Preparation method of submicron / nanometer sphere-like rare earth fluoride
By using rare earth salt, hydrogen fluoride and ammonia water in ethanol or ethylene glycol solvents, the reaction conditions are controlled, and the preparation of submicro/nano spherical fluorinated rare earths without modifications is achieved, and the uneven particle size and agglomeration in the prior art are solved. In the problem, rare earth fluoride with high dispersion and uniform particle size was obtained.
Patent Information
- Application Number
- CN202411223328.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure CN119080046A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earth material preparation, and in particular to a method for preparing submicron / nano-like spherical rare earth fluoride. Background Art
[0002] Submicron powder and nano powder of rare earth compounds are one of the most popular new materials. It is not only a new material, but also can be used as a raw material for preparing new materials. Among them, rare earth fluorides have broad application prospects in many fields due to their unique electrical, optical and magnetic properties. At present, the commonly used synthesis methods for rare earth fluorides include solid phase synthesis, hydrothermal and solvothermal methods, precipitation, pyrolysis, gel-sol method, solvent volatilization method, etc. The direct precipitation method of solution is an effective method for preparing small-particle powders. It is simple to operate, low in cost, and suitable for mass production, but it is not easy to control the precipitated particle size.
[0003] As we all know, due to RE 3+ 、F - The low solubility in ethanol and ethylene glycol, the high viscosity of the solvents, and the controllable ion diffusion rates all make these solvents proven to be effective solvents in aiding the nucleation and growth rates of nanoparticles.
[0004] Jan W. Stouwdam et al. used Re 3+ With F - The coprecipitation of LaF3:Ln (Ln = Eu, Er, Nd, Ho) nanoparticles less than 10nm were prepared at 75℃ in an ethanol-water system. Tao Xiaojun et al. added a certain amount of dioctadecyloxy dithiophosphate pyridinium salt and sodium fluoride to a water-alcohol mixed medium, and prepared LaF3 nanoparticles modified with organic compounds by the same cation coprecipitation surface modification method. Wu Zhishen et al. added octadecyloxy dithiophosphate pyridinium salt and sodium fluoride to an alcohol-water mixed solvent and prepared nano CeF3 by chemical modification. In summary, in the synthesis process of the small-particle rare earth fluorides reported so far, in addition to using organic solvents as the liquid phase system, a large amount of organic additives and inorganic salts are used to modify the surface of the rare earth fluoride particles to control the particle size.
[0005] Therefore, providing a method for preparing submicron / nano-spherical rare earth fluoride without adding other substances for modification is of great significance to the technical field of rare earth fluoride preparation. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing submicron / nano-like spherical rare earth fluoride. The method can obtain submicron / nano-like spherical rare earth fluoride without adding other substances for modification.
[0007] To achieve the above object, the present invention provides the following solutions:
[0008] One of the technical solutions of the present invention is a method for preparing submicron / nano-like spherical rare earth fluoride, comprising the following steps:
[0009] Adding the rare earth salt solution and the precipitant solution into the organic solvent simultaneously for reaction to obtain the submicron / nano-spherical rare earth fluoride;
[0010] The precipitant solution includes hydrogen fluoride and aqueous ammonia.
[0011] The second technical solution of the present invention is a submicron / nano-spherical rare earth fluoride prepared by the above-mentioned preparation method.
[0012] The third technical solution of the present invention is the use of the above-mentioned submicron / nano-spherical rare earth fluoride in the preparation of optical materials or electronic materials.
[0013] The present invention discloses the following technical effects:
[0014] The method of the present invention can prepare spherical small-size (submicron and nanometer) rare earth fluoride rare earth fluoride with a size distribution of 20nm to 300nm. The method only needs to be carried out in an organic solvent (ethanol or ethylene glycol) system without adding other substances for modification.
[0015] The invention adopts rare earth salt (rare earth chloride, rare earth nitrate or rare earth sulfate), hydrogen fluoride and ammonia water as raw materials, and carries out reaction in ethanol or ethylene glycol organic polar solvent. By controlling the concentration and acidity of rare earth salt solution, the use of organic solvent and the reaction temperature, micro / nano-scale rare earth fluoride with uniform particle size distribution, good dispersibility and less agglomeration is finally obtained.
