Ordered high-water-retention cathode catalyst layer and application thereof

By introducing an ordered high-water-retaining intermediate layer and hydrophobic carbon paper material into the cathode catalytic layer, the electrolytic performance degradation and durability problems caused by disordered film electrodes are solved, and more efficient hydrogen production and electrolytic cell durability are achieved.

CN119082754APending Publication Date: 2024-12-06GUANGDONG MINGYANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411278998.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The disordered membrane electrode structure leads to an increase in mass transfer resistance and an increase in charge impedance during electrolysis, reducing hydrogen production rate, increasing electrolytic energy consumption, and affecting the contact between the catalytic layer and the ion exchange membrane, resulting in water shortage at the cathode interface, affecting Electrolytic properties and durability.

Method used

The ordered high-water-retaining cathode catalytic layer consisting of the exchange membrane base layer, the ordered high-water-retaining intermediate layer and the cathode catalytic layer are used to inject hydrophilic materials and ionomers into the anodic aluminum AAO template to form a gradient cone. The active site and structure of the catalyst are optimized by combining hydrophobic carbon paper as the cathode gas diffusion layer material.

Benefits of technology

Significantly improve the performance and efficiency of the catalyst, maintain the wet state of the cathode electrode, improve electrolyte conduction and diffusion of reactant substances, extend the service life of the electrode, and improve electrolytic efficiency and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082754A_ABST
    Figure CN119082754A_ABST
Patent Text Reader

Abstract

The invention discloses an ordered high-water-retention cathode catalyst layer which is composed of an exchange membrane substrate layer, an ordered high-water-retention middle layer and a cathode catalyst layer in sequence, and the ordered high-water-retention middle layer is composed of a hydrophilic material and an ionomer. According to the invention, the film of the oxide and the ionomer is added as the water-retaining intermediate layer, the supply of water at the three-phase interface of the cathode is increased, then the hydrophobic carbon paper is selected as a cathode gas diffusion layer material, the loss of water at the GDL is effectively delayed, and a good water-retaining function can be formed at the interface of the cathode catalyst layer through the combined use of the oxide and the ionomer; the electrolysis efficiency and the durability of the electrolytic cell are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen production by electrolysis of water using anion exchange membranes, and relates to an ordered high water-retention cathode catalyst layer and an application thereof. Background Art

[0002] Anion exchange membrane water electrolysis (AEMWE) is an emerging method for efficient and low-cost hydrogen production. Compared with other water electrolysis technologies, AEMWE uses lower-cost non-precious metal catalysts and anion exchange membranes, and the electrolyzer performance can reach 1-2 A / cm at 60°C. 2 Although not yet commercialized on a large scale, AEMWE technology has great potential to improve the efficiency and reduce the cost of hydrogen production.

[0003] Among them, the disordered membrane electrode structure is a major factor hindering the performance improvement of AEMWE. The disordered membrane electrode will lead to an increase in mass transfer resistance and an increase in charge transfer impedance during electrolysis, thereby reducing the hydrogen production rate and increasing electrolysis energy consumption. In addition, disorder may also lead to poor contact between the catalyst layer and the ion exchange membrane, affecting the transmission efficiency of protons or ions, and thus affecting the overall hydrogen production performance.

[0004] In order to save costs and extract high-purity hydrogen more quickly on the cathode side, most of the current mainstream AEM electrolyzers adopt a single-side electrolyte feeding method at the anode. However, under the single-anode side feeding condition, the effect of maintaining sufficient water as a reactant at the cathode end only through the limited water permeability of the anion membrane is limited, and this feeding method will lead to a decrease in the performance of the electrolyzer; at the same time, the lack of water at the cathode end hinders the exchange of heat and easily leads to the generation of local high temperature. The long-term water-deficient environment accelerates the degradation of the anion membrane and ionomer, resulting in a decrease in the durability of the electrolyzer.

