Ice surface antiskid sole material and preparation method thereof

The vulcanization of rubber substrates in the prior art is solved by using a combination of modified glass fiber and tetra-needle zinc oxide whiskers and styrene-ethylene/butene-styrene block copolymers in ice-surface anti-slip sole materials and the vulcanization of rubber substrates and the prior art. The problem of anti-slip performance that is prone to fall off of fibers has achieved efficient anti-slip performance and environmental protection on the ice surface.

CN119081336APending Publication Date: 2024-12-06SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411212273.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The vulcanization of rubber substrates in existing ice-surface anti-slip sole materials leads to waste of resources and easy fiber fall off, resulting in the problem of insufficient anti-slip performance.

Method used

Use styrene-ethylene/butene-styrene block copolymer as the substrate, and add modified glass fibers and tetra-shaped zinc oxide whiskers, and treat them with silane coupling agent to form a firm interface bond to improve Anti-slip properties of composite materials.

Benefits of technology

It realizes the high anti-slip performance, wear resistance and durability of the sole material on the ice surface, solves the problems of vulcanization of rubber substrates and easy fibers falling off, and the material can be recycled and has good environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081336A_ABST
    Figure CN119081336A_ABST
Patent Text Reader

Abstract

The invention discloses an ice surface antiskid sole material and a preparation method thereof, and belongs to the technical field of sole materials. The ice surface anti-skid sole material is prepared from the following raw materials in parts by mass: 80 to 120 parts of styrene-ethylene / butylene-styrene block copolymer, 10 to 105 parts of composite modified material, 10 to 60 parts of white mineral oil, 0.2 to 0.8 part of calcium stearate and 0.3 to 0.4 part of antioxidant 1010, the composite modified material comprises modified glass fibers and modified tetrapod-like zinc oxide whiskers; or the composite modified material comprises glass fibers, tetrapod-like zinc oxide whiskers and a first modifier; through the steps of mixing, hot pressing, cutting and the like, while glass fibers are added into a thermoplastic elastomer base material, tetrapod-like zinc oxide whiskers are adopted as a synergistic anti-skid additive, so that the problems of resource waste caused by vulcanization of a rubber base material and non-lasting anti-skid performance caused by easy falling of fibers in the existing ice surface anti-skid sole material technology are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sole materials, and particularly relates to an anti-skid sole material for ice surfaces and a preparation method thereof. Background Art

[0002] In recent years, my country's ice and snow sports have developed rapidly. The ice and snow sports industry has initially formed an industrial pattern with fitness and leisure as the main focus, and coordinated development of competition performances, sports training and sports tourism. This is conducive to meeting the diverse sports and cultural needs of the masses and promoting the deep integration of national fitness and national health. However, when carrying out daily activities and sports on ice and snow, the risk of falling and injury increases sharply, especially for children and the elderly with relatively weak athletic ability. Therefore, the anti-slip performance of ice sports equipment, especially shoes and boots, has attracted much attention. When walking on the ice, the water film between the sole and the ice surface leads to the particularity and complexity of anti-slip on the ice surface. How to make the sole material "pierce" the water film, reach the contact surface, and improve the grip of the sole on the ice surface has become an important problem to be solved in anti-slip shoes and boots. In the prior art, rubber is mainly used as the base material. Rubber must be vulcanized first during the sole molding process, and the molecular chains form a spatial network structure through cross-linking, thereby improving the elasticity and tensile strength of the product, but this reaction is irreversible, resulting in difficulty in processing after curing, difficulty in recycling the product after service, and difficulty in degrading waste rubber, resulting in waste of resources and environmental pollution. In addition, adding glass fiber to the substrate and then directly molding it cannot ensure that most of the glass fiber protrudes from the surface of the substrate, resulting in the anti-slip effect may not meet expectations; glass fiber has poor compatibility with rubber, and during friction with the contact surface, the glass fiber is easily pulled out, causing the glass fiber to be lost faster than the substrate, making it difficult for the sole to maintain long-lasting anti-slip performance on ice. Summary of the invention

[0003] In view of the above-mentioned prior art, the present invention provides an anti-skid sole material for ice surfaces and a preparation method thereof. Glass fiber is added to a thermoplastic elastomer substrate and four-needle zinc oxide whiskers are used as a synergistic anti-skid additive to solve the problems of resource waste caused by vulcanization of the rubber substrate and short-lasting anti-skid performance caused by easy shedding of fibers in the prior art of anti-skid sole materials for ice surfaces.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is: to provide an anti-skid sole material for ice surfaces, comprising the following raw materials in parts by weight: 80 to 120 parts of styrene-ethylene / butylene-styrene block copolymer, 10 to 105 parts of composite modified material, 10 to 60 parts of white mineral oil, 0.2 to 0.8 parts of calcium stearate and 0.3 to 0.4 parts of antioxidant 1010;