[0016] The method of the invention is simple, low in cost and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 is a SEM image of lanthanum fluoride prepared in Example 1;
[0019] Figure 2 is a SEM image of samarium fluoride prepared in Example 2;
[0020] Figure 3 This is a SEM image of praseodymium fluoride prepared in Example 3;
[0021] Figure 4 is a SEM image of lanthanum fluoride prepared in Example 4;
[0022] Figure 5 is a SEM image of lanthanum fluoride prepared in Example 5;
[0023] Figure 6 This is a SEM image of the cerium fluoride prepared in Example 6;
[0024] Figure 7 This is the SEM image of lanthanum fluoride prepared in Example 7. DETAILED DESCRIPTION
[0025] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0026] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0027] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0028] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0029] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0030] The first aspect of the present invention provides a method for preparing submicron / nano-like spherical rare earth fluoride, comprising the following steps:
[0031] Adding the rare earth salt solution and the precipitant solution into the organic solvent simultaneously for reaction to obtain the submicron / nano-spherical rare earth fluoride;
[0032] The precipitant solution includes hydrogen fluoride and aqueous ammonia.
[0033] In some embodiments of the present invention, the rare earth salt in the rare earth salt solution is one of rare earth chloride, rare earth nitrate, and rare earth sulfate; the rare earth in the rare earth salt solution is one of lanthanum, cerium, praseodymium, neodymium, samarium, and europium; the concentration of the rare earth salt solution is 0.3 to 1.8 mol / L, and the pH is 2 to 4. More preferably, the concentration of the rare earth salt solution is 0.75 to 1.5 mol / L.
[0034] The concentration and pH of the rare earth salt solution are limited to the above parameter ranges: in order to control the pH of the reaction system to be acidic, and there is ammonia water in the precipitant solution. If the pH is too low, a large amount of ammonia water will be consumed, which is not conducive to control. If the pH is too high, the generated particles will be relatively large, which is not conducive to control below the micron level.
[0035] In some embodiments of the present invention, the molar ratio of the hydrogen fluoride to the ammonia water is 1:0.6-1.0, and more preferably 1:0.6-0.8; the pH of the precipitant solution is 3-4.
[0036] The reason why the molar ratio of hydrogen fluoride to ammonia water is limited to 1:0.6 to 1.0 in the present invention is as follows: exceeding the above range will affect the rare earth yield, F - Excessive use will increase the acid effect and complexing effect (generating REF4 - ) and salt effect (F - and NH4 + Forming electrolyte) increases the solubility of REF3; NH4 + Excessive dosage will result in incomplete fluoridation
[0037] In some embodiments of the present invention, the organic solvent is an ethanol solution or an ethylene glycol solution.
[0038] In some embodiments of the present invention, the volume ratio of the organic solvent to the rare earth salt solution is 15 to 40:100, preferably 20 to 30:100.
[0039] In some embodiments of the present invention, the RE in the rare earth salt solution 3+ With the F in the precipitant solution - The molar ratio is 1:3.
[0040] In some embodiments of the present invention, the reaction temperature is 20-90°C, and the reaction time is 0.5-3.0 hours. More preferably, the reaction temperature is 40-60°C, and the reaction time is 1-1.5 hours.
[0041] If the reaction time is too short, it will not be conducive to the complete reaction. If the reaction time is too long, the particles will grow larger and it will be impossible to obtain submicron / nano particles.
[0042] In some embodiments of the present invention, during the reaction, the pH of the reaction system is less than 4, and the pH at the reaction endpoint is 1-2.
[0043] When the pH of the reaction system exceeds 4 during the reaction, the rare earth fluoride particles generated after the reaction are relatively large. The pH of the reaction end point is 1-2 in order to ensure the highest rare earth yield.