[0005] Feeding on the single anode side can easily lead to water shortage at the cathode interface. First, water shortage will directly affect the electrolysis efficiency of water, resulting in a decrease in hydrogen production capacity; second, water shortage will reduce the proton transfer efficiency, increase the resistance of the electrolyzer, and thus increase the energy required for electrolysis; third, the catalyst on the cathode side usually requires a hydrated environment to maintain activity. Water shortage may lead to the deactivation of the catalyst active sites, resulting in the loss of catalyst on the cathode electrode during long-term operation; fourth, long-term water shortage operation will aggravate the loss of anion exchange membranes and electrode materials, affecting the durability of the electrolyzer. Summary of the invention

[0006] The object of the present invention is to overcome at least one disadvantage of the prior art and to provide an ordered high water-retaining cathode catalyst layer and its application.

[0007] The technical solution adopted by the present invention is: In a first aspect, the present invention provides an ordered high water retention cathode catalyst layer, which is composed of an exchange membrane substrate layer, an ordered high water retention middle layer and a cathode catalyst layer in sequence, wherein the ordered high water retention middle layer is composed of a hydrophilic material and an ionomer.

[0008] In some examples, the hydrophilic material is selected from at least one of oxides or hydroxides of titanium, aluminum, silicon, zirconium, molybdenum, cobalt, niobium, tantalum, iron, and nickel.

[0009] In some examples, the ionomer is selected from any one of polyaryl, polynorbornene, polyetheretherketone, polybenzimidazole, polysulfone, and polyether high molecular polymers developed by Mingyang Company.

[0010] In some examples, the mass ratio of the hydrophilic material to the ionomer is 1:(0.05-0.5).

[0011] In some examples, the cathode catalyst layer includes a catalyst and an ionomer.

[0012] In some examples, the catalyst is selected from at least one of Pt / C, PtRu / C, transition metal (Ni, Fe, Co) nanoparticles, transition metal oxides, transition metal hydroxides, transition metal sulfides, and transition metal phosphides.

[0013] In some examples, the mass ratio of the catalyst to the ionomer is 1:(0.1-0.5).

[0014] In some embodiments, the exchange membrane substrate layer is selected from the polyaryl, polyphenylene ether, polyarylether, polyolefin, polybenzimidazole, polyetherketone, polyarylethernitrile, polyaromatic hydrocarbon or aromatic polymer ion exchange membrane without ether oxygen bond developed by Mingyang Company, and the commercially available Fumatech: Fumasep® FAA3 series, Tokuyama: A201 series, Ionomr: AEMION TM Series, Dioxide Materials: SUSTAINION® Series, Orion Polymer: TM1 Series, Versogen: PiperIon TM One of the series of anion exchange membranes. The preparation method of the self-developed exchange membrane substrate material can be found in CN118546339A.

[0015] In some examples, the method for preparing the ordered high water retention cathode catalyst layer comprises the following steps: 1) Inject evenly dispersed hydrophilic material and ionomer into the anodized aluminum oxide (AAO) template and heat at 50-85°C for 15-60 minutes; 2) removing the anodic aluminum oxide AAO template, transferring the high water retention oxide film to the anion exchange membrane through a hot pressing transfer process, and then spraying the cathode catalyst layer onto the surface of the high water retention oxide intermediate layer to prepare the ordered high water retention cathode catalyst layer.

[0016] In a second aspect, the use of the ordered high water-retention cathode catalyst layer provided in the first aspect of the present invention in the preparation of a membrane electrode for water electrolysis is characterized in that the cathode gas diffusion layer material of the membrane electrode is selected from surface hydrophobic carbon paper.

