Luminescent layer structure, composite insertion layer structure and preparation method and application thereof

By adopting a composite insertion layer structure in the nitride light emitting diode LED, the hybridization distribution of AlN and SiN microstructures reduces stress and improves radiation recombination efficiency, the problem of low stress and efficiency of the nitride light emitting layer in the prior art is solved, and the problem of low stress and efficiency of the nitride light emitting layer in the prior art is realized. Higher LED brightness and leakage performance.

CN119092606AActive Publication Date: 2024-12-06JIANGSU INST OF ADVANCED SEMICON CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411183479.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The light emission intensity and efficiency of existing nitride light-emitting diode LEDs are mainly due to the mismatch of lattice constants and differences in thermal expansion coefficients caused by difficulty in growing GaN materials, which makes it difficult to achieve epitaxial growth of high-quality nitride materials, thereby reducing the brightness and efficiency of LEDs.

Method used

The composite insertion layer structure is adopted, including AlN and SiN layers stacked in sequence in selected directions, through heat treatment, Al and Si atoms bind to N atoms to form AlN and SiN microstructures, forming multiple AlN and SiN microstructures with hybrid distributions. Reduce the stress of the luminescent layer and improve the radiation recombination efficiency.

Benefits of technology

It effectively reduces the stress of the luminescent layer in the epitaxial sheet, improves the brightness and radiation recombination efficiency of the LED, and enhances the crystal quality and leakage performance of the luminescent layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092606A_ABST
    Figure CN119092606A_ABST
Patent Text Reader

Abstract

The invention discloses a light-emitting layer structure, a composite insertion layer structure and a preparation method and application of the light-emitting layer structure and the composite insertion layer structure. The composite insertion layer structure comprises at least one composite insertion layer unit, and each composite insertion layer unit comprises a first AlN layer, a first SiN layer, a second AlN layer and a second SiN layer which are sequentially stacked in a selected direction, and a plurality of AlN microstructures and a plurality of SiN microstructures which are distributed in a crossing manner are arranged in a laminated structure layer formed by the first AlN layer, the first SiN layer and the second AlN layer. According to the invention, the stress of the light-emitting layer in the epitaxial wafer is reduced, the radiation recombination efficiency in the light-emitting layer is enhanced, and the brightness of the LED epitaxial wafer is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention particularly relates to a light-emitting layer structure, a composite insertion layer structure, a preparation method and application thereof, and belongs to the technical field of semiconductor devices. Background Art

[0002] Nitride light emitting diode (LED) is a semiconductor light emitting device with the advantages of long life, low energy consumption, small size and high reliability. It plays an increasingly important role in large-screen color display, traffic lights and lighting fields. However, there are still problems of low luminous intensity and efficiency. Further improving the luminous intensity and efficiency of LED is the goal that LED lighting display application technology is constantly pursuing.

[0003] LED production process generally goes through three stages: epitaxial growth, chip manufacturing and packaging. Epitaxial growth determines more than 80% of the brightness of LED and is the core of the entire industry chain. At present, due to the lack of GaN single crystal materials in nature and the extremely difficult growth of bulk single crystal GaN, the growth of GaN materials mainly adopts heteroepitaxial method. Due to the large lattice constant mismatch and thermal expansion coefficient difference between substrate materials and III-V group nitride semiconductor materials, it is very difficult to epitaxially grow high-quality nitride materials. At the same time, it will bring about polarization effect in the nitride light-emitting layer, and the electrons and holes will be separated in space, which reduces the overlap of electron and hole wave functions in the active area, reduces the probability of radiation recombination, and thus reduces the brightness of LED and causes efficiency droop effect. Summary of the invention

[0004] The main purpose of the present invention is to provide a light-emitting layer structure, a composite insertion layer structure and a preparation method and application thereof, so as to overcome the deficiencies in the prior art.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0006] A first aspect of the present invention provides a composite insertion layer structure, comprising at least one composite insertion layer unit, wherein the composite insertion layer unit comprises a first AlN layer, a first SiN layer, a second AlN layer and a second SiN layer stacked in sequence along a selected direction, wherein the interior of the stacked structure layer formed by the first AlN layer, the first SiN layer and the second AlN layer has a plurality of AlN microstructures and a plurality of SiN microstructures that are intertwined and distributed.

