Lignin-based carbon fiber composite material with high tensile strength as well as preparation method and application thereof
The lignin-based carbon fiber prepared by electrospinning and segmented thermal stability treatment combined with blending and curing technology solves the problem of low tensile strength of lignin-based carbon fibers, achieving efficient carbon fiber structural optimization and mechanical performance improvement. Suitable for a variety of industry applications.
Patent Information
- Application Number
- CN202411196732.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, the tensile strength of lignin-based carbon fibers is low and the synthesis steps are complicated, and the interface adhesion between the polyacrylonitrile-based carbon nanofiber and the epoxy resin is insufficient, resulting in the mechanical properties not reaching the optimal level.
Preparation of lignin-based carbon fiber precursors by electrospinning lignin and polyacrylonitrile solutions at room temperature, and undergoing segmented heating and thermal stability and quenching treatment, followed by carbonization under a nitrogen atmosphere, and finally with dichloromethane and E51 epoxy resin , 4,4-diaminodiphenylmethane blended and cured to prepare lignin-based carbon fiber composite material with high tensile strength.
It improves the tensile strength of lignin-based carbon fibers, has a dense material structure, uniform fiber diameter, and carbon fibers produced after thermal stability and carbonization have good tensile strength and modulus, and has low raw material cost and good structural stability. It is suitable for wind energy, aerospace and automotive fields.
Smart Images

Figure BDA0005016650510000101 
Figure BDA0005016650510000111 
Figure BDA0005016650510000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrostatic spinning carbon fiber composite materials, and particularly relates to a lignin-based carbon fiber composite material with high tensile strength, and a preparation method and application thereof. Background Art
[0002] As fossil energy is increasingly depleted and environmental pollution is increasing, people have begun to pay attention to finding sustainable alternative raw materials for key petrochemical products. In this context, it is crucial to develop effective ways to convert biomass into valuable chemicals and materials. Carbon fiber has the advantages of high modulus and high strength and is widely used in many industries such as aerospace, aircraft, automobiles, sports and medical equipment. Common precursors for the production of carbon fiber include polyacrylonitrile, petroleum asphalt and regenerated cellulose. Today, nearly 91% of carbon fiber is made from polyacrylonitrile. The cost of carbon fiber precursors prepared using polyacrylonitrile as raw material is as high as 51%. Lignin is the second largest natural polymer material after cellulose in terms of reserves. It contains a large number of aromatic ring structures and can be used as a precursor to prepare carbon fiber. The production cost is more than 50% lower than that of polyacrylonitrile-based carbon fiber. Lignin materials can be obtained from agricultural waste and pulp industry waste, with significant low cost and sustainable advantages.
[0003] Lignin contains aromatic and phenolic groups, making it suitable as a carbon precursor. Electrospinning technology has the characteristics of simple synthesis requirements, easy control, and low price. By adjusting and controlling the process parameters of electrospinning, a series of one-dimensional nanofibrous materials with different diameters and lengths can be prepared. Electrospinning is a simple and versatile technique that involves the use of an electric field to generate a fine jet of polymer solution or melt, which is then collected on a grounded substrate to form a fiber mat. The resulting nanofibers have a high surface area to volume ratio, making them ideal for a variety of applications. The carbon fiber reinforced epoxy resin material prepared by compounding it with epoxy resin has high stiffness, excellent damping properties and significant tensile resistance, and is an important lightweight material. However, due to the presence of inert non-polar compounds on the surface of polyacrylonitrile-based carbon nanofibers (CNTs), traditional combinations of CNT-reinforced epoxy resins (EPs) usually face low interfacial adhesion between CNTs and EPs, and therefore, the mechanical properties