of the polytetrafluoroethylene film after film formation are also effectively improved, effectively delaying the thermal shrinkage of the permeable membrane under high-pressure overheating conditions.

[0040] (3) The present invention uses a composite modifier to hydrophobically modify a specific fumed silica, blends it with fumed silica of the same nanometer level, and then composites it with polytetrafluoroethylene. On the one hand, it solves the problem that the commonly used modifiers have poor modification effects on fumed silica and that it still has uneven dispersion in the polymer system when the added amount increases; on the other hand, it plays a role in toughening and enhancing the mechanical strength of the permeable membrane; on the other hand, it increases the volume of the amorphous region between the fumed silica and the polymer, further increasing the gas flux. DETAILED DESCRIPTION

[0041] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0042] Unless otherwise specified, the reagents used below can be easily obtained from commercial companies, wherein polysilazane was purchased from Perri Technology Co., Ltd.; polytetrafluoroethylene was purchased from Dongguan Hongyu Plastic Co., Ltd.

[0043] Unless otherwise specified, the average particle size of the fumed silica used below is 200 nm.

[0044] Preparation Example 1

[0045] The preparation steps of modified fumed silica are as follows:

[0046] 1) Add 20 mL of water, 80 mL of ethanol, 4.35 g of KH-570 and 2.15 g of hexamethyldisilazane into a reactor, adjust the pH to 6, stir for 25 min, then add 5 g of fumed silica, stir for 2 h at room temperature, centrifuge, wash and dry to obtain pretreated fumed silica;

[0047] 2) 10 g of fumed silica and 7.5 g of the pretreated fumed silica prepared in step 1) were stirred and mixed to obtain modified fumed silica.

[0048] Preparation Example 2

[0049] The preparation steps of modified fumed silica are the same as those of Preparation Example 1, except that 6.5 g of KH-570 is added in step 1).

[0050] Preparation Example 3

[0051] The preparation steps of modified fumed silica are the same as those of Preparation Example 1, except that 4 g of fumed silica is added in step 1).

[0052] Preparation Example 4

[0053] The preparation steps of modified fumed silica are the same as those of Preparation Example 1, except that 11 g of pretreated fumed silica is added in step 2).

[0054] Example 1

[0055] A method for preparing a permeable membrane for efficient oil-gas separation comprises the following steps:

[0056] (1) Preparation of primary modified polytetrafluoroethylene: polytetrafluoroethylene is treated at a discharge interval of 8 mm, a discharge power of 10000 Hz, a voltage of 40 V, a current of 2 A for 6 min to obtain primary modified polytetrafluoroethylene;

[0057] (2) Preparation of secondary modified polytetrafluoroethylene: 10 g of primary modified polytetrafluoroethylene and 30 mL of n-butanol were mixed, 2.5 g of polysilazane, 1 g of ethylene glycol and 0.013 g of potassium persulfate were added, the temperature was raised to 60° C., the reaction was carried out for 3.5 h, and the secondary modified polytetrafluoroethylene was obtained after washing and drying.

[0058] (3) Preparation of permeable membrane: 50 g of secondary modified polytetrafluoroethylene and 100 mL of n-butanol were added to a reactor and stirred for 2 h. Then, 0.3 g of modified fumed silica was added and stirred for 3 h to obtain a mixed solution. The mixed solution was placed in an oven for degassing and then dripped onto a dry and smooth substrate while rotating at 500 r / min. After completion, the speed was increased to 1500 r / min and the substrate was rotated for 50 s to form a membrane. The membrane was dried at room temperature for 1 day to obtain a permeable membrane with a thickness of 55 μm.

[0059] Wherein, the modified fumed silica used in step (3) is obtained from Preparation Example 1.

[0060] Example 2

[0061] A method for preparing a permeable membrane for efficient oil-gas separation comprises the following steps:

[0062] (1) Preparation of primary modified polytetrafluoroethylene: polytetrafluoroethylene is treated at a discharge interval of 8 mm, a discharge power of 10000 Hz, a voltage of 30 V, a current of 3 A for 2 min to obtain primary modified polytetrafluoroethylene;

[0063] (2) Preparation of secondary modified polytetrafluoroethylene: 10 g of primary modified polytetrafluoroethylene and n-butanol were mixed, 2 g of polysilazane, 1 g of ethylene glycol and 0.01 g of potassium persulfate were added, the temperature was raised to 50° C., the reaction was carried out for 5 h, and the secondary modified polytetrafluoroethylene was obtained after washing and drying;

[0064] (3) Preparation of permeable membrane: 50 g of secondary modified polytetrafluoroethylene and 100 mL of n-butanol were added to a reactor and stirred for 1 h. Then, 0.15 g of modified fumed silica was added and stirred for 2 h to obtain a mixed solution. The mixed solution was placed in an oven for degassing and then dripped onto a dry and smooth substrate while rotating at 200 r / min. After completion, the speed was increased to 2000 r / min and the substrate was rotated for 30 s to form a membrane. The membrane was dried at room temperature for 1 day to obtain a permeable membrane with a thickness of 40 μm.

[0065] Wherein, the modified fumed silica used in step (3) is obtained from Preparation Example 1.

