Adhesive for bonding wood boards as well as preparation method and application of adhesive
A thermoplastic polyurethane-based adhesive with polycaprolactone and colorless petroleum resin, combined with a high-boiling-point solvent, addresses color and compatibility issues, ensuring strong and uniform bonding without bulging on light-colored wood boards.
Patent Information
- Application Number
- CN202411231120.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
Smart Images

Figure BDA0005026166350000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to an adhesive for bonding wood boards, and a preparation method and application thereof. Background Art
[0002] Adhesives for wood board bonding are used to bond solid wood, composite boards, fiberboards of different densities and other furniture and home decoration substrates with decorative film layers. They have high requirements for initial bonding strength. If the initial bonding strength is not enough, the solvent volatilizes at high temperatures and easily causes bulging of the decorative film layer. Therefore, improving initial bonding strength is an important requirement for adhesives.
[0003] In order to improve the initial adhesion strength of the adhesive, the R&D personnel carried out relevant R&D work:
[0004] Patent CN106496500A discloses a high initial viscosity hot melt polyurethane adhesive and a preparation method thereof, and specifically discloses that by using a reactive tackifier containing a natural rosin-modified resin containing a hydroxyl group, the prepared adhesive has high stability and high initial viscosity. Although its creep resistance reaches 3500 grams, the natural rosin-modified resin used therein has a darker color, and when applied to a light-colored film such as white, it will not be aesthetically pleasing due to the color development, affecting the sensory experience.
[0005] Patent CN108624278A discloses a room temperature triphenylene-free modified polyurethane coating adhesive and a preparation method thereof, and specifically discloses that the tackifying resins used in the modified polyurethane coating adhesive include polyketone resin, phenolic resin, and hydrogenated rosin, which will also affect the appearance due to color development.
[0006] Patent CN114874739A discloses a reactive polyurethane adhesive for bonding and a preparation method thereof. The adhesive is composed of the following raw materials in parts by weight: 39.6-175.8 parts of diisocyanate, 0.2-5 parts of triphenylmethane triisocyanate, 5-50 parts of polyester diol, 100-400 parts of polyether diol, 0.5-10 parts of polyether triol, 10-40 parts of chain extender, 0.1-1 parts of silane coupling agent, 0.2-2 parts of latent curing agent and 0.01-0.5 parts of catalyst.
[0007] Patent CN112142961A discloses a tackifying additive and its application in woodworking glue. The tackifying additive is copolymerized by a dibasic acid, a diol and a capping agent, and has a glass transition temperature of 35-55°C and a molecular weight of 3000-7000g / mol; the dibasic acid is composed of an aromatic dibasic acid and an aliphatic dibasic acid; the diol is composed of a linear small molecule diol, an alicyclic diol and an aromatic diol; the molar ratio of the dibasic acid to the diol is 1.1-1.3:1, and the molar ratio of the capping agent to the dibasic acid is 0.06-0.2:1.
[0008] At present, tackifying resins are mostly used to increase the initial adhesion strength of adhesives. However, conventional tackifying resins such as rosin resins, terpene resins, phenolic resins, phenolic terpene resins, etc. are all dark in color. Therefore, when they are applied to light-colored films such as white, they will cause color development, affecting the normal use and scope of use of the adhesive. Conventional colorless tackifying resins C5-C9 have poor compatibility with TPU and cannot be evenly mixed, making them unusable. In addition, phenolic resins generally have high molecular weights, and some have active hydroxyl groups, which will affect the solubility of the particles and the storage stability when used with a curing agent later.
[0009] In view of the above, it is desirable to provide an adhesive having high initial viscosity, no foaming, and no coloring. Summary of the invention
[0010] In order to solve the above technical problems existing in the prior art, the present invention provides an adhesive for bonding wood boards and a preparation method and application thereof.
[0011] The technical solution of the present invention to solve the above technical problems is as follows:
[0012] The first aspect of the present invention is to provide an adhesive for bonding wood boards, which comprises the following components by weight: 10-20 parts of thermoplastic polyurethane, 5-10 parts of polycaprolactone, 10-20 parts of petroleum resin, and 50-80 parts of organic solvent;
[0013] The organic solvent includes a first solvent and a second solvent, and the boiling point of the first solvent is higher than that of the second solvent.