[0005] The composite modified material includes modified glass fiber and modified tetrapod-shaped zinc oxide whisker in a mass ratio of 5-60:5-40; or, the composite modified material includes glass fiber, tetrapod-shaped zinc oxide whisker and a first modifier in a mass ratio of 5-60:5-40:0.5-5, and the first modifier is silane coupling agent KH-550 or silane coupling agent KH-570;

[0006] The modified tetrapod-shaped zinc oxide whiskers are prepared by the following steps:

[0007] A1: Prepare an ethanol aqueous solution with a concentration of 85-95 wt%, and adjust its pH to 3-4;

[0008] A2: Add a second modifier to the solution obtained in step A1, and hydrolyze for 3 hours to obtain a hydrolyzate; the second modifier is silane coupling agent KH-550 or silane coupling agent KH-570;

[0009] A3: Add tetrapod-shaped zinc oxide whiskers to the hydrolyzate, stir for 10-14 hours, and filter; the mass ratio of tetrapod-shaped zinc oxide whiskers to modifier is 1:0.05;

[0010] A4: Rinse the filtered product repeatedly with anhydrous ethanol and dry it at 70-90℃ to obtain the product;

[0011] The modified glass fiber is prepared by the following steps:

[0012] B1: Prepare an ethanol aqueous solution with a concentration of 90-95 wt%, and adjust its pH to 3-4;

[0013] B2: Add a third modifier to the solution obtained in step B1, and hydrolyze for 3 hours to obtain a hydrolyzate; the third modifier is a silane coupling agent KH-550 or a silane coupling agent KH-570;

[0014] B3: Add glass fiber to the hydrolyzate, stir for 2-4 hours, and filter; the mass ratio of glass fiber to modifier is 1:0.05;

[0015] B4: Rinse the filtered product repeatedly with anhydrous ethanol, and dry it at 70-90℃ to obtain the product.

[0016] The beneficial effects of the technical scheme adopted by the present invention are as follows: the matrix material of the present invention is selected from styrene-ethylene / butylene block copolymer (SEBS), SEBS does not contain active carbon-carbon double bonds, has excellent tolerance to ozone and ultraviolet rays, and has good outdoor weather resistance. In addition, SEBS can be directly thermoplastic processed and formed, has the excellent application performance of rubber without vulcanization, and the scraps can be recycled without damaging the physical properties and processing performance of the elastomer, which is safe and environmentally friendly. The four-needle zinc oxide whisker (T-ZnOw) is composed of four needle-shaped single crystal microfibers extending from a center to four directions, and has a special three-dimensional four-needle structure, so that it has a completely isotropic modification effect on polymer composite materials, and part of the needle-shaped structure can also be exposed on the material surface, changing its surface microscopic morphology from the nanometer scale, strengthening the grip of the material surface and the contact surface, and greatly improving its anti-skid performance. The addition of the four-needle zinc oxide has a reinforcing effect on SEBS, and also increases the wetting effect of SEBS on glass fiber (GF), so that more fibers protrude from the material surface, and the anti-skid effect is enhanced. In addition, glass fiber is a brittle fiber. When wearing shoes, some of the glass fiber may be worn off. At this time, the four-needle zinc oxide whiskers exposed on the surface of the material can replace the anti-skid function to a certain extent. The glass fiber and the four-needle zinc oxide whiskers are treated with a modifier to form a strong interface bond with the SEBS matrix, while improving the compatibility between the inorganic filler and the organic matrix, further improving the anti-skid performance of the composite material on ice surfaces.

[0017] Based on the above technical solution, the present invention can also be improved as follows.

[0018] Furthermore, the anti-skid sole material for ice surfaces comprises the following raw materials in parts by mass: 100 parts of styrene-ethylene / butylene-styrene block copolymer, 21 parts of composite modified material, 30 parts of white mineral oil, 0.5 parts of calcium stearate and 0.3 parts of antioxidant 1010;

[0019] The composite modified material comprises modified glass fiber and modified four-needle zinc oxide whisker in a mass ratio of 1:1.

[0020] Furthermore, the glass fiber has a diameter of 10 to 15 μm and a length of 3 to 6 mm.