[0066] Example 3

[0067] A method for preparing a permeable membrane for efficient oil-gas separation comprises the following steps:

[0068] (1) Preparation of primary modified polytetrafluoroethylene: polytetrafluoroethylene is treated at a discharge interval of 8 mm, a discharge power of 10000 Hz, a voltage of 50 V, and a current of 1 A for 10 min to obtain primary modified polytetrafluoroethylene;

[0069] (2) Preparation of secondary modified polytetrafluoroethylene: 10 g of primary modified polytetrafluoroethylene and n-butanol were mixed, 3 g of polysilazane, 1 g of ethylene glycol and 0.015 g of potassium persulfate were added, the temperature was raised to 60° C., the reaction was carried out for 3.5 h, and the secondary modified polytetrafluoroethylene was obtained after washing and drying;

[0070] (3) Preparation of permeable membrane: 50 g of secondary modified polytetrafluoroethylene and 100 mL of n-butanol were added to a reactor and stirred for 2 h. Then, 0.5 g of modified fumed silica was added and stirred for 3 h to obtain a mixed solution. The mixed solution was placed in an oven for degassing and then dripped onto a dry and smooth substrate while rotating at 800 r / min. After completion, the speed was increased to 1000 r / min and the substrate was rotated for 1 min to form a membrane. The membrane was dried at room temperature for 1 day to obtain a permeable membrane with a thickness of 70 μm.

[0071] Wherein, the modified fumed silica used in step (3) is obtained from Preparation Example 1.

[0072] Example 4

[0073] A method for preparing a permeable membrane for efficient oil-gas separation, the specific implementation method is the same as Example 1, except that the modified fumed silica used in step (3) is obtained from Preparation Example 2.

[0074] Example 5

[0075] A method for preparing a permeable membrane for efficient oil-gas separation, the specific implementation method is the same as Example 1, except that the modified fumed silica used in step (3) is obtained from Preparation Example 3.

[0076] Example 6

[0077] A method for preparing a permeable membrane for efficient oil-gas separation, the specific implementation method is the same as Example 1, except that the modified fumed silica used in step (3) is obtained from Preparation Example 4.

[0078] Example 7

[0079] A method for preparing a permeable membrane for efficient oil and gas separation, the specific implementation method is the same as that of Example 1, except that the amount of polysilazane added in step (2) is 3.5 g.

[0080] Example 8

[0081] A method for preparing a permeable membrane for efficient oil-gas separation, the specific implementation method is the same as that of Example 1, except that the amount of modified fumed silica added in step (3) is 0.6 g.

[0082] Comparative Example 1

[0083] A method for preparing a permeable membrane for efficient oil-gas separation, the specific implementation method is the same as that of Example 1, except that 0.3 g of fumed silica is added in step (3) to replace 0.3 g of modified fumed silica.

[0084] Comparative Example 2

[0085] A method for preparing a permeable membrane for efficient oil-gas separation comprises the following steps:

[0086] Add 50g of polytetrafluoroethylene and 100mL of n-butanol into the reactor, stir and mix for 2h, then add 0.3g of modified fumed silica, stir and mix for 3h to obtain a mixed solution, place the mixed solution in an oven for degassing, and then drip the glue on a dry and smooth substrate while rotating at a speed of 500r / min. After completion, increase the speed to 1500r / min and rotate for 50s to form a film, and dry it at room temperature for 1d to obtain a permeable membrane with a thickness of 55μm.

[0087] The modified fumed silica used is obtained from Preparation Example 1.

[0088] Performance Testing:

[0089] The permeable membranes prepared in the above Examples 1-8 and Comparative Examples 1-2 were subjected to the following performance tests:

[0090] (1) Mechanical strength performance test-1: Use a metal hollow plate frame to fix each permeable membrane and seal it on the side wall of the oil chamber top space along the circumferential direction. Each permeable membrane and the oil chamber top space form an air chamber. Fill the oil chamber below the metal hollow plate frame with insulating oil. The front port of the oil chamber is sealed and connected to the gas cylinder. The pressure valve of the gas cylinder is adjusted to 500 kPa and maintained for 48 hours. Check whether each permeable membrane has cracks, oil leakage or layer separation. The specific test results are shown in Table 1:

[0091] (2) Mechanical strength performance test-2: According to standard GB / T 1040, each permeable membrane was cut into strip specimens of 5 cm×1 cm, and a tensile strength test was performed using a CMT6104 electronic universal testing machine, wherein the tensile rate was set to 10 mm / min.

[0092] (3) Air permeability test: The air permeability of the permeable membrane was tested by the differential pressure method. Nitrogen and liquefied gas were mixed in a mixing tank at a volume ratio of 80:20 as the inlet gas and passed through a membrane assembly containing each permeable membrane at room temperature. The inlet pressure in the mixing tank was set to be maintained at 0.4 MPa. A soap bubble flowmeter was connected to the other side of the membrane assembly to test the gas flow rate to characterize the air permeability of the permeable membrane.