[0014] The beneficial effects of the adhesive for bonding wood boards provided by the present invention are:
[0015] The adhesive for bonding wooden boards provided by the present invention has a residual organic solvent that is mainly a first solvent with a high boiling point after being heated and cured, thereby reducing the amount of solvent volatilization in the subsequent placement process, reducing bulging and foaming, and being safe and environmentally friendly; at the same time, the partial residue of the high-boiling-point solvent can effectively improve the wettability of the adhesive, making it easier for the adhesive to penetrate into the wooden board material to improve the initial adhesion; by adding polycaprolactone, the compatibility of thermoplastic polyurethane and petroleum resin is effectively improved to form a uniform glue, thereby improving the initial adhesion of the adhesive; and the polycaprolactone resin has a low melting point and good fluidity, which can effectively improve the wettability of the adhesive during the bonding process, further improving the initial adhesion.
[0016] On the basis of the above technical solution, the present invention can also make the following technical improvements:
[0017] Furthermore, based on 100 parts by weight of all components, the weight fraction of the first solvent is 1-8 parts.
[0018] The beneficial effect of adopting the above further technical solution is: adjusting the ratio of the first solvent and the second solvent with different boiling points in the adhesive, after heating and curing, avoiding bulging and bubbles caused by too high solvent content, and avoiding poor wettability of the adhesive caused by too low content.
[0019] Furthermore, the boiling point of the first solvent is higher than 150°C.
[0020] The beneficial effects of adopting the above further technical solution are:
[0021] The high-boiling-point first solvent used in the organic solvent can ensure its low volatility, so that after the adhesive is heated and cured, the residual organic solvent is mainly a high-boiling-point solvent, thereby reducing the amount of solvent volatilization during the placement process and reducing the occurrence of bulging; at the same time, a small amount of high-boiling-point solvent residue in the organic solvent can effectively improve the wettability of the adhesive, making it easier for the glue to penetrate into the board.
[0022] Furthermore, the first solvent is N,N-dimethylformamide (DMF) or methyl nylonate (DBE); the second solvent is one or a combination of ethyl acetate, acetone, toluene and dimethyl carbonate.
[0023] Wherein, the nylon acid methyl ester (DBE) is a mixture of three divalent acid esters, namely, dimethyl succinate (CH3OOC(CH2)2COOCH3), dimethyl glutarate (CH3OOC(CH2)3COOCH3) and dimethyl adipate (CH3OOC(CH2)4COOCH3), and the ester content of nylon acid methyl ester (DBE) is greater than 99%.
[0024] The boiling point of ethyl acetate is 77.1° C., the boiling point of acetone is 56.2° C., the boiling point of toluene is 111.0° C., and the boiling point of dimethyl carbonate is 90-91° C. During the heating and curing process of the adhesive, the second solvent can be completely volatilized.
[0025] Furthermore, the number average molecular weight of the polycaprolactone is 30000-100000 g / mol.
[0026] Further, the polycaprolactone is Capa TM 6500.
[0027] The beneficial effect of adopting the above further technical solution is that the polycaprolactone resin has a low melting point and good fluidity, which can effectively improve the wettability of the glue during the bonding process and further improve the initial adhesion of the adhesive.
[0028] Furthermore, the tackifying resin is one or a combination of light-colored or colorless petroleum resins.
[0029] Furthermore, the petroleum resin is C5 or C9.
[0030] The beneficial effects of adopting the above further technical solution are:
[0031] Colorless C5 and C9 petroleum resins are used to improve the appearance of the substrate and the decorative film layer after bonding. At the same time, polycaprolactone is used to improve the compatibility between the petroleum resin and thermoplastic polyurethane, thereby forming a uniform adhesive.