[0021] Furthermore, in step A1, the concentration of the ethanol aqueous solution is 90 wt % and the pH is 3; in step A3, the stirring time is 12 h; in step A4, the drying temperature is 80° C. and the drying time is 12 h.

[0022] Furthermore, the concentration of the ethanol aqueous solution in step B1 is 95wt% and the pH is 3; the stirring time in step B3 is 3h; and the drying temperature in step B4 is 80°C and the drying time is 24h.

[0023] Furthermore, the method for preparing the anti-skid sole material for ice surfaces comprises the following steps:

[0024] (1) mixing styrene-ethylene / butylene-styrene block copolymer, white mineral oil, antioxidant 1010 and calcium stearate at a temperature of 160 to 190° C., a rotation speed of 60 to 80 rpm, and a time of 4 to 6 minutes to obtain a mixture A;

[0025] (2) Adding the composite modified material to the mixture A and kneading them together for 10 to 15 minutes to obtain the mixture B;

[0026] (3) Mixture B is smelted for 4 to 6 minutes and then cut into blocks;

[0027] (4) The block material is hot pressed under the conditions of a pressure of 0.9 to 1.1 MPa and a temperature of 170 to 190° C. to obtain the product.

[0028] Furthermore, in step (1), the mixing temperature is 175° C., the rotation speed is 70 rpm, and the mixing time is 5 min.

[0029] Furthermore, the co-mixing time in step (2) is 12 minutes.

[0030] Furthermore, the refining time in step (3) is 5 minutes.

[0031] Furthermore, in step (4), the pressure is 1 MPa and the temperature is 180°C.

[0032] The beneficial effects of the above further technical solution adopted by the present invention are: the preparation method in the present invention is simple, and the preparation of the anti-skid sole material can be achieved through the steps of mixing, hot pressing, cutting, etc., which is conducive to expanding production. During the preparation process, part of the needle-like structure is exposed on the surface of the material, and the microscopic morphology of the material surface is changed from the nanoscale, so that the sole material can "pierce" the water film and reach the contact surface, thereby enhancing the grip of the material surface on the ice surface and greatly improving the anti-skid performance; the addition of four needle-like zinc oxide whiskers has a reinforcing effect on SEBS, and also increases the wetting effect of SEBS on glass fibers, so that more fibers protrude almost vertically from the surface of the material, and the anti-skid effect is enhanced.

[0033] The invention has the following beneficial effects: the invention selects styrene-ethylene / butylene block copolymer as a substrate, adds glass fiber to the thermoplastic elastomer substrate, and uses four-needle zinc oxide whiskers as a synergistic anti-skid additive, fully exerts the synergistic effect of four-needle zinc oxide whiskers and glass fiber in the production process, and the four-needle zinc oxide whiskers and glass fiber are treated with a modifier to form a stronger bond with the styrene-ethylene / butylene block copolymer matrix, thereby further improving the overall performance of the composite material. The raw material formula and preparation method of the anti-skid sole of the invention give play to the synergistic effect between the components, not only considering the mechanical properties of the material, but also taking into account the processability, stability and environmental protection and other aspects. The prepared sole not only has high anti-skid performance on the ice surface, but also does not affect its stability when walking on normal ground, and has excellent properties such as anti-skid performance, wear resistance, high strength and durability, and solves the problems of resource waste caused by vulcanization of rubber substrate and non-persistent anti-skid performance caused by easy shedding of fibers in the existing anti-skid sole material technology on ice. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 To modify the microscopic surface morphology of tetrapod-shaped zinc oxide whiskers;

[0035] Figure 2 This is a microscopic morphology of the surface of the anti-skid sole material for ice surfaces prepared in Example 1. DETAILED DESCRIPTION

[0036] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0037] Example 1

[0038] An anti-skid sole material for ice surfaces comprises the following raw materials in parts by mass: 100 parts of styrene-ethylene / butylene-styrene block copolymer, 10.5 parts of modified glass fiber, 10.5 parts of modified four-needle zinc oxide whisker, 30 parts of white mineral oil, 0.5 parts of calcium stearate and 0.3 parts of antioxidant 1010; the specific preparation method is as follows:

[0039] 1. Preparation of modified tetrapod-shaped zinc oxide whiskers (T-ZnOw)

[0040] A1: Prepare a 90 wt% ethanol aqueous solution and adjust the pH to 3 with hydrochloric acid;

[0041] A2: Add silane coupling agent KH-570 to the solution obtained in step A1, and hydrolyze at room temperature for 3 hours to obtain a hydrolyzate;

[0042] A3: Add tetrapod-shaped zinc oxide whiskers to the hydrolyzate, stir on a magnetic stirrer at room temperature for 12 hours, and then filter with a vacuum pump; the mass ratio of tetrapod-shaped zinc oxide whiskers to silane coupling agent KH-570 is 1:0.05;

[0043] A4: Rinse the filtered product repeatedly with anhydrous ethanol, and then dry it in a vacuum oven at 80°C for 12 hours, and then break it up to obtain the product.