[0044] Due to the presence of ethanol and ethylene glycol organic polar solvents, the fluoride is coated by the organic solvent during the nucleation process, reducing the surface free energy of the crystal nucleus, and diffuses and distributes in the liquid around the particles to form a double electric layer, which hinders the agglomeration of nanoparticles through Coulomb repulsion. At the same time, the use of organic solvents for washing during the washing process is aimed at inhibiting the agglomeration of particles. Secondly, the temperature of the reaction process is controlled at 40 to 60°C. In this relatively low temperature range, the crystal nucleation rate is high, the nucleation rate is fast, and the grain growth rate is slow, which is more conducive to obtaining fine grains. In summary, in the precipitation and post-treatment process of the present invention, the presence of organic solvents reduces the surface energy between particles, and finally obtains submicron / nano fluorinated rare earth with good dispersibility and less agglomeration.
[0045] In some embodiments of the present invention, after the reaction is completed, the steps of centrifugal separation, washing and drying are further included. The washing is specifically washing with water and washing with alcohol alternately until the pH of the last washing liquid is greater than 6. The drying temperature is 50-70°C, more preferably 55-65°C.
[0046] The second aspect of the present invention provides a submicron / nano-spherical rare earth fluoride prepared by the above-mentioned preparation method.
[0047] The third aspect of the present invention provides an application of the above-mentioned submicron / nano-like spherical rare earth fluoride in the preparation of optical materials or electronic materials.
[0048] The test method involved in the embodiment of the present invention is as follows:
[0049] Morphology characterization: Sigma-500 scanning electron microscope (FESEM) was used for characterization. Before the test, the sample was first dried at 60°C for 1 hour, and then used for test sample preparation. First, conductive glue was pasted on the sample stage, a small amount of dry sample was taken on the conductive glue, and the excess sample outside the conductive glue was blown off with an ear-cleaning bulb. Then, the sample stage was gold-sprayed on an ion sputtering coating instrument (30 to 90 seconds) to increase the conductivity of the sample. After the gold plating was completed, a test voltage of 10kV was selected, and the sample stage was placed in the sample chamber for observation and imaging.
[0050] Unless otherwise specified, the raw materials and reagents used in the examples of the present invention can be obtained through commercial sources.
[0051] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0052] Example 1
[0053] Take 60 mL of ethanol as the base liquid (solvent), prepare a lanthanum chloride solution with a concentration of 0.7674 mol / L, and use hydrochloric acid solution to adjust the pH value to 3.1±0.2.
[0054] Preparation F - The concentration of the precipitant solution is 2.3022 mol / L, and the precipitant solution is a mixed solution of hydrofluoric acid (mass concentration 40%) and ammonia water, wherein the amount of ammonia water added is such that the pH value of the precipitant solution is adjusted to 3.6±0.2.
[0055] The prepared lanthanum chloride solution and precipitant solution were mixed according to RE 3+ With F - The molar ratio is 1:3 and two peristaltic pumps are used to inject anhydrous ethanol, the reaction temperature (water bath heating) is controlled to be 40°C, and the reaction is carried out for 1 hour. After the reaction is completed, the slurry is centrifuged, washed with water and alcohol alternately until the pH of the last washing solution is greater than 6, and then dried at 50°C to obtain nano-lanthanum fluoride, which is a nano-cluster with a particle size between 55nm and 60nm. Figure 1 shown.
[0056] Example 2
[0057] Take 60 mL of ethanol as the base liquid, prepare a samarium chloride solution with a concentration of 0.7740 mol / L, and use hydrochloric acid solution to adjust the pH value to 2.4±0.2.
[0058] Preparation F - The concentration of the precipitant solution is 2.3228 mol / L, and the precipitant solution is a mixed solution of hydrofluoric acid (mass concentration 40%) and ammonia water, wherein the amount of ammonia water added is such that the pH value of the precipitant solution is adjusted to 3.3±0.2.
[0059] The prepared samarium chloride solution and precipitant solution were mixed according to RE 3+ With F - The molar ratio is 1:3 and injected into anhydrous ethanol using two peristaltic pumps respectively. The reaction temperature (water bath heating) is controlled to be 30°C and the reaction is carried out for 1 hour. After the reaction is completed, the slurry is centrifuged, washed with water and alcohol alternately until the pH of the last washing solution is greater than 6, and then dried at 50°C to obtain submicron samarium fluoride, which is flat round small particles, partially agglomerated, and the particle size is between 150nm and 260nm. Figure 2 shown.