[0032] Furthermore, the thermoplastic polyurethane is prepared from isocyanate and polyester polyol, the isocyanate is MDI, the polyester polyol is poly(hexanediol adipate), and the number average molecular weight of the poly(hexanediol adipate) is 2500-5000 g / mol.
[0033] The second aspect of the present invention is to provide a method for preparing the above-mentioned adhesive for bonding wood boards, comprising the following steps:
[0034] Add the organic solvent into the stirring kettle, raise the temperature to 30-50°C, control the rotation speed to 300-500 r / min, then add thermoplastic polyurethane and polycaprolactone, stir for 1-2h, then add petroleum resin and stir for 1-2h to prepare the adhesive.
[0035] The present invention also provides application of the adhesive for bonding wooden boards, wherein the adhesive is used in combination with a curing agent.
[0036] Compared with the prior art, the present invention has the following technical effects:
[0037] (1) The adhesive for bonding wood boards obtained by the present invention has a wide range of applications. When applied to light-colored films such as white, it does not cause color development, thereby improving the appearance of the product.
[0038] (2) The adhesive for bonding wood boards obtained by the present invention has the characteristics of high initial bonding strength, good initial bonding force, easy coating, and no blistering, and can be widely used in bonding substrates such as solid wood, composite boards, and fiberboards of different densities with decorative layers. DETAILED DESCRIPTION
[0039] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0040] The “parts” in the following examples and comparative examples all refer to parts by mass.
[0041] Example 1
[0042] 20 parts of thermoplastic polyurethane particles, 10 parts of C5, 5 parts of DBE, 30 parts of ethyl acetate, 30 parts of acetone, 5 parts of Capa TM 6500 made into adhesive;
[0043] The thermoplastic polyurethane particles are synthesized by using MDI and poly(hexanediol adipate) (R value is 0.95, i.e. the molar ratio of isocyanate group (NCO) to hydroxyl group (OH) is 0.95), and the number average molecular weight of poly(hexanediol adipate) is 3000 g / mol;
[0044] Add DBE, ethyl acetate and acetone into the stirring tank, raise the temperature of the stirring tank to 40°C, adjust the speed to 400r / min, and then add thermoplastic polyurethane particles and Capa TM 6500, stir for 1.5h, then add C5 and stir for 1.5h to obtain the finished product.
[0045] Example 2
[0046] 10 parts of thermoplastic polyurethane particles, 20 parts of C5, 1 part of DBE, 30 parts of ethyl acetate, 29 parts of acetone, 10 parts of Capa TM 6500 made into adhesive;
[0047] The thermoplastic polyurethane particles are synthesized by using MDI and poly(hexanediol adipate) (R value is 0.95, i.e. the molar ratio of isocyanate group (NCO) to hydroxyl group (OH) is 0.95), and the number average molecular weight of poly(hexanediol adipate) is 3000 g / mol;
[0048] Add DBE, ethyl acetate and acetone into a stirring tank, raise the temperature of the stirring tank to 40°C, adjust the speed to 400r / min, then add thermoplastic polyurethane particles and CapaTM6500, stir for 1.5h, then add C5 and stir for 1.5h to obtain the finished product.
[0049] Example 3
[0050] An adhesive was prepared using 15 parts of thermoplastic polyurethane particles, 15 parts of C5, 3 parts of DBE, 30 parts of ethyl acetate, 30 parts of acetone, and 7 parts of CapaTM6500;
[0051] The thermoplastic polyurethane particles are synthesized by using MDI and poly(hexanediol adipate) (R value is 0.95, i.e. the molar ratio of isocyanate group (NCO) to hydroxyl group (OH) is 0.95), and the number average molecular weight of poly(hexanediol adipate) is 3000 g / mol;
[0052] Add DBE, ethyl acetate and acetone into a stirring tank, raise the temperature of the stirring tank to 40°C, adjust the speed to 400r / min, then add thermoplastic polyurethane particles and CapaTM6500, stir for 1.5h, then add C5 and stir for 1.5h to obtain the finished product.
[0053] Comparative Example 1
[0054] An adhesive was prepared using 20 parts of thermoplastic polyurethane particles, 10 parts of C5, 5 parts of DBE, 30 parts of ethyl acetate, and 30 parts of acetone;
[0055] The rest is the same as in Example 1.