[0007] A second aspect of the present invention provides a method for preparing a composite insert layer structure, comprising:

[0008] The step of making a precursor for forming a composite insert layer structure, the precursor comprising a first Al layer, a Si layer, and a second Al layer stacked in a selected direction;

[0009] At least under the condition that a Si source and a N source coexist, the precursor is heat-treated to make at least part of the Al atoms in the first Al layer and the second Al layer and part of the Si atoms in the Si layer mutually dissolve and diffuse, and at least part of the Al atoms and at least part of the Si atoms in the precursor are respectively combined with the N atoms provided by the N source to form AlN and SiN, and part of the Si atoms in the Si source are also combined with part of the Si atoms in the N source to form SiN, thereby forming a composite insertion layer unit.

[0010] The third aspect of the present invention provides a light-emitting layer structure, which includes at least one quantum well layer and at least one quantum barrier layer stacked in sequence along a selected direction, the quantum barrier layer includes at least two barrier layers stacked along the selected direction and at least one composite insertion layer, wherein at least one composite insertion layer is arranged between two adjacent barrier layers, and the composite insertion layer includes the composite insertion layer structure.

[0011] A fourth aspect of the present invention provides an epitaxial wafer comprising the light-emitting layer structure.

[0012] A fifth aspect of the present invention provides a light-emitting device, which includes the epitaxial wafer.

[0013] Compared with the prior art, the present invention reduces the stress of the light-emitting layer in the epitaxial wafer, enhances the radiation recombination efficiency in the light-emitting layer, and improves the brightness of the LED epitaxial wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a structural schematic diagram of an LED epitaxial wafer provided in a typical implementation case of the present invention;

[0015] Figure 2 It is a schematic structural diagram of a composite insertion layer provided in a typical implementation case of the present invention;

[0016] Figure 3 This is an electron microscope image of a partial structure of a composite insertion layer provided in a typical embodiment of the present invention;

[0017] Figure 4 It is a schematic diagram of a preparation process of an LED epitaxial wafer provided in a typical implementation case of the present invention;

[0018] Figure 5 It is a schematic diagram of a preparation process of a composite insertion layer provided in a typical implementation case of the present invention;

[0019] Figure 6 Schematic diagram of the structure of the composite insertion layer used in Comparative Example 1. DETAILED DESCRIPTION

[0020] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.

[0021] A first aspect of the present invention provides a composite insertion layer structure, comprising at least one composite insertion layer unit, wherein the composite insertion layer unit comprises a first AlN layer, a first SiN layer, a second AlN layer and a second SiN layer stacked in sequence along a selected direction, wherein the interior of the stacked structure layer formed by the first AlN layer, the first SiN layer and the second AlN layer has a plurality of AlN microstructures and a plurality of SiN microstructures that are intertwined and distributed.

[0022] Furthermore, the plurality of AlN microstructures include a plurality of first AlN microstructures and a plurality of second AlN microstructures, and the plurality of first AlN microstructures and the plurality of second AlN microstructures are distributed in the first SiN layer at intervals.

[0023] Furthermore, the plurality of SiN microstructures include a plurality of first SiN microstructures and a plurality of second SiN microstructures, the plurality of first SiN microstructures are distributed at intervals in the first AlN layer, and the plurality of second SiN microstructures are distributed at intervals in the second AlN layer.

[0024] Furthermore, the plurality of the first AlN microstructures are integrated with the first AlN layer, and the plurality of the second AlN microstructures are integrated with the second AlN layer.

[0025] Furthermore, the plurality of the first SiN microstructures and the plurality of the second SiN microstructures are integrated with the first SiN layer.

[0026] Furthermore, the second SiN layer has a plurality of nanopore structures therein.

[0027] Further, the nanopore structure is a through hole within a through hole that penetrates the second SiN layer along the selected direction.

[0028] Furthermore, the nanopore structure is formed by the discontinuity of the membrane structure of the second SiN layer itself.