[0060] Example 3
[0061] Take 60 mL of ethanol as the base liquid, prepare a 0.8168 mol / L praseodymium chloride solution, and use hydrochloric acid solution to adjust the pH value to 3.2±0.2.
[0062] Preparation F - The concentration of the precipitant solution is 2.4504 mol / L, and the precipitant solution is a mixed solution of hydrofluoric acid (mass concentration 40%) and ammonia water, wherein the amount of ammonia water added is such that the pH value of the precipitant solution is adjusted to 3.5±0.2.
[0063] The prepared praseodymium chloride solution and precipitant solution were mixed according to RE 3+ With F - The molar ratio is 1:3 and injected into anhydrous ethanol using two peristaltic pumps respectively, and the reaction temperature (water bath heating) is controlled to be 40°C. The reaction is carried out for 1 hour. After the reaction is completed, the slurry is centrifuged, washed with water and alcohol alternately until the pH of the last washing solution is greater than 6, and then dried at 50°C to obtain nano-praseodymium fluoride, which is a mixture of spherical small particles and clusters with a particle size between 90nm and 140nm. Figure 3 shown.
[0064] Example 4
[0065] Take 60 mL of ethanol as the base liquid, prepare a lanthanum nitrate solution with a concentration of 0.7620 mol / L, and use nitric acid solution to adjust the pH value to 2.9±0.2.
[0066] Preparation F - The concentration of the precipitant solution is 2.2860 mol / L, and the precipitant solution is a mixed solution of hydrofluoric acid (mass concentration is 40%) and ammonia water, wherein the amount of ammonia water added is to adjust the pH value of the precipitant solution to 3.7±0.2.
[0067] The prepared lanthanum chloride solution and precipitant solution were mixed according to RE 3+ With F -The molar ratio is 1:3 and injected into anhydrous ethanol using two peristaltic pumps respectively, and the reaction temperature (water bath heating) is controlled to be 60°C. The reaction is carried out for 1 hour. After the reaction is completed, the slurry is centrifuged, washed with water and alcohol alternately until the pH of the last washing solution is greater than 6, and then dried at 50°C to obtain nano-lanthanum fluoride, which is a mixture of spherical small particles and clusters with a particle size between 60nm and 110nm. Figure 4 shown.
[0068] Example 5
[0069] Take 60 mL of ethylene glycol as the base liquid, prepare a 0.7620 mol / L lanthanum chloride solution, and use hydrochloric acid solution to adjust the pH value to 3.3±0.2.
[0070] Preparation F - The concentration of the precipitant solution is 2.2860 mol / L, and the precipitant solution is a mixed solution of hydrofluoric acid (mass concentration is 40%) and ammonia water, wherein the amount of ammonia water added is to adjust the pH value of the precipitant solution to 3.2±0.2.
[0071] The prepared lanthanum chloride solution and precipitant solution were mixed according to RE 3+ With F - The molar ratio is 1:3 and two peristaltic pumps are used to inject anhydrous ethylene glycol, the reaction temperature (water bath heating) is controlled to be 40°C, and the reaction is carried out for 1 hour. After the reaction is completed, the slurry is centrifuged, washed with water, and washed with alcohol alternately until the pH of the last washing liquid is greater than 6, and then dried at 50°C to obtain nano-lanthanum fluoride, which is a mixture of spherical small particles and nano-clusters with a particle size between 20nm and 30nm. Figure 5 shown.
[0072] Example 6
[0073] Take 60 mL of ethanol as the base liquid, prepare a 0.7500 mol / L cerium chloride solution, and use hydrochloric acid solution to adjust the pH value to 3.0±0.2.
[0074] Preparation F - The concentration of the precipitant solution is 2.2500 mol / L, and the precipitant solution is a mixed solution of hydrofluoric acid (mass concentration is 40%) and ammonia water, wherein the amount of ammonia water added is to adjust the pH value of the precipitant solution to 3.5±0.2.