[0093] Table 1

[0094]

[0095]

[0096] As can be seen from Table 1, the permeable membranes disclosed in Examples 1-3 of the present invention have excellent performance in terms of air permeability and mechanical strength;

[0097] By comparing Examples 4 and 5 with Example 1, it can be seen that when the amount of KH-570 and fumed silica added in step 1) is changed respectively when preparing the modified fumed silica, the mechanical strength of the permeable membrane will be greatly reduced;

[0098] By comparing Example 6 with Example 1, it can be seen that when the amount of pretreated fumed silica added in step 2) is changed during the preparation of modified fumed silica, the air permeability and mechanical strength of the permeable membrane will deteriorate to varying degrees;

[0099] By comparing Example 7 with Example 1, it can be seen that when the amount of polysilazane added in step (2) of the preparation method is changed, the air permeability of the permeable membrane will deteriorate, which may be caused by the weakening of the dissolution diffusion effect;

[0100] By comparing Example 8 with Example 1, it can be seen that when the amount of modified fumed silica added in step (3) of the preparation method is changed, the mechanical strength of the permeable membrane will decrease due to the agglomeration effect;

[0101] From the comparison between Comparative Example 1 and Example 1, it can be seen that when the modified fumed silica is replaced by an equal amount of fumed silica in step (3) of the preparation method, the mechanical strength of the permeable membrane is greatly affected, the brittleness thereof is increased, and the interaction force between the components of the system is reduced, resulting in poor air permeability.

[0102] From the comparison between Comparative Example 2 and Example 1, it can be seen that when unmodified polytetrafluoroethylene is directly added during the preparation of the permeable membrane, the mechanical strength of the permeable membrane will decrease, and oil leakage and layer separation will occur.

[0103] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a high-efficiency oil-gas separation permeable membrane, characterized in that: The following steps are involved: (1) Preparation of primary modified polytetrafluoroethylene: polytetrafluoroethylene is pretreated with plasma to obtain primary modified polytetrafluoroethylene; (2) Preparation of secondary modified polytetrafluoroethylene: Mix the primary modified polytetrafluoroethylene and an organic solvent, add a grafting modifier, a crosslinking agent and an initiator, heat to 50-70°C, react for 2-5 hours, wash and dry to obtain the secondary modified polytetrafluoroethylene; (3) Preparation of permeable membrane: Add secondary modified polytetrafluoroethylene and organic solvent into a reactor, stir and mix for 1 to 3 hours, then add modified fumed silica, stir and mix for 2 to 4 hours to obtain a mixed solution, place the mixed solution in an oven for degassing, and then spin-coat the mixed solution onto a dry and smooth substrate to form a film, and dry at room temperature to obtain the permeable membrane.

2. The method for preparing a permeable membrane for efficient oil-gas separation according to claim 1, characterized in that: In step (1), the plasma pretreatment is performed by setting the discharge interval to 8 mm, the discharge power to 10000 Hz, the voltage to 30-50 V, the current to 1-3 A, and the treatment time to 2-10 min.

3. The method for preparing a permeable membrane for efficient oil-gas separation according to claim 1, characterized in that: In step (2), the grafting modifier is polysilazane.

4. The method for preparing a permeable membrane for efficient oil-gas separation according to claim 1, characterized in that: In step (2), the mass ratio of the primary modified polytetrafluoroethylene to the grafting modifier is 10:(2-3).

5. The method for preparing a permeable membrane for efficient oil-gas separation according to claim 1, characterized in that: In step (3), the amount of modified fumed silica added is 0.3 to 1% of the mass of the secondary modified polytetrafluoroethylene.

6. The method for preparing a permeable membrane for efficient oil-gas separation according to claim 1, characterized in that: The preparation steps of the modified fumed silica are as follows: 1) Add water, ethanol and a modifier into a reactor, adjust the pH to 5-7, stir for 20-30 minutes, then add fumed silica, stir for 1-3 hours at room temperature, centrifuge, wash and dry to obtain pretreated fumed silica; 2) The fumed silica and the pretreated fumed silica in step 1) are stirred and mixed to obtain modified fumed silica.

7. The method for preparing a permeable membrane for efficient oil-gas separation according to claim 6, characterized in that: In step 1), the modifier is a composite of KH-570 and hexamethyldisilazane.

8. The method for preparing a permeable membrane for efficient oil-gas separation according to claim 6, characterized in that: In step 1), the mass ratio of the modifier to the fumed silica is (1-1.5):

1.

9. A permeable membrane for efficient oil-gas separation obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The thickness of the permeable membrane is 40-70 μm.

10. Use of the permeable membrane obtained by the preparation method according to any one of claims 1 to 8 or the permeable membrane according to claim 9 in the field of analysis of dissolved gases in transformer oil.

Citation Information

Patent Citations

  • Oil-gas separation membrane for on-line detection of transformer and preparation method of oil-gas separation membrane

    CN116328550A

  • Preparation method of strong-stability anti-pollution composite nanofiltration membrane

    CN111298660A

  • Hydrophobic PVDF membrane, and preparation method and application thereof

    CN113248780A

  • Preparation method of modified fumed silica

    CN116606559A

  • Hydrophilic polytetrafluoroethylene microporous membrane as well as preparation method and application thereof

    CN117959943A