cannot reach the optimal level. To solve this problem, it is imperative to develop sizing agents that can enhance the interfacial compatibility of CNT / EP. The combination of bio-based materials and nanomaterials is a viable strategy for the synthesis of sizing agents. In general, lignin is a biopolymer with a three-dimensional network structure that is rich in aromatic rings, aliphatic and hydroxyl reactive groups. Its phenolic hydroxyl and hydroxyl groups can be easily modified to achieve functionality and applicability. In addition, 3D lignin and 1DCNT can act as sizing agents to enhance interfacial interactions. In addition, the benzene rings of lignin and the hexavalent carbon of CNT can produce π-π conjugation on the CF surface, promoting the uniform dispersion of CNT on the lignin CF surface, thereby satisfying the nano-effect required for strengthening. Therefore, lignin can be an ideal raw material for environmental protection, utilizing its abundant benzene rings and the hexavalent carbon of CNT to carry out π-π conjugation on the CF surface to enhance the interfacial adhesion between CF and CNT, thereby enhancing the tensile strength of the material. Summary of the invention
[0004] In order to solve the shortcomings and deficiencies of the above-mentioned prior art, such as low tensile strength of lignin-based carbon fibers and complicated synthesis steps, the primary purpose of the present invention is to provide a method for preparing a lignin-based carbon fiber composite material with high tensile strength; the method comprises preparing a lignin-based carbon fiber precursor by electrospinning lignin and polyacrylonitrile solution at room temperature, and then subjecting the obtained lignin-based carbon fiber precursor to thermal stabilization by stepwise heating in a muffle furnace and then quenching; then carbonizing the quenched fibers under a nitrogen atmosphere to obtain a lignin-based carbon fiber material; finally, the carbonized lignin-based carbon fiber material is blended with dichloromethane, E51 epoxy resin, and 4,4-diaminodiphenylmethane to obtain a lignin-based carbon fiber composite material after curing.
[0005] Another object of the present invention is to provide a lignin-based carbon fiber composite material with high tensile strength prepared by the above preparation method.
[0006] Another object of the present invention is to provide an application of the above-mentioned lignin-based carbon fiber composite material with high tensile strength.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A method for preparing a lignin-based carbon fiber composite material with high tensile strength comprises the following steps:
[0009] (1) adding lignin and polyacrylonitrile to N,N-dimethylformamide and stirring to obtain a uniform spinning solution;
[0010] (2) electrospinning the spinning solution obtained in step (1), followed by vacuum drying to obtain a lignin-based carbon fiber precursor;
[0011] (3) The lignin-based carbon fiber precursor obtained in step (2) is subjected to the following stepwise heating and thermal stabilization in an air atmosphere in a muffle furnace: heating to 230°C at a rate of 0.5-3°C / min and thermally stabilizing for 2h, then heating to 250°C at a rate of 0.5-3°C / min and thermally stabilizing for 2h, and then heating to 280°C at a rate of 0.5-3°C / min and thermally stabilizing for 2h; after the thermal stabilization is completed, quenching is immediately performed until it is cooled to room temperature;
[0012] (4) heating to 600-1500° C. for carbonization to obtain lignin-based carbon fibers;
[0013] (5) The lignin-based carbon fiber obtained in step (4) is mixed and cured with E51 epoxy resin, dichloromethane, and 4,4-diaminodiphenylmethane to obtain a lignin-based carbon fiber composite material with high tensile strength.
[0014] The mass volume ratio of lignin to N,N-dimethylformamide in step (1) is 0.01-0.2 g:1 mL, more preferably 0.17 g:1 mL; the mass volume ratio of polyacrylonitrile to N,N-dimethylformamide is 0.01-0.2 g:1 mL, more preferably 0.17 g:1 mL.
[0015] The stirring time in step (1) is 1-72h, more preferably 12h, and the temperature is 20-80°C, more preferably 30°C; the vacuum drying temperature in step (2) is 60-90°C, more preferably 60°C, and the time is 1-120h, more preferably 12h.
[0016] The conditions for the electrospinning in step (2) are: voltage of 10-20 kV, distance between the needle and the aluminum disk of 10-20 cm, and solution feed rate of 0.1-0.5 mL / h.