[0044] 2. Preparation of modified glass fiber (GF)

[0045] B1: Prepare an ethanol aqueous solution with a concentration of 95 wt%, and adjust the pH to 3 with hydrochloric acid;

[0046] B2: Add silane coupling agent KH-570 to the solution obtained in step B1, and hydrolyze at room temperature for 3 hours to obtain a hydrolyzate;

[0047] B3: Add glass fiber to the hydrolyzate, stir on a magnetic stirrer at room temperature for 3 hours, and then filter with a vacuum pump; wherein the diameter of the glass fiber is about 12 μm and the length is about 5 mm; the mass ratio of the glass fiber to the silane coupling agent KH-570 is 1:0.05;

[0048] B4: Rinse the filtered product repeatedly with anhydrous ethanol, and then dry it in a vacuum oven at 80°C for 24 hours.

[0049] 3. Preparation of anti-skid sole materials for ice surfaces

[0050] (1) SEBS, white mineral oil, antioxidant 1010 and calcium stearate were mixed in an internal mixer at a temperature of 175° C., a rotation speed of 70 rpm, and a time of 5 min to obtain a mixture A;

[0051] (2) Add modified T-ZnOw and modified GF to mixed material A, and mix them together for 12 minutes after the torque is stable to obtain mixed material B;

[0052] (3) Mixture B was milled for 5 min and cut into blocks;

[0053] (4) The block material is placed in a mold and hot-pressed into a block material with a thickness of 10 mm at a hot-pressing temperature of 180° C. and a pressure of 1 MPa.

[0054] 4. Preparation of anti-skid soles for ice surfaces

[0055] (1) Cut the anti-skid sole material for ice surface into sheets with a thickness of 2 mm and punch them into specific shapes with a die cutter;

[0056] (2) The above-mentioned sheet of specific shape is placed in a sole mold, and ordinary sole materials are covered on its surface, and hot-pressed to form an ice-resistant non-slip sole.

[0057] Example 2

[0058] An anti-skid sole material for ice surfaces comprises the following raw materials in parts by mass: 100 parts of styrene-ethylene / butylene-styrene block copolymer, 15.75 parts of modified glass fiber, 10.5 parts of modified four-needle zinc oxide whisker, 30 parts of white mineral oil, 0.5 parts of calcium stearate and 0.3 parts of antioxidant 1010; the specific preparation method is as follows:

[0059] 1. Preparation of modified tetrapod-shaped zinc oxide whiskers (T-ZnOw)

[0060] A1: Prepare a 95wt% ethanol aqueous solution and adjust the pH to 4 with hydrochloric acid;

[0061] A2: Add silane coupling agent KH-570 to the solution obtained in step A1, and hydrolyze at room temperature for 3 hours to obtain a hydrolyzate;

[0062] A3: Add tetrapod-shaped zinc oxide whiskers to the hydrolyzate, stir on a magnetic stirrer at room temperature for 14 hours, and then filter with a vacuum pump; the mass ratio of tetrapod-shaped zinc oxide whiskers to silane coupling agent KH-570 is 1:0.05;

[0063] A4: Rinse the filtered product repeatedly with anhydrous ethanol, and then dry it in a 70℃ oven under vacuum for 12 hours. Then break it up to obtain the product.

[0064] 2. Preparation of modified glass fiber (GF)

[0065] B1: Prepare a 90 wt% ethanol aqueous solution and adjust the pH to 4 with hydrochloric acid;

[0066] B2: Add silane coupling agent KH-570 to the solution obtained in step B1, and hydrolyze at room temperature for 3 hours to obtain a hydrolyzate;

[0067] B3: Add glass fiber to the hydrolyzate, stir on a magnetic stirrer at room temperature for 4 hours, and then filter with a vacuum pump; the diameter of the glass fiber is about 12 μm and the length is about 5 mm; the mass ratio of the glass fiber to the silane coupling agent KH-570 is 1:0.05;

[0068] B4: Rinse the filtered product repeatedly with anhydrous ethanol, and then dry it in a 70°C oven under vacuum for 24 hours.