[0017] The beneficial effects of the present invention are: The present invention, based on single anode side feed, constructs an ordered cathode water-retaining catalytic layer, which can form an ordered catalytic layer, optimize the arrangement and structure of active sites, significantly improve the performance of the catalyst, and enhance its activity, selectivity, stability and efficiency; On the other hand, the construction of the water-retaining layer can effectively keep the cathode electrode moist, maintain a certain amount of water to promote the conduction of the electrolyte and the diffusion of the reactants, thereby better maintaining the activity of the catalyst. At the same time, the water-retaining layer provides a proton transfer channel to improve the efficiency and stability of the electrochemical reaction. The appropriate water-retaining layer design can reduce the corrosion and deactivation rate of the cathode electrode and extend the service life of the electrode. By adding an oxide + ionomer film as a water-retaining intermediate layer, the water supply at the cathode three-phase interface is increased, and hydrophobic carbon paper is selected as the cathode gas diffusion layer material to effectively delay the loss of water at the GDL. The combination of the two can form a good water-retaining function at the cathode catalyst layer interface, thereby improving the electrolysis efficiency and the durability of the electrolyzer; By using the AAO template to prepare the water-retaining layer, a gradient cone array of oxide water-retaining intermediate layers can be formed. The AAO template provides a highly ordered nanoporous structure for the water-retaining layer, which helps to achieve a uniform distribution of active sites in the catalytic layer and can increase the contact area between the catalytic layer and the reactants, thereby improving the catalytic activity and reaction rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The flowchart is a preparation process of the cathode ordered membrane electrode containing a high water-retaining oxide intermediate layer in each example of the present invention.

[0019] Figure 2 This is a schematic diagram of the cathode ordered membrane electrode structure containing a high water-retaining oxide intermediate layer of the present invention.

[0020] Figure 3 It is a polarization performance curve diagram of the membrane electrode of Examples 1-3 and Comparative Examples 1-2.

[0021] Figure 4The durability test diagram of the membrane electrode of Examples 1-3 and Comparative Examples 1-2. DETAILED DESCRIPTION

[0022] The following disclosure provides many different implementations or examples for implementing different solutions of the present invention. The preparation flow chart of the cathode ordered membrane electrode containing a high water retention oxide intermediate layer in each embodiment of the present invention is as follows: Figure 1 shown.

[0023] Example 1 1) Preparation of ordered high water-retention intermediate layer: Take 1g of polyaryl resin in 9.47g of methanol, stir at room temperature until the ionomer is dissolved, add 9.47g of deionized water and continue stirring for 15 minutes, add 10g of titanium dioxide dispersion (20wt%) and ultrasonically stir for half an hour. Take an appropriate amount of the above solution and drop it into the pores of the cleaned AAO template, and heat it at 60℃ for one hour. Then soak the AAO template in 1 mol / L alkaline solution for 15 minutes to remove the membrane and obtain a high water-retention titanium oxide array membrane. After the high water-retention oxide array membrane is washed and dried, it is hot pressed at 2 MPa and 200℃ for 3 min, and the array membrane is pressed onto one side of the anion exchange membrane; 2) Preparation of cathode ordered membrane electrode: Take 0.67 g of polyaryl resin in 15.2 g of methanol, stir at room temperature until the solid is dissolved, then add 45.6 g of n-propanol and 15.2 g of deionized water, and continue stirring for one hour. After filtering the ionomer solution, add 3.3 g of platinum carbon particles, stir and ultrasonicate for one hour to obtain a catalyst slurry. Platinum carbon is deposited on the surface of the hot-pressed oxide array membrane by a flat-plate spraying device, and the platinum loading is 0.5 mg / cm 2 , kept warm on a hot plate at 60°C for 20 minutes, then transferred to an oven and dried at 50°C for 3 hours to obtain a cathode ordered membrane electrode containing a high water-retaining oxide intermediate layer.

[0024] 3) Preparation of membrane electrode: Same as step 2, nickel ferrite (NiFe2O4) was selected as the anode catalyst to prepare the anode catalyst slurry, and sprayed on the other side of the anion membrane, with an effective loading of 1 mg / cm 2 , forming the final membrane electrode structure.