[0017] The heating rate in step (4) is 2-8°C / min; the carbonization time is 1-3h; and the carbonization is carried out under a protective gas atmosphere.
[0018] The protective gas is one or more of helium, argon, nitrogen and carbon dioxide.
[0019] The lignin-based carbon fiber in step (5) is ground into powder, and the dispersion area in the mold is 0.01-2mm 2 , and then compounded with dichloromethane, E51 epoxy resin, and 4,4-diaminodiphenylmethane.
[0020] In step (5), the mass ratio of the lignin-based carbon fiber to the E51 epoxy resin is 0.1-0.25:1; the mass volume ratio of the E51 epoxy resin to dichloromethane is 2-10 g:1-5 mL; and the mass ratio of the lignin-based carbon fiber to 4,4-diaminodiphenylmethane is 0.1-2.5:1.
[0021] The mass fraction of the lignin-based carbon fiber in the lignin-based carbon fiber composite material in step (5) is 0.5wt%, and the effect is best at this time.
[0022] The co-mixing and curing in step (5) specifically includes the following steps:
[0023] First, weigh E51 epoxy resin (EP) in a glass beaker. To ensure that as little EP as possible remains on the wall of the beaker, the epoxy resin can be heated in a water bath not exceeding 45°C (the most suitable temperature is 42°C) to increase its fluidity. Then, dichloromethane (DCM) is added to the curing agent 4,4'-diaminodiphenylmethane (DDM), and heated and stirred in a water bath not exceeding 45°C (the most suitable temperature is 42°C) until the particles are completely dissolved and the solution is transparent and clear. At this time, the bubbles generated by stirring should be minimized to obtain a mixed solution. Finally, the mixed solution is added to the heated EP mentioned above, and stirred rapidly in a water bath to mix thoroughly until it becomes a slightly viscous transparent liquid. Then, it is molded in a vacuum dryer (T≤40°C) to expel most of the bubbles. Finally, it is cured in a drying oven to obtain a lignin-based carbon fiber composite material with high tensile strength.
[0024] A lignin-based carbon fiber composite material with high tensile strength prepared by the above preparation method, wherein the tensile strength of the lignin-based carbon fiber composite material is as high as 78 MPa.
[0025] Carbon fiber composites have attracted attention from a wide range of industries including wind energy, aerospace and automotive due to their high strength-to-weight ratio, with the automotive industry being particularly interested in carbon fiber reinforced polymers (CFRP). The above-mentioned high tensile strength lignin-based carbon fiber composites can be very well applied in the wind energy, aerospace and automotive fields.
[0026] Unless otherwise specified, the "mass volume ratio" and "molar volume ratio" in the context of the present invention should be understood in a conventional manner in the art, that is, the ratio of the mass of the solid substance (in g) to the liquid volume (in mL) or the ratio of the mass volume of the solid substance. For example, when the "mass volume ratio of lignin to N,N-dimethylformamide is 0.1:1", if the amount of N,N-dimethylformamide added is 100 mL, the amount of lignin added is 10 mg.
[0027] Compared with the prior art, the present invention has the following advantages and effects:
[0028] (1) The present invention prepares lignin-based fibers by co-electrospinning a lignin solution at room temperature, and finally performs nitrogen source mixing and calcination. The obtained lignin-based carbon fibers have a dense structure, no visible macropores, and a relatively uniform fiber diameter. After thermal stabilization and carbonization, carbon fibers with good tensile strength and tensile modulus are produced. The carbon fibers of the present invention use optimized stabilization and carbonization technology to make the carbon fiber structure denser, which is beneficial to improve the tensile strength during the tensile performance test.
[0029] (2) From the perspective of application, the lignin-based carbon fiber composite material of the present invention has significant innovation. Compared with carbon fiber composite materials prepared from other precursors, the lignin-based carbon fiber composite material of the present invention has the advantages of cheaper and easier to obtain raw materials and better structural stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The XRD spectra of the lignin-based carbon fibers prepared by the present invention in different thermal stabilization methods and at different carbonization temperatures are compared.