[0069] 3. Preparation of anti-skid sole materials for ice surfaces

[0070] (1) SEBS, white mineral oil, antioxidant 1010 and calcium stearate were mixed in a torque rheometer at a temperature of 160° C., a rotation speed of 60 rpm, and a time of 5 min to obtain a mixture A;

[0071] (2) Add modified T-ZnOw and modified GF to mixed material A, and mix them together for 15 minutes after the torque is stable to obtain mixed material B;

[0072] (3) Mixture B was milled for 5 min and cut into blocks;

[0073] (4) The block material is placed in a mold and hot-pressed into a block material with a thickness of 10 mm at a hot-pressing temperature of 190° C. and a pressure of 1 MPa.

[0074] 4. Preparation of anti-skid soles for ice surfaces

[0075] (1) Cut the anti-skid sole material for ice surface into sheets with a thickness of 2 mm and punch them into specific shapes with a die cutter;

[0076] (2) The above-mentioned sheet of specific shape is placed in a sole mold, and ordinary sole materials are covered on its surface, and hot-pressed to form an ice-resistant non-slip sole.

[0077] Example 3

[0078] An anti-skid sole material for ice surfaces comprises the following raw materials in parts by weight: 80 parts of styrene-ethylene / butylene-styrene block copolymer, 5.25 parts of modified glass fiber, 5.25 parts of modified four-needle zinc oxide whisker, 10 parts of white mineral oil, 0.2 parts of calcium stearate and 0.3 parts of antioxidant 1010; the specific preparation method is as follows:

[0079] 1. Preparation of modified tetrapod-shaped zinc oxide whiskers (T-ZnOw)

[0080] A1: Prepare an ethanol aqueous solution with a concentration of 85 wt%, and adjust the pH to 3 with hydrochloric acid;

[0081] A2: Add silane coupling agent KH-550 to the solution obtained in step A1, and hydrolyze at room temperature for 3 hours to obtain a hydrolyzate;

[0082] A3: Add tetrapod-shaped zinc oxide whiskers to the hydrolyzate, stir on a magnetic stirrer at room temperature for 10 hours, and then filter with a vacuum pump; the mass ratio of tetrapod-shaped zinc oxide whiskers to silane coupling agent KH-550 is 1:0.05;

[0083] A4: Rinse the filtered product repeatedly with anhydrous ethanol, and then dry it in a 90℃ oven under vacuum for 12 hours.

[0084] 2. Preparation of modified glass fiber (GF)

[0085] B1: Prepare an ethanol aqueous solution with a concentration of 95 wt%, and adjust the pH to 3 with hydrochloric acid;

[0086] B2: Add silane coupling agent KH-550 to the solution obtained in step B1, and hydrolyze at room temperature for 3 hours to obtain a hydrolyzate;

[0087] B3: Add glass fiber to the hydrolyzate, stir on a magnetic stirrer at room temperature for 2 hours, and then filter with a vacuum pump; the diameter of the glass fiber is about 10 μm and the length is about 6 mm; the mass ratio of the glass fiber to the silane coupling agent KH-550 is 1:0.05;

[0088] B4: Rinse the filtered product repeatedly with anhydrous ethanol, and then dry it in a 90°C oven under vacuum for 24 hours.

[0089] 3. Preparation of anti-skid sole materials for ice surfaces

[0090] (1) SEBS, white mineral oil, antioxidant 1010 and calcium stearate were mixed in an internal mixer at a temperature of 190° C. and a rotation speed of 80 rpm for 5 min to obtain a mixture A;

[0091] (2) Add modified T-ZnOw and modified GF to mixed material A, and mix them together for 10 minutes after the torque is stable to obtain mixed material B;

[0092] (3) Mixture B was milled for 5 min and cut into blocks;

[0093] (4) The block material is placed in a mold and hot-pressed into a block material with a thickness of 10 mm at a hot-pressing temperature of 170° C. and a pressure of 1 MPa.

[0094] 4. Preparation of anti-skid soles for ice surfaces

[0095] (1) Cut the anti-skid sole material for ice surface into sheets with a thickness of 2 mm and punch them into specific shapes with a die cutter;

[0096] (2) The above-mentioned sheet of specific shape is placed in a sole mold, and ordinary sole materials are covered on its surface, and hot-pressed to form an ice-resistant non-slip sole.