[0029] In a more typical embodiment, the composite insertion layer structure includes: a plurality of the composite insertion layer units, and the plurality of the composite insertion layer units are stacked in sequence along the selected direction.

[0030] A second aspect of the present invention provides a method for preparing a composite insert layer structure, comprising:

[0031] The step of making a precursor for forming a composite insert layer structure, the precursor comprising a first Al layer, a Si layer, and a second Al layer stacked in a selected direction;

[0032] At least under the condition that a Si source and a N source coexist, the precursor is heat-treated to make at least part of the Al atoms in the first Al layer and the second Al layer and part of the Si atoms in the Si layer mutually dissolve and diffuse, and at least part of the Al atoms and at least part of the Si atoms in the precursor are respectively combined with the N atoms provided by the N source to form AlN and SiN, and part of the Si atoms in the Si source are also combined with part of the Si atoms in the N source to form SiN, thereby forming a composite insertion layer unit.

[0033] Further, the composite insertion layer unit comprises a first AlN layer, a first SiN layer, a second AlN layer and a second SiN layer sequentially stacked in a selected direction, the stacked structure layer formed by the first AlN layer, the first SiN layer and the second AlN layer has a plurality of AlN microstructures and a plurality of SiN microstructures interlaced and distributed inside, and the second SiN layer has a plurality of nanopore structures inside;

[0034] The first AlN layer is formed by combining a portion of Al atoms in the first Al layer with N atoms provided by the N source, the second AlN layer is formed by combining a portion of Al atoms in the second Al layer with N atoms provided by the N source, the first SiN layer is formed by combining a portion of Si in the Si layer with N atoms provided by the N source, a plurality of AlN microstructures are formed by combining a portion of Al atoms diffused from the first Al layer or the second Al layer into the Si layer or the first SiN layer with N atoms provided by the N source, and a plurality of SiN microstructures are formed by combining a portion of Si atoms diffused from the Si layer into the first Al layer / the first AlN layer, the second Al layer / the second AlN layer with N atoms provided by the N source.

[0035] Furthermore, the plurality of AlN microstructures include a plurality of first AlN microstructures and a plurality of second AlN microstructures, and the plurality of the first AlN microstructures and the plurality of the second AlN microstructures are distributed at intervals in the first SiN layer, the first AlN microstructure is formed by combining a portion of Al atoms diffused from the first Al layer into the Si layer or the first SiN layer with N atoms provided by the N source, and the second AlN microstructure is formed by combining a portion of Al atoms diffused from the second Al layer into the Si layer or the first SiN layer with N atoms provided by the N source.

[0036] Furthermore, the plurality of SiN microstructures include a plurality of first SiN microstructures and a plurality of second SiN microstructures, the plurality of first SiN microstructures are spaced apart in the first AlN layer, the plurality of second SiN microstructures are spaced apart in the second AlN layer, the first SiN microstructure is formed by combining a portion of Si atoms diffused from the Si layer into the first Al layer / the first AlN layer with N atoms provided by the N source, and the second SiN microstructure is formed by combining a portion of Si atoms diffused from the Si layer into the second Al layer / the second AlN layer with N atoms provided by the N source.

[0037] Further, the plurality of the first AlN microstructures are integrated with the first AlN layer, and the plurality of the second AlN microstructures are integrated with the second AlN layer.

[0038] Furthermore, the plurality of the first SiN microstructures and the plurality of the second SiN microstructures are integrated with the first SiN layer.

[0039] Furthermore, the heat treatment temperature is 900° C. to 1200° C., and the pressure is 100 torr to 500 torr.

[0040] Furthermore, when the precursor is heat-treated, the supply flow rate of the Si source is 10 scc to 300 sccm, and the supply flow rate of the N source is 2 slm to 50 slm.

[0041] Furthermore, the heat treatment time is 15s to 45s.

[0042] Furthermore, the second SiN layer has a plurality of nanopore structures therein.

[0043] Further, the nanopore structure is a through hole within a through hole that penetrates the second SiN layer along the selected direction.

[0044] Furthermore, the nanopore structure is formed by the discontinuity of the membrane structure of the second SiN layer itself.