[0031] Figure 2 This is the SEM of the lignin-based carbon fiber prepared in Example 1 of the present invention.
[0032] Figure 3 This is a comparison of tensile performance test graphs of the lignin-based carbon fiber composite materials prepared by adjusting different mass fractions of the present invention. DETAILED DESCRIPTION
[0033] The present invention is further described below with reference to specific embodiments, but they should not be construed as limiting the present invention.
[0034] Unless otherwise defined, all technical terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The technical terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or can be prepared by existing methods.
[0035] Example 1
[0036] A lignin-based carbon fiber, the preparation method of which comprises the following steps:
[0037] (1) 1.7 g of lignin and 1.7 g of polyacrylonitrile were added to 20 mL of N,N-dimethylformamide and stirred at 30 °C for 12 h to obtain a uniform spinning solution.
[0038] (2) The spinning solution obtained in step (1) was loaded into a syringe with a stainless steel needle for electrospinning, and the electrospinning conditions were as follows: the voltage was 15 kV, the distance between the needle and the aluminum disk was 15 cm, and the solution feed rate was 0.25 mL / h; the solution was then vacuum dried in a vacuum drying oven at 60° C. for 12 h to obtain a lignin-based carbon fiber precursor.
[0039] (3) heating the lignin-based carbon fiber precursor obtained in step (2) to 230° C. at a heating rate of 0.5° C. / min in an air atmosphere in a muffle furnace and thermally stabilizing for 2 h, heating the temperature to 250° C. at a heating rate of 0.5° C. / min and thermally stabilizing for 2 h, and heating the temperature to 280° C. at a heating rate of 0.5° C. / min and thermally stabilizing for 2 h; immediately quenching the mixture after thermal stabilization until it cools to room temperature;
[0040] (4) heating the sample again under a nitrogen atmosphere at a rate of 5°C / min to 1200°C for carbonization; the carbonization time was 2 hours to obtain lignin-based carbon fibers;
[0041] The morphology of the lignin-based carbon fibers prepared by the above method was detected by X-ray diffractometer and scanning electron microscope, respectively. Figure 1 and Figure 2 The XRD results show that the peak positions of the spectrum lines in the figure correspond to all the diffraction crystal planes of the JCPDF standard card (25-0283). The broad diffraction peak at about 25° corresponds to the lignin-based carbon fiber, and no impure diffraction peaks are found, indicating that the pure phase lignin-based carbon fiber is obtained (see Figure 1 ). The interlayer spacing results were calculated by fitting the Bragg equation, which showed the comparison of theoretical intermolecular forces of carbon fibers with different proportions and optimized calcination and carbonization (see Table 1). SEM results showed that the prepared lignin carbon fibers showed a dense structure, no visible macropores, and a relatively uniform fiber diameter (see Figure 2 ).
[0042] Example 2
[0043] This embodiment provides a method for preparing lignin-based carbon fibers. The difference from Embodiment 1 is that in step (1), the mass ratio of lignin to polyacrylonitrile in the spinning solution is 3:7.
[0044] Example 3
[0045] This embodiment provides a method for preparing lignin-based carbon fibers. The difference from Embodiment 1 is that in step (1), the mass ratio of lignin to polyacrylonitrile in the spinning solution is 1:9.
[0046] Example 4
[0047] This embodiment provides a method for preparing lignin-based carbon fibers. The difference from Embodiment 1 is that in step (1), the mass ratio of lignin to polyacrylonitrile in the spinning solution is 0:10.
[0048] Comparative Example 1
[0049] This comparative example provides a method for preparing lignin-based carbon fibers. The difference from Example 1 is that in step (1), the mass ratio of lignin to polyacrylonitrile in the spinning solution is 9:1.
[0050] Comparative Example 2
[0051] This comparative example provides a method for preparing lignin-based carbon fibers. The difference from Example 1 is that in step (1), the mass ratio of lignin to polyacrylonitrile in the spinning solution is 10:0.