[0097] Example 4

[0098] A non-slip sole material for ice surfaces comprises the following raw materials in parts by mass: 120 parts of styrene-ethylene / butylene-styrene block copolymer, 63 parts of modified glass fiber, 42 parts of modified four-needle zinc oxide whisker, 60 parts of white mineral oil, 0.8 parts of calcium stearate and 0.4 parts of antioxidant 1010; the specific preparation method is the same as that of Example 1, wherein the glass fiber has a diameter of about 15 μm and a length of about 3 mm; and the modifier is a silane coupling agent KH-570.

[0099] Example 5

[0100] An anti-skid sole material for ice surfaces comprises the following raw materials in parts by mass: 100 parts of styrene-ethylene / butylene-styrene block copolymer, 21 parts of composite modified material, 30 parts of white mineral oil, 0.5 parts of calcium stearate and 0.3 parts of antioxidant 1010. The specific preparation method is as follows:

[0101] 1. Preparation of anti-skid sole materials for ice surfaces

[0102] (1) SEBS, white mineral oil, antioxidant 1010 and calcium stearate were mixed in an internal mixer at a temperature of 175° C., a rotation speed of 70 rpm, and a time of 5 min to obtain a mixture A;

[0103] (2) adding a composite modified material to the mixture A, and mixing them together for 12 minutes after the torque is stable, to obtain a mixture B; wherein the composite modified material includes glass fiber, four-needle zinc oxide whisker and a first modifier in a mass ratio of 10:10:1, the glass fiber has a diameter of about 12 μm and a length of about 5 mm; and the first modifier is a silane coupling agent KH-570;

[0104] (3) Mixture B was milled for 5 min and cut into blocks;

[0105] (4) The block material is placed in a mold and hot-pressed into a block material with a thickness of 10 mm at a hot-pressing temperature of 180° C. and a pressure of 1 MPa.

[0106] 2. Preparation of anti-skid soles for ice surfaces

[0107] (1) Cut the anti-skid sole material for ice surface into sheets with a thickness of 2 mm and punch them into specific shapes with a die cutter;

[0108] (2) The above-mentioned sheet of specific shape is placed in a sole mold, and ordinary sole materials are covered on its surface, and hot-pressed to form an ice-resistant non-slip sole.

[0109] Comparative Example 1

[0110] An anti-skid sole material for ice surfaces comprises the following raw materials in parts by weight: 100 parts of styrene-ethylene / butylene-styrene block copolymer, 10.5 parts of modified glass fiber, 30 parts of white mineral oil, 0.25 parts of calcium stearate and 0.3 parts of antioxidant 1010. The specific preparation method is as follows:

[0111] 1. Preparation of modified glass fiber (GF)

[0112] B1: Prepare an ethanol aqueous solution with a concentration of 95 wt%, and adjust the pH to 3 with hydrochloric acid;

[0113] B2: Add silane coupling agent KH-570 to the solution obtained in step B1, and hydrolyze at room temperature for 3 hours to obtain a hydrolyzate;

[0114] B3: Add glass fiber to the hydrolyzate, stir on a magnetic stirrer at room temperature for 3 hours, and then filter with a vacuum pump; the diameter of the glass fiber is about 12 μm and the length is about 5 mm; the mass ratio of the glass fiber to the silane coupling agent KH-570 is 1:0.05;

[0115] B4: Rinse the filtered product repeatedly with anhydrous ethanol, and then dry it in a vacuum oven at 80°C for 24 hours.

[0116] 2. Preparation of anti-skid sole materials for ice surfaces

[0117] (1) SEBS, white mineral oil, antioxidant 1010 and calcium stearate were mixed in an internal mixer at a temperature of 175° C., a rotation speed of 70 rpm, and a time of 5 min to obtain a mixture A;

[0118] (2) Add modified GF to mixed material A, and after the torque becomes stable, mix together for 12 minutes to obtain mixed material B;

[0119] (3) Mixture B was milled for 5 min and cut into blocks;

[0120] (4) The block material is placed in a mold and hot-pressed into a block material with a thickness of 10 mm at a hot-pressing temperature of 180° C. and a pressure of 1 MPa.

[0121] 3. Preparation of anti-skid soles for ice surfaces

[0122] (1) Cut the anti-skid sole material for ice surface into sheets with a thickness of 2 mm and punch them into specific shapes with a die cutter;

[0123] (2) The above-mentioned sheet of specific shape is placed in a sole mold, and ordinary sole materials are covered on its surface, and hot-pressed to form an ice-resistant non-slip sole.