[0045] The third aspect of the present invention provides a light-emitting layer structure, which includes at least one quantum well layer and at least one quantum barrier layer stacked in sequence along a selected direction, the quantum barrier layer includes at least two barrier layers stacked along the selected direction and at least one composite insertion layer, wherein at least one composite insertion layer is arranged between two adjacent barrier layers, and the composite insertion layer includes the composite insertion layer structure.

[0046] Further, the quantum barrier layer includes a first barrier layer, a second barrier layer and a third barrier layer stacked along the selected direction, and the composite insertion layer is stacked between the second barrier layer and at least one of the first barrier layer and the third barrier layer.

[0047] Furthermore, the quantum well layer and the quantum barrier layer are periodically and repeatedly stacked.

[0048] Furthermore, the quantum well layer and the quantum barrier layer are both made of nitride.

[0049] Furthermore, the materials of the quantum well layer and the quantum barrier layer are both III-V group nitrides.

[0050] Furthermore, the material of the quantum barrier layers is nitride containing Al.

[0051] A fourth aspect of the present invention provides an epitaxial wafer comprising the light-emitting layer structure.

[0052] A fifth aspect of the present invention provides a light-emitting device, which includes the epitaxial wafer.

[0053] The technical solution, its implementation process and principles will be further explained below in conjunction with the accompanying drawings and specific implementation cases. Unless otherwise specified, the semiconductor epitaxial growth, metal deposition, nitrogen heat treatment processes and equipment used in the embodiments of the present invention are known to those skilled in the art and are not specifically limited or described herein.

[0054] In a typical implementation case, please refer to Figure 1 , an LED epitaxial wafer, comprising a substrate and a first nitride layer, a nitride light-emitting layer and a second nitride layer sequentially stacked on the substrate along a selected direction, the nitride light-emitting layer comprising a nitride quantum well layer, a first nitride barrier layer, a composite insertion layer, a second nitride barrier layer and a third nitride barrier layer sequentially stacked on the first nitride layer along a selected direction, the second nitride layer being stacked on the third nitride barrier layer. It should be noted that, Figure 1 Only the case where a composite insertion layer is provided between the first nitride barrier layer and the second nitride barrier layer is shown. Of course, the composite insertion layer can also be provided between the second nitride barrier layer and the third nitride barrier layer, or a composite insertion layer can be provided between the first nitride barrier layer and the second nitride barrier layer and between the second nitride barrier layer and the third nitride barrier layer.

[0055] Specifically, the first nitride layer is an n-type doped nitride layer, and the doping concentration of the n-type impurities is 1×10 18 cm -3 1×10 19 cm -3More specifically, the material of the first nitride layer is a III-V group nitride. Exemplarily, the first nitride layer can be an n-type GaN layer, an n-type AlGaN layer, or an n-type InGaN layer. Specifically, the second nitride layer is a p-type doped nitride layer, and the doping concentration of the p-type impurity is 1×10 19 cm -3 ~1×10 21 cm -3 More specifically, the second nitride layer is made of III-V group nitride. Exemplarily, the second nitride layer may be a p-type GaN layer, a p-type AlGaN layer, or a p-type InGaN layer.

[0056] Specifically, the material of the nitride quantum well layer is group III-V nitride. Exemplarily, the nitride quantum well layer can be a GaN quantum well layer, an AlGaN quantum well layer, or an InGaN quantum well layer.

[0057] Specifically, the material of the first nitride barrier layer is a III-V group nitride. Exemplarily, the first nitride barrier layer can be a GaN barrier layer, an AlGaN barrier layer, or an InGaN barrier layer. Specifically, the second nitride barrier layer is mainly used to reduce the resistance of the nitride light-emitting layer, thereby reducing the operating voltage of the epitaxial wafer. Specifically, the material of the second nitride barrier layer is a III-V group nitride. Exemplarily, the second nitride barrier layer can be a GaN barrier layer, an AlGaN barrier layer, or an InGaN barrier layer, with a doping concentration of 2×10 17 cm -3 ~8×10 17 cm -3 Specifically, the material of the third nitride barrier layer is a III-V group nitride. Exemplarily, the third nitride barrier layer may be a GaN barrier layer, an AlGaN barrier layer, or an InGaN barrier layer.