[0052] Comparative Example 3
[0053] This comparative example provides a method for preparing lignin-based carbon fiber. Different from Example 1, in step (3), the lignin-based carbon fiber precursor is heated from room temperature to 250°C in a muffle furnace at a heating rate of 1°C / min for 2 hours, and then slowly cooled in the muffle furnace after the thermal stabilization.
[0054] Comparative Example 4
[0055] This comparative example provides a method for preparing lignin-based carbon fiber. Different from Example 2, in step (3), the lignin-based carbon fiber precursor is heated from room temperature to 250°C in a muffle furnace at a heating rate of 1°C / min for 2 hours, and then slowly cooled in the muffle furnace after the thermal stabilization.
[0056] Comparative Example 5
[0057] This comparative example provides a method for preparing lignin-based carbon fiber. The difference from Example 1 is that after quenching and cooling to room temperature in step (4), the lignin-based carbon fiber precursor is carbonized from room temperature to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere for 2 hours.
[0058] Comparative Example 6
[0059] This comparative example provides a method for preparing lignin-based carbon fiber. The difference from Example 1 is that after quenching and cooling to room temperature in step (4), the lignin-based carbon fiber precursor is carbonized from room temperature to 1100°C at a heating rate of 5°C / min for 2 hours in a nitrogen atmosphere.
[0060] Embodiment a
[0061] A lignin-based carbon fiber composite material, the preparation method of which comprises the following steps:
[0062] (i) The lignin-based carbon fiber obtained in Example 1 above was mixed and cured with dichloromethane (volume: 2.4 ml), E51 epoxy resin (mass: 6 g), and 4,4-diaminodiphenylmethane (mass: 0.32 g) to obtain a lignin-based carbon fiber composite material, wherein the mass fraction of the lignin-based carbon fiber in the lignin-based carbon fiber composite material is 2 wt%.
[0063] Embodiment b
[0064] This embodiment provides a method for preparing a lignin-based carbon fiber composite material. The difference from Embodiment A is that the mass fraction of the lignin-based carbon fiber in step (i) is 0.5 wt%.
[0065] Example c
[0066] This embodiment provides a method for preparing a lignin-based carbon fiber composite material. The difference from Embodiment A is that the mass fraction of the lignin-based carbon fiber in step (i) is 1 wt%.
[0067] Embodiment d
[0068] This embodiment provides a method for preparing a lignin-based carbon fiber composite material. The difference from Embodiment A is that the mass fraction of the lignin-based carbon fiber in step (i) is 10 wt%.
[0069] Comparative Example a
[0070] This comparative example provides a method for preparing a lignin-based carbon fiber composite material. Different from Example a, the method for preparing the lignin-based carbon fiber used in step (i) has the following differences from Example 1: In step (4), the heating is increased from room temperature to 800°C under a nitrogen atmosphere at a heating rate of 5°C / min and carbonized for 2 hours to obtain the lignin-based carbon fiber.
[0071] Comparative Example b
[0072] This comparative example provides a method for preparing a lignin-based carbon fiber composite material. Unlike Example B, the method for preparing the lignin-based carbon fiber used in step (i) has the following differences from Example 1: In step (4), the heating is carried out under a nitrogen atmosphere by raising the temperature from room temperature to 800°C at a heating rate of 5°C / min and carbonizing for 2 hours to obtain the lignin-based carbon fiber.
[0073] Comparative Example c
[0074] This comparative example provides a method for preparing a lignin-based carbon fiber composite material. Unlike Example C, the method for preparing the lignin-based carbon fiber used in step (i) has the following differences from Example 1: In step (4), the heating is carried out under a nitrogen atmosphere by raising the temperature from room temperature to 800°C at a heating rate of 5°C / min and carbonizing for 2 hours to obtain the lignin-based carbon fiber.