[0124] Comparative Example 2

[0125] An anti-skid sole material for ice surfaces comprises the following raw materials in parts by mass: 100 parts of styrene-ethylene / butylene-styrene block copolymer, 10 parts of glass fiber, 10 parts of four-needle zinc oxide whiskers, 30 parts of white mineral oil, 0.5 parts of calcium stearate and 0.3 parts of antioxidant 1010; the specific preparation method is as follows:

[0126] 1. Preparation of anti-skid sole materials for ice surfaces

[0127] (1) SEBS, white mineral oil, antioxidant 1010 and calcium stearate were mixed in an internal mixer at a temperature of 175° C., a rotation speed of 70 rpm, and a time of 5 min to obtain a mixture A;

[0128] (2) T-ZnOw and GF were added to the mixture A, and after the torque was stable, they were mixed together for 12 minutes to obtain the mixture B, in which the diameter of the glass fiber was about 12 μm and the length was about 5 mm;

[0129] (3) Mixture B was milled for 5 min and cut into blocks;

[0130] (4) The block material is placed in a mold and hot-pressed into a block material with a thickness of 10 mm at a hot-pressing temperature of 180° C. and a pressure of 1 MPa.

[0131] 2. Preparation of anti-skid soles for ice surfaces

[0132] (1) Cut the anti-skid sole material for ice surface into sheets with a thickness of 2 mm and punch them into specific shapes with a die cutter;

[0133] (2) The above-mentioned sheet of specific shape is placed in a sole mold, and ordinary sole materials are covered on its surface, and hot-pressed to form an ice-resistant non-slip sole.

[0134] Comparative Example 3

[0135] An anti-skid sole material for ice surfaces comprises the following raw materials in parts by weight: 100 parts of styrene-ethylene / butylene-styrene block copolymer, 30 parts of mineral oil, 0.5 parts of calcium stearate and 0.3 parts of antioxidant 1010; the specific preparation method is as follows:

[0136] 1. Preparation of anti-skid sole materials for ice surfaces

[0137] (1) SEBS, white mineral oil, antioxidant 1010 and calcium stearate were mixed in an internal mixer at a temperature of 175° C., a rotation speed of 70 rpm, and a time of 5 min to obtain a mixture A;

[0138] (2) Mixture A was milled for 5 min and cut into blocks;

[0139] (3) The block material is placed in a mold and hot-pressed into a block material with a thickness of 10 mm at a hot-pressing temperature of 180° C. and a pressure of 1 MPa.

[0140] 2. Preparation of anti-skid soles for ice surfaces

[0141] (1) Cut the anti-skid sole material for ice surface into sheets with a thickness of 2 mm and punch them into specific shapes with a die cutter;

[0142] (2) The above-mentioned sheet of specific shape is placed in a sole mold, and ordinary sole materials are covered on its surface, and hot-pressed to form an ice-resistant non-slip sole.

[0143] Experimental example

[0144] The performances of the anti-skid shoe soles on ice prepared in Examples 1 to 5 are similar. Taking Examples 1 and 2 as examples, the performances of the anti-skid shoe soles on ice are described in detail.

[0145] 1. The microscopic surface morphology of the modified T-ZnOw prepared in Example 1 is as follows Figure 1 As shown, it indicates that the modified T-ZnOw still maintains a complete four-needle structure.

[0146] 2. The surface microscopic morphology of the anti-skid shoe sole material on ice prepared in Example 1 is shown in Figure 2 As shown, it shows that the addition of four-needle zinc oxide whiskers and glass fibers changes the surface micromorphology of the material at the nanoscale, enhances the grip of the material surface and the contact surface, and greatly improves its anti-slip performance.

[0147] 3. The performance indicators of composite soles are shown in Table 1

[0148] Table 1 Physical properties of anti-slip soles

[0149]

[0150] Note: Anti-skid coefficient 1 is the anti-skid coefficient of a brand new sole on ice; anti-skid coefficient 2 is the anti-skid coefficient of a sole on ice after it has been worn 1mm.

[0151] The anti-skid soles for ice surfaces prepared in Example 1 and Example 2 have anti-skid coefficients significantly better than those of the comparative examples in both the new state and after wear, indicating that the four-needle zinc oxide whiskers and glass fibers play a significant anti-skid role in the anti-skid soles for ice surfaces. The components in the anti-skid sole formula for ice surfaces of the present invention work together to improve the anti-skid performance, wear resistance, strength and durability of the soles through synergistic effects; not only the mechanical properties of the material are considered, but also the requirements of processability, stability and environmental protection are taken into account, solving the problems of resource waste caused by the vulcanization of the rubber substrate and the non-durable anti-skid performance caused by the easy shedding of fibers in the existing anti-skid sole material technology for ice surfaces.