[0058] Please also read Figure 2 and Figure 3 , the composite insert layer comprises at least one composite insert layer unit, Figure 2 The structure of a single composite insertion layer unit is shown, each of the composite insertion layer units includes a first AlN layer, a first SiN layer, a second AlN layer, and a second SiN layer stacked in sequence along a selected direction, wherein the interior of the stacked structure layer formed by the first AlN layer, the first SiN layer, and the second AlN layer has a plurality of AlN microstructures and a plurality of SiN microstructures that are intertwined and distributed.

[0059] Specifically, the plurality of AlN microstructures include a plurality of first AlN microstructures and a plurality of second AlN microstructures, the plurality of the first AlN microstructures and the plurality of the second AlN microstructures are spaced apart and distributed in the first SiN layer, the plurality of SiN microstructures include a plurality of first SiN microstructures and a plurality of second SiN microstructures, the plurality of the first SiN microstructures are spaced apart and distributed in the first AlN layer, and the plurality of the second SiN microstructures are spaced apart and distributed in the second AlN layer.

[0060] More specifically, the plurality of first AlN microstructures are integrated with the first AlN layer, the plurality of second AlN microstructures are integrated with the second AlN layer, and the plurality of first SiN microstructures and the plurality of second SiN microstructures are integrated with the first SiN layer.

[0061] On the one hand, the composite insertion layer in the present invention can effectively release the stress in the composite insertion layer through relaxation between the internal AlN and SiN polycrystalline interfaces, improve the crystal quality of the AlN layer / AlN microstructure, reduce the scattering of light by defects, and greatly improve the brightness and leakage performance of the epitaxial wafer; on the other hand, the composite insertion layer in the present invention increases the longitudinal extension distance of Si atoms with small atomic radius in the thickness direction, and the lattice constant modulation effect of the Al-containing nitride quantum barrier layer can be utilized by the introduction of Si atoms, and tensile stress can be further introduced into the nitride quantum barrier layer, which can better compensate for the compressive stress of the nitride quantum well layer, reduce the internal stress distribution of the nitride quantum well layer, improve the crystal quality and component uniformity of the nitride quantum well layer, and reduce non-radiative recombination. Furthermore, the surface of the composite insertion layer introduced by the present invention has a surface with a low N vacancy concentration distribution, which reduces the capture of holes, improves the uniformity of carrier distribution in the nitride light-emitting layer, improves the radiative recombination efficiency, and improves the brightness of the epitaxial wafer.

[0062] More specifically, the second SiN layer has a plurality of nanopore structures, and specifically, the nanopore structure is a through hole in the through hole that penetrates the second SiN layer along the selected direction, and more specifically, the nanopore structure is formed by the discontinuity of the membrane structure of the second SiN layer itself. The nanofilm layer tends to nucleate at the center of the dislocation, which can shield the surface dislocation of the composite insertion layer and prevent the dislocation from extending upward to form a leakage channel, and the N heat treatment can also form the filling of N vacancies, reduce the nitrogen vacancy defects on the surface of the composite insertion layer, and improve the leakage performance of the epitaxial wafer.

[0063] In a more specific implementation, please refer to Figure 4 , a method for preparing an LED epitaxial wafer, comprising the following steps:

[0064] (1) Providing a substrate, wherein the substrate is used to grow an LED epitaxial wafer, and the substrate may be a Si substrate, a GaN substrate, or a sapphire substrate, etc.

[0065] (2) A first nitride layer having a thickness of 1 μm to 10 μm is grown on the substrate at a temperature of 1050° C. to 1150° C. and a pressure of 100 torr to 500 torr.

[0066] Specifically, the first nitride layer is an n-type doped nitride layer, and the doping concentration of the n-type impurities is 1×10 18 cm -3 ~1×10 19 cm -3 More specifically, the material of the first nitride layer is group III-V nitride. Exemplarily, the first nitride layer can be an n-type GaN layer, an n-type AlGaN layer, or an n-type InGaN layer.

[0067] (3) growing a nitride light-emitting layer on the first nitride layer, specifically comprising:

[0068] S31: growing a nitride quantum well layer with a thickness of 1 nm to 8 nm on the first nitride layer at a temperature of 700° C. to 1000° C. and a pressure of 100 torr to 500 torr.