[0075] Comparative Example d
[0076] This comparative example provides a method for preparing a lignin-based carbon fiber composite material. Unlike Example d, the method for preparing the lignin-based carbon fiber used in step (i) has the following differences from Example 1: In step (4), the heating is carried out under a nitrogen atmosphere by raising the temperature from room temperature to 800°C at a heating rate of 5°C / min and carbonizing for 2 hours to obtain the lignin-based carbon fiber.
[0077] Performance Testing
[0078] 1. XRD test: The test was conducted on a CMT microcomputer-controlled electronic universal testing machine. The XRD spectra of Example 1 and the lignin-based carbon fibers prepared by different thermal stabilization methods and different carbonization temperatures were compared. The test angle range of the samples was 10°-80°, and the loading speed was 10° / min. The (002) peak position and half-peak width were obtained by fitting, and the interlayer spacing was calculated using the Bragg equation. The test results are shown in Figure 2. Figure 1 The calculation results are shown in Table 1.
[0079] Table 1
[0080]
[0081] The smaller the interlayer spacing data obtained, the greater the intermolecular force, which theoretically means that the tensile properties in macroscopic characterization are better. It can be seen from the chart that the interlayer spacing d(002) of Example 1 (5 / 5-quench-1200) is 0.36349, which is the smallest in the chart. In theory, its intermolecular force is the largest and the tensile properties are the best.
[0082] 2. Tensile property test: The test was carried out on a CMT microcomputer-controlled electronic universal testing machine. The samples of lignin-based carbon fibers obtained by comparing Example a, Example b, Example c, and Example d (EP / LCF (5 / 5) quench-1200-2wt%, EP / LCF (5 / 5) quench-1200-0.5wt%, EP / LCF (5 / 5) quench-1200-1wt%, and EP / LCF (5 / 5) quench-1200-10wt%) and Comparative Example a, Comparative Example b, Comparative Example c, and Comparative Example d (EP / LCF (5 / 5) quench-800-2wt%, EP / LCF (5 / 5) quench-800-0.5wt%, EP / LCF (5 / 5) quench-800-1wt%, and EP / LCF (5 / 5) quench-800-10wt%) were tested according to GB / T 1040.1-2018 "Determination of tensile properties of plastics" prepared the test specimens for tensile strength, the specimen loading speed was 2mm / min, 5 samples were tested in each group, and the results were averaged. The test results are shown in Table 2. Comparison of tensile properties test graphs of lignin-based carbon fiber composites prepared by adjusting different mass fractions Figure 3 shown.
[0083] Table 2
[0084]
[0085]
[0086] From the data in Table 2, it can be seen that the tensile strengths of Example a, Example b, Example c, Example d and Comparative Example a, Comparative Example b, Comparative Example c, and Comparative Example d are between 41 and 78 MPa. The advantages of Example a, Example b, Example c, and Example d are that the three-dimensional network structure formed by lignin and polyacrylonitrile mixes and further fixes and fuses EP and carbon fiber powder, enhancing the interfacial fusion force of the two, which is best when the mass fraction of carbon fiber powder is 2 wt%. The tensile strength of Example a is about 78 MPa, and the lignin-based carbon fiber obtained by the optimized treatment of quenching and increasing the carbonization temperature presents a denser structure, no visible macropores, and a more uniform fiber diameter, which also improves the tensile properties of the prepared lignin-based carbon fiber composite material.
[0087] Tensile properties test results (Table 2, Figure 3 ) further confirmed that the carbon fibers produced by lignin-based carbon fiber precursors after optimized thermal stabilization and carbonization have good tensile strength and tensile modulus.
[0088] The carbonization temperature is used as a comparative example because the difference in the interlayer spacing between Comparative Example 5 and Example 1 in Table 1 is reasonably considered to be sufficiently confirmed by the tensile performance test.