[0075] The prepared cerium chloride solution and precipitant solution were mixed according to RE 3+ With F -The molar ratio is 1:3 and injected into anhydrous ethanol using two peristaltic pumps respectively, and the reaction temperature (water bath heating) is controlled to be 40°C. The reaction is carried out for 1 hour. After the reaction is completed, the slurry is centrifuged, washed with water, and washed with alcohol alternately until the pH of the last washing liquid is greater than 6, and then dried at 50°C to obtain nano-cerium fluoride, which is a mixture of spherical small particles and nano-clusters with a particle size between 40nm and 55nm. Figure 6 shown.
[0076] Example 7
[0077] Take 45 mL of ethanol as the base liquid, prepare a 0.7839 mol / L lanthanum chloride solution, and use hydrochloric acid solution to adjust the pH value to 2.4±0.2.
[0078] Preparation F - The concentration of the precipitant solution is 2.3517 mol / L, and the precipitant solution is a mixed solution of hydrofluoric acid (mass concentration is 40%) and ammonia water, wherein the amount of ammonia water added is to adjust the pH value of the precipitant solution to 3.2±0.2.
[0079] The prepared lanthanum chloride solution and precipitant solution were mixed according to RE 3+ With F - The molar ratio is 1:3 and injected into anhydrous ethanol using two peristaltic pumps respectively, and the reaction temperature (water bath heating) is controlled to be 40°C. The reaction is carried out for 1 hour. After the reaction is completed, the slurry is centrifuged, washed with water, and washed with alcohol alternately until the pH of the last washing liquid is greater than 6, and then dried at 50°C to obtain nano-lanthanum fluoride, which is a mixture of spherical small particles and nano-clusters with a particle size between 50nm and 90nm. Figure 7 shown.
[0080] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing submicron / nano-spherical rare earth fluoride, characterized in that: The following steps are involved: Adding the rare earth salt solution and the precipitant solution into the organic solvent simultaneously for reaction to obtain the submicron / nano-spherical rare earth fluoride; The precipitant solution includes hydrogen fluoride and aqueous ammonia.
2. The method for preparing submicron / nano-like spherical rare earth fluoride according to claim 1, characterized in that: The rare earth salt in the rare earth salt solution is one of rare earth chloride, rare earth nitrate and rare earth sulfate; the rare earth in the rare earth salt solution is one of lanthanum, cerium, praseodymium, neodymium, samarium and europium; the concentration of the rare earth salt solution is 0.3-1.8 mol / L, and the pH is 2-4.
3. The method for preparing submicron / nano-like spherical rare earth fluoride according to claim 1, characterized in that: The molar ratio of the hydrogen fluoride to the ammonia water is 1:0.6-1.0; the pH of the precipitant solution is 3-4.
4. The method for preparing submicron / nano-like spherical rare earth fluoride according to claim 1, characterized in that: The organic solvent is an ethanol solution or an ethylene glycol solution.
5. The method for preparing submicron / nano-like spherical rare earth fluoride according to claim 1, characterized in that: The RE in the rare earth salt solution 3+ The F in the precipitant solution - The molar ratio is 1:
3.
6. The method for preparing submicron / nano-like spherical rare earth fluoride according to claim 1, characterized in that: The reaction temperature is 20-90° C. and the reaction time is 0.5-3.0 h.
7. The method for preparing submicron / nano-like spherical rare earth fluoride according to claim 1, characterized in that: During the reaction, the pH of the reaction system is less than 4, and the pH at the reaction end point is 1-2.
8. The method for preparing submicron / nano-like spherical rare earth fluoride according to claim 1, characterized in that: After the reaction is completed, the steps of centrifugal separation, washing and drying are also included.
9. A submicron / nano-spherical rare earth fluoride prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the submicron / nano-spherical rare earth fluoride as claimed in claim 9 in the preparation of optical materials or electronic materials.
Citation Information
Patent Citations
Method for preparing composite rare-earth fluoride nano hollow sphere
CN101386422A
Method for preparing rare earth doped lanthanum fluoride luminous hollow nano powder by using multi-element solvothermal method
CN102093892A
Method for synthesizing amino functionalized rare earth-doped lanthanum fluoride nano fluorescent marker material
CN102676171A
Cerium fluoride material, rare earth ion-doped cerium fluoride material as well as preparation method and application thereof
CN104556192A
Method for preparing rare earth fluoride nanoparticles
US20120164049A1