[0069] Specifically, the material of the nitride quantum well layer is group III-V nitride. Exemplarily, the nitride quantum well layer can be a GaN quantum well layer, an AlGaN quantum well layer, or an InGaN quantum well layer.

[0070] S32: Under the conditions of a temperature of 750°C to 1050°C and a pressure of 100 torr to 500 torr, a first nitride barrier layer (i.e., the aforementioned first barrier layer) with a thickness of 1 nm to 3 nm is grown on the nitride quantum well layer. The first nitride barrier layer serves as a contact layer of the nitride quantum well layer and also as a growth template for the composite insertion layer.

[0071] Specifically, the material of the first nitride barrier layer is group III-V nitride. Exemplarily, the first nitride barrier layer can be a GaN barrier layer, an AlGaN barrier layer, or an InGaN barrier layer.

[0072] S33: Please also refer to Figure 5 , growing a composite insertion layer on the first nitride barrier layer, comprising at least the following steps:

[0073] S331: Under the conditions of temperature of 500℃~1000℃, pressure of 200torr~300torr and reducing atmosphere, an Al source is introduced into the reaction chamber with an introduction flow rate of 100sccm~300sccm and maintained for 2s~10s to form a first Al deposition layer (i.e. the aforementioned first Al layer, the same below) on the first nitride barrier layer.

[0074] Specifically, the first deposited Al layer can play a blocking role when performing step S332, preventing Si atoms from crossing the first nitride barrier layer and entering the nitride quantum well layer, thereby avoiding the non-radiative recombination in the nitride quantum well layer, reduced brightness of the epitaxial wafer, and leakage problems caused thereby.

[0075] S332: Under a reducing gas atmosphere and a temperature of 500°C to 1000°C and a pressure of 200 torr to 300 torr, a Si source is introduced into the reaction chamber at a flow rate of 10 sccm to 300 sccm. Heat treatment is performed for 5s to 20s to form a Si deposition layer (i.e., the aforementioned Si layer, the same below) on the first Al deposition layer.

[0076] S333: Under the conditions of temperature of 500℃~1000℃, pressure of 100torr~200torr and reducing atmosphere, Al source is introduced into the reaction chamber with an introduction flow rate of 10sccm~100sccm. Heat treatment is performed for 5s~15s to form a second Al deposition layer (i.e. the aforementioned second Al layer, the same below) on the Si deposition layer, thereby forming a precursor of the composite insertion layer.

[0077] Specifically, the second Al deposition layer acts as a covering layer to block the Si atom enrichment in the Si deposition layer, thereby preventing the enriched Si from acting as a carrier scattering center and causing scattering of carriers during transmission in the nitride light-emitting layer, thereby reducing the carrier transmission capacity in the nitride light-emitting layer, and ultimately causing uneven distribution of carriers in the nitride light-emitting layer, affecting the luminescence performance.

[0078] S334: Under the conditions of a temperature of 900° C. to 1200° C., a pressure of 100 torr to 500 torr and a reducing atmosphere, a Si source and a N source are continuously introduced into the reaction chamber, the Si source flow rate is 10 sccm to 300 sccm, and the N source flow rate is 2 slm to 50 slm, and the precursor of the composite insertion layer is heat-treated for 15 s to 45 s, thereby converting the precursor of the composite insertion layer into a composite insertion layer, such as Figure 2 and Figure 3 shown.

[0079] Specifically, during the N and Si co-heat treatment process of step S334, on the one hand, Al atoms and Si atoms in the precursor of the composite insertion layer diffuse with each other, and under the N heat treatment, the first Al deposition layer and the second Al deposition layer, the diffused Al atoms form AlN, and the Si deposition layer and the diffused Si atoms form SiN, thereby forming an AlN and SiN stacked body with multiple AlN microstructures and multiple SiN microstructures with interlaced distribution. On the other hand, a part of Si atoms in the Si source treatment in step S334 and a part of N atoms that do not participate in the nitrogen heat reaction of the first and second Al deposition layers and the Si deposition layer combine to form a SiN layer with a nanometer-level thickness (i.e., the aforementioned second SiN layer), and are distributed on the surface of the AlN and SiN stacked body, and the SiN layer has multiple nanopore structures formed by discontinuity, and the nanofilm layer often nucleates at the center of the dislocation, which can shield the surface dislocation of the composite insertion layer and prevent the dislocation from extending upward to form a leakage channel, and the N heat treatment can also form the filling of N vacancies, reduce the nitrogen vacancy defects on the surface of the composite insertion layer, and improve the leakage performance of the epitaxial wafer.