[0152] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. An anti-skid sole material for ice surfaces, characterized in that: The invention comprises the following raw materials in parts by weight: 80 to 120 parts of styrene-ethylene / butylene-styrene block copolymer, 10 to 105 parts of composite modified material, 10 to 60 parts of white mineral oil, 0.2 to 0.8 parts of calcium stearate and 0.3 to 0.4 parts of antioxidant 1010; The composite modified material comprises modified glass fiber and modified tetrapod-shaped zinc oxide whisker in a mass ratio of 5-60:5-40; or, the composite modified material comprises glass fiber, tetrapod-shaped zinc oxide whisker and a first modifier in a mass ratio of 5-60:5-40:0.5-5, wherein the first modifier is silane coupling agent KH-550 or silane coupling agent KH-570; The modified four-needle zinc oxide whisker is prepared by the following steps: A1: Prepare an ethanol aqueous solution with a concentration of 85-95 wt%, and adjust its pH to 3-4; A2: adding a second modifier to the solution obtained in step A1, hydrolyzing for 3 hours to obtain a hydrolyzate; the second modifier is a silane coupling agent KH-550 or a silane coupling agent KH-570; A3: Add tetrapod-shaped zinc oxide whiskers to the hydrolyzate, stir for 10 to 14 hours, and filter; the mass ratio of the tetrapod-shaped zinc oxide whiskers to the modifier is 1:0.05; A4: Rinse the filtered product repeatedly with anhydrous ethanol and dry it at 70-90℃ to obtain the product; The modified glass fiber is prepared by the following steps: B1: Prepare an ethanol aqueous solution with a concentration of 90-95 wt%, and adjust its pH to 3-4; B2: Add a third modifier to the solution obtained in step B1, and hydrolyze for 3 hours to obtain a hydrolyzate; the third modifier is a silane coupling agent KH-550 or a silane coupling agent KH-570; B3: Add glass fiber to the hydrolyzate, stir for 2 to 4 hours, and filter; the mass ratio of the glass fiber to the modifier is 1:0.05; B4: Rinse the filtered product repeatedly with anhydrous ethanol, and dry it at 70-90℃ to obtain the product.

2. The anti-skid sole material for ice surfaces according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of styrene-ethylene / butylene-styrene block copolymer, 21 parts of composite modified material, 30 parts of white mineral oil, 0.5 parts of calcium stearate and 0.3 parts of antioxidant 1010; The composite modified material comprises modified glass fiber and modified four-needle zinc oxide whisker in a mass ratio of 1:

1.

3. The anti-skid sole material for ice surfaces according to claim 1 or 2, characterized in that: The glass fiber has a diameter of 10 to 15 μm and a length of 3 to 6 mm.

4. The anti-skid sole material for ice surfaces according to claim 1, characterized in that: The concentration of the ethanol aqueous solution in step A1 is 90wt% and the pH is 3; the stirring time in step A3 is 12h; and the drying temperature in step A4 is 80°C and the drying time is 12h.

5. The anti-skid sole material for ice surfaces according to claim 1, characterized in that: The concentration of the ethanol aqueous solution in step B1 is 95wt% and the pH is 3; the stirring time in step B3 is 3h; the drying temperature in step B4 is 80°C and the drying time is 24h.

6. The method for preparing the anti-skid sole material for ice surfaces according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) mixing styrene-ethylene / butylene-styrene block copolymer, white mineral oil, antioxidant 1010 and calcium stearate at a temperature of 160 to 190° C., a rotation speed of 60 to 80 rpm, and a time of 4 to 6 minutes to obtain a mixture A; (2) adding the composite modified material to the mixed material A and kneading them together for 10 to 15 minutes to obtain a mixed material B; (3) the mixed material B is smelted for 4 to 6 minutes and then cut into block materials; (4) The block material is hot pressed under the conditions of a pressure of 0.9 to 1.1 MPa and a temperature of 170 to 190° C. to obtain the block material.

7. The method for preparing the anti-skid sole for ice surface according to claim 6, characterized in that: In the step (1), the mixing temperature is 175° C., the rotation speed is 70 rpm, and the mixing time is 5 min.

8. The method for preparing the anti-skid sole for ice surface according to claim 6, characterized in that: The co-mixing time in step (2) is 12 minutes.

9. The method for preparing the anti-skid sole for ice surface according to claim 6, characterized in that: The refining time in step (3) is 5 minutes.

10. The method for preparing the anti-skid sole for ice surface according to claim 6, characterized in that: In the step (4), the pressure is 1 MPa and the temperature is 180°C.