[0025] Example 2 The difference between this embodiment and embodiment 1 lies in the preparation of the ordered high water retention intermediate layer in step 1), and the specific operation is as follows: Take 1g of polyaryl resin in 14.5g of methanol, stir at room temperature until the ionomer is dissolved, add 14.5g of deionized water and continue stirring for 15 minutes, add 20g of titanium dioxide dispersion (20wt%) and stir ultrasonically for half an hour. Take an appropriate amount of the above solution and drop it into the pores of the cleaned AAO template, and heat it at 60℃ for one hour. Then soak the AAO template in 1 mol / L alkali solution for 15 minutes to remove the membrane and obtain a high water-retaining titanium oxide array membrane. After the high water-retaining oxide array membrane is washed and dried, it is hot pressed at 2 MPa and 200℃ for 3 min, and the array membrane is pressed onto one side of the anion exchange membrane.

[0026] Example 3 The difference between this embodiment and embodiment 1 lies in the preparation of the ordered high water retention intermediate layer in step 1), and the specific operation is as follows: Take 1g of polybenzimidazole resin in 6.31g of methanol, stir at room temperature until the ionomer is dissolved, add 6.31g of n-propanol and deionized water in turn and continue stirring for 15 minutes, add 10g of nano zirconium oxide dispersion (20wt%) and ultrasonically stir for half an hour. Take an appropriate amount of the above solution and drop it into the pores of the cleaned AAO template, and heat it at 60℃ for one hour. Then soak the AAO template in 1mol / L alkali solution for 15 minutes to remove the membrane, and obtain a high water retention zirconium oxide array membrane. After the high water retention oxide array membrane is washed and dried, it is hot pressed at 2 MPa and 200℃ for 3 min, and the array membrane is pressed onto one side of the anion exchange membrane.

[0027] Comparative Example 1 The difference from Example 1 is that step 1 is omitted, and the cathode catalyst slurry and the anode catalyst slurry are directly sprayed on both sides of the anion exchange membrane. The operation steps and spraying load are consistent with those in Example 1.

[0028] Comparative Example 2 The difference between this embodiment and embodiment 1 lies in the preparation of the ordered high water retention intermediate layer in step 1), and the specific operation is as follows: Take 1g of polyaryl resin in 9.47g of methanol, stir at room temperature until the ionomer is dissolved, add 9.47g of deionized water and continue stirring for 15 minutes, add 5g of titanium dioxide dispersion (20wt%) and ultrasonically stir for half an hour, the mass ratio of hydrophilic material to ionomer is 1:1. Take an appropriate amount of the above solution and drop it into the pores of the cleaned AAO template, and heat it at 60℃ for one hour. Then soak the AAO template in 1 mol / L alkali solution for 15 minutes to remove the membrane, and obtain a high water retention titanium oxide array membrane. After the high water retention oxide array membrane is washed and dried, it is hot pressed at 2 MPa and 200℃ for 3 min, and the array membrane is pressed onto one side of the anion exchange membrane.

[0029] Membrane electrode test like Figure 2 As shown, the AEM device was assembled, and the membrane electrode prepared in the above examples was selected as the core material, the hydrophobic carbon paper + nickel felt combination was used as the cathode gas diffusion layer, and the nickel felt was used as the anode gas diffusion layer. The effective area of ​​MEA was 25 cm 2 , 1 mol / L KOH as electrolyte, alkali solution temperature of 40-80 ℃, flow rate of 125 ml / min. The self-developed AEM test bench was used to carry out polarization performance test and durability test of relevant membrane electrodes. The polarization performance test of AEM membrane electrode was carried out in the voltage range of 1.6 V to 2.4 V; the stability test was carried out by applying a constant current (1 A / cm 2 ), observe the change trend of the overall membrane electrode voltage over time.