[0089] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a lignin-based carbon fiber composite material with high tensile strength, characterized in that The steps include: (1) adding lignin and polyacrylonitrile to N,N-dimethylformamide and stirring to obtain a uniform spinning solution; (2) electrospinning the spinning solution obtained in step (1), followed by vacuum drying to obtain a lignin-based carbon fiber precursor; (3) The lignin-based carbon fiber precursor obtained in step (2) is subjected to the following stepwise heating and thermal stabilization in an air atmosphere in a muffle furnace: heating to 230°C at a rate of 0.5-3°C / min and thermally stabilizing for 2h, then heating to 250°C at a rate of 0.5-3°C / min and thermally stabilizing for 2h, and then heating to 280°C at a rate of 0.5-3°C / min and thermally stabilizing for 2h; after the thermal stabilization is completed, quenching is immediately performed until it is cooled to room temperature; (4) heating to 600-1500° C. for carbonization to obtain lignin-based carbon fibers; (5) The lignin-based carbon fiber obtained in step (4) is mixed and cured with dichloromethane, E51 epoxy resin, and 4,4-diaminodiphenylmethane to obtain a lignin-based carbon fiber composite material with high tensile strength.
2. The method for preparing a lignin-based carbon fiber composite material with high tensile strength according to claim 1, characterized in that: In step (1), the mass volume ratio of lignin to N,N-dimethylformamide is 0.01-0.2 g:1 mL; the mass volume ratio of polyacrylonitrile to N,N-dimethylformamide is 0.01-0.2 g:1 mL.
3. The method for preparing a lignin-based carbon fiber composite material with high tensile strength according to claim 1, characterized in that: The stirring time in step (1) is 1-72 hours and the temperature is 20-80° C.; the vacuum drying temperature in step (2) is 60-90° C. and the time is 1-120 hours.
4. The method for preparing a lignin-based carbon fiber composite material with high tensile strength according to claim 1, characterized in that: The conditions for the electrospinning in step (2) are: voltage of 10-20 kV, distance between the needle and the aluminum disk of 10-20 cm, and solution feed rate of 0.1-0.5 mL / h.
5. The method for preparing a lignin-based carbon fiber composite material with high tensile strength according to claim 1, characterized in that: The heating rate in step (4) is 2-8°C / min; the carbonization time is 1-3h; and the carbonization is carried out under a protective gas atmosphere.
6. The method for preparing a lignin-based carbon fiber composite material with high tensile strength according to claim 1, characterized in that: The lignin-based carbon fiber in step (5) is ground into powder, and the dispersion area in the mold is 0.01-2mm 2 , and then compounded with E51 epoxy resin and 4,4-diaminodiphenylmethane.
7. The method for preparing a lignin-based carbon fiber composite material with high tensile strength according to claim 1, characterized in that: In step (5), the mass ratio of the lignin-based carbon fiber to the E51 epoxy resin is 0.1-0.25:1; the mass volume ratio of the E51 epoxy resin to dichloromethane is 2-10 g:1-5 mL; and the mass ratio of the lignin-based carbon fiber to 4,4-diaminodiphenylmethane is 0.1-2.5:
1.
8. The method for preparing a lignin-based carbon fiber composite material with high tensile strength according to claim 1, characterized in that: The mass fraction of the lignin-based carbon fiber in the lignin-based carbon fiber composite material in step (5) is 2wt%.
9. A lignin-based carbon fiber composite material with high tensile strength prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The lignin-based carbon fiber composite material has a tensile strength of up to 78 MPa.
10. Application of the lignin-based carbon fiber composite material with high tensile strength according to claim 9 in the fields of wind energy, aerospace and automobile.
Citation Information
Patent Citations
Lignin / polyacrylonitrile-containing dopes, fibers, and methods of making same
CN103080390A
Method for preparing carbon nanofiber through electrostatic blending of polyacrylonitrile / lignin
CN109943920A
Preparation method of lignin-based carbon material with high wave-absorbing performance
CN111235697A
Carbon fiber hub for automobile and preparation method of carbon fiber hub
CN118126493A
Production of carbonaceous nano-fibrous materials with ultra-high specific surface area from alkali (Kraft) lignin
US9190222B1