[0056] Comparative Example 2
[0057] Using 20 parts of thermoplastic polyurethane particles, 5 parts of DBE, 30 parts of ethyl acetate, and 30 parts of acetone;
[0058] The rest is the same as in Example 1.
[0059] Comparative Example 3
[0060] 20 parts of thermoplastic polyurethane particles, 10 parts of C5, 30 parts of ethyl acetate, 30 parts of acetone, 5 parts of Capa TM 6500 made into adhesive;
[0061] The rest is the same as in Example 1.
[0062] Comparative Example 4
[0063] 15 parts of thermoplastic polyurethane particles, 5 parts of C5, 15 parts of DBE, 20 parts of ethyl acetate, 20 parts of acetone, 5 parts of Capa TM 6500 made into adhesive;
[0064] The rest is the same as in Example 1.
[0065] Performance Testing
[0066] The performance of the prepared adhesive was tested by laminating bamboo fiberboard with glued PVC. The tape size was 25 mm wide. The specific test process was as follows:
[0067] The initial bonding strength test was carried out using a micro tensile machine. The initial bonding strength was tested 10 minutes after the PVC film and the bamboo fiberboard were glued together. The bonded bamboo fiberboard was placed in a 30°C oven for 24 hours to see if there were any bulges.
[0068] The test results are shown in Table 1.
[0069] Table 1 Performance test results of embodiments and comparative examples
[0070]
[0071] It can be seen from the data in Table 1 that the adhesives prepared in Examples 1-3 of the present invention have high initial viscosity, do not bubble, and do not develop color. Although the adhesive obtained in Comparative Example 3 has normal color and no bulging, its initial viscosity is relatively low, which is far less than the initial viscosity of the adhesives obtained in the examples of the present application.
[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An adhesive for bonding wood boards, characterized in that: In parts by mass, it includes the following components: 10-20 parts of thermoplastic polyurethane, 5-10 parts of polycaprolactone, 10-20 parts of tackifying resin, 50-80 parts of organic solvent; The organic solvent includes a first solvent and a second solvent, and the boiling point of the first solvent is higher than that of the second solvent.
2. The adhesive for bonding wood boards according to claim 1, characterized in that: Based on 100 parts by weight of all components, the weight fraction of the first solvent is 1-5 parts.
3. The adhesive for bonding wood boards according to claim 1, characterized in that: The boiling point of the first solvent is higher than 150°C.
4. The adhesive for bonding wood boards according to claim 1, characterized in that: The first solvent is N,N-dimethylformamide (DMF) or methyl nylonate (DBE); the second solvent is one or a combination of ethyl acetate, acetone, toluene and dimethyl carbonate.
5. The adhesive for bonding wood boards according to claim 1, characterized in that: The number average molecular weight of the polycaprolactone is 30000-100000 g / mol.
6. The adhesive for bonding wood boards according to claim 5, characterized in that: The polycaprolactone is Capa TM 6500.
7. The adhesive for bonding wood boards according to claim 1, characterized in that: The tackifying resin is one or a combination of light-colored or colorless petroleum resins.
8. The adhesive for bonding wood boards according to claim 1, characterized in that: The thermoplastic polyurethane is prepared from isocyanate and polyester polyol, the isocyanate is MDI, the polyester polyol is polyhexanediol adipate, and the number average molecular weight of the polyhexanediol adipate is 2500-5000 g / mol.
9. A method for preparing the adhesive for bonding wood boards according to any one of claims 1 to 8, characterized in that: The following steps are involved: Add the organic solvent into the stirring kettle, raise the temperature to 30-50°C, control the rotation speed to 300-500 r / min, then add thermoplastic polyurethane and polycaprolactone, stir for 1-2h, then add petroleum resin and stir for 1-2h to prepare the adhesive.
10. An application of the adhesive for bonding wood boards according to any one of claims 1 to 8, characterized in that: The adhesive is used in combination with a curing agent.