[0030] Polarization performance test Figure 3 As shown, in the high voltage range (1.9 V - 2.4 V), due to the introduction of the high water retention layer, the cathode end three-phase interface can maintain more sufficient water as a reactant, which promotes the continuous progress of the hydrogen evolution half-reaction. At the same time, the ordering of the cathode catalyst layer significantly increases the surface area of ​​the overall catalyst layer, provides more active sites, and promotes the improvement of electrolysis performance. Compared with Comparative Example 1, the performance of Example 1 at an operating voltage of 2.0 V is improved by 36.01%, Example 2 is improved by 12.52%, and Example 3 is improved by 16.17%.

[0031] Durability test Figure 4 As shown. At 1 A / cm 2 In the constant current density and 200-hour continuous operation test, the voltage change values ​​of Examples 1-3 are smaller than those of Comparative Examples 1-2, and the membrane electrode performance attenuation is significantly reduced, indicating that the design of the ordered water electrolysis electrode with a high water-retaining oxide intermediate layer in the present invention is an effective method to improve the durability of the electrolyzer.

[0032] The above is a further detailed description of the present invention, which should not be regarded as a limitation on the specific implementation of the present invention. For ordinary technicians in the technical field to which the present invention belongs, simple deduction or replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A cathode catalyst layer for electrolyzing water using an ordered high water retention anion exchange membrane, characterized in that: It is composed of an exchange membrane substrate layer, an ordered high water retention middle layer and a cathode catalyst layer in sequence, wherein the ordered high water retention middle layer is composed of a hydrophilic material and an ionomer.

2. The cathode catalyst layer according to claim 1, characterized in that: The hydrophilic material is selected from at least one of oxides or hydroxides of titanium, aluminum, silicon, zirconium, molybdenum, cobalt, niobium, tantalum, iron and nickel.

3. The cathode catalyst layer according to claim 1, characterized in that: The ionomer is selected from any one of polyaryl, polynorbornene, polyetheretherketone, polybenzimidazole, polysulfone and polyether high molecular polymer developed by Mingyang Company.

4. The cathode catalyst layer according to any one of claims 1 to 3, characterized in that: The mass ratio of the hydrophilic material to the ionomer is 1:(0.05-0.5).

5. The cathode catalyst layer according to claim 1, characterized in that: The cathode catalyst layer includes a catalyst and an ionomer.

6. The cathode catalyst layer according to claim 5, characterized in that: The catalyst is selected from one or more of Pt / C, PtRu / C, transition metal nanoparticles, transition metal oxides, transition metal hydroxides, transition metal sulfides, and transition metal phosphides.

7. The cathode catalyst layer according to claim 3 or 6, characterized in that: The mass ratio of the catalyst to the ionomer is 1:(0.1-0.5).

8. The cathode catalyst layer according to claim 1, characterized in that: The exchange membrane substrate layer is selected from the polyaryl, polyphenylene ether, polyarylether, polyolefin, polybenzimidazole, polyetherketone, polyarylethernitrile, polyaromatic hydrocarbon or aromatic polymer ion exchange membrane without ether oxygen bond developed by Mingyang Company, and the commercially available Fumatech: Fumasep® FAA3 series, Tokuyama: A201 series, Ionomr: AEMION TM Series, Dioxide Materials: SUSTAINION® Series, OrionPolymer: TM1 Series, Versogen: PiperIon TM One of a series of anion exchange membranes.

9. The cathode catalyst layer according to any one of claims 1 to 8, characterized in that: The method for preparing the ordered high water retention cathode catalyst layer comprises the following steps: 1) Inject evenly dispersed hydrophilic material and ionomer into the anodized aluminum oxide (AAO) template and heat at 50-85°C for 15-60 minutes; 2) removing the anodic aluminum oxide AAO template, transferring the high water retention oxide film to the anion exchange membrane through a hot pressing transfer process, and then spraying the cathode catalyst layer onto the surface of the high water retention oxide intermediate layer to prepare the ordered high water retention cathode catalyst layer.

10. Use of the cathode catalyst layer according to any one of claims 1 to 8 in preparing a membrane electrode for water electrolysis, characterized in that: The cathode gas diffusion layer material of the membrane electrode is selected from surface hydrophobic carbon paper.