[0080] Specifically, the AlN / SiN stack includes a first AlN layer, a first SiN layer, and a second AlN layer stacked in sequence, as well as a plurality of AlN microstructures and a plurality of SiN microstructures, wherein the plurality of AlN microstructures include a plurality of first AlN microstructures and a plurality of second AlN microstructures, wherein the plurality of first AlN microstructures and the plurality of second AlN microstructures are spaced apart in the first SiN layer, and the plurality of SiN microstructures include a plurality of first SiN microstructures and a plurality of second SiN microstructures, wherein the plurality of first SiN microstructures are spaced apart in the first AlN layer, and the plurality of second SiN microstructures are spaced apart in the second AlN layer, wherein the first AlN layer is formed by converting a portion of the first Al deposited layer through N heat treatment, and ... The first SiN layer is formed by converting a portion of the Si deposited layer through N heat treatment, the second AlN layer is formed by converting a portion of the second Al deposited layer through N heat treatment, the first AlN microstructure is formed by converting a portion of Al atoms diffused from the first Al deposited layer into the Si deposited layer through N heat treatment, the second AlN microstructure is formed by converting a portion of Al atoms diffused from the second Al deposited layer into the Si deposited layer through N heat treatment, the first SiN microstructure is formed by converting a portion of Si atoms diffused from the Si deposited layer into the first Al deposited layer through N heat treatment, and the second SiN microstructure is formed by converting a portion of Si atoms diffused from the Si deposited layer into the second Al layer through N heat treatment.

[0081] S34: Under the conditions of a temperature of 750° C. to 1050° C. and a pressure of 100 torr to 500 torr, a second nitride barrier layer (ie, the aforementioned second barrier layer) with a thickness of 3 nm to 9 nm is grown on the composite insertion layer.

[0082] Specifically, the second nitride barrier layer is mainly used to reduce the resistance of the nitride light-emitting layer, thereby reducing the operating voltage of the epitaxial wafer.

[0083] Specifically, the material of the second nitride barrier layer is a III-V group nitride. Exemplarily, the second nitride barrier layer can be a GaN barrier layer, an AlGaN barrier layer, or an InGaN barrier layer, etc., with a doping concentration of 2×10 17 cm -3 ~8×10 17 cm -3 ;

[0084] S35: Under the conditions of a temperature of 750° C. to 1050° C. and a pressure of 100 torr to 500 torr, a third nitride barrier layer (ie, the aforementioned third barrier layer) with a thickness of 3 nm to 9 nm is grown on the second nitride barrier layer.

[0085] Specifically, the material of the third nitride barrier layer is a III-V group nitride. Exemplarily, the third nitride barrier layer can be a GaN barrier layer, an AlGaN barrier layer, or an InGaN barrier layer, etc.

[0086] S36: Periodically repeating steps S31 to S360 or more times to form a nitride light-emitting layer. As a typical implementation, steps S31 to S362 to 15 times may be periodically repeated to form a nitride light-emitting layer.

[0087] (4) Under the conditions of a temperature of 950° C. to 1150° C. and a pressure of 100 torr to 500 torr, a second nitride layer with a thickness of 20 nm to 300 nm is grown on the nitride light-emitting layer to form an LED epitaxial wafer.

[0088] Specifically, the second nitride layer is a p-type doped nitride layer, and the doping concentration of the p-type impurities is 1×10 19 cm -3 ~1×10 21 cm -3 More specifically, the second nitride layer is made of III-V group nitride. Exemplarily, the second nitride layer may be a p-type GaN layer, a p-type AlGaN layer, or a p-type InGaN layer.

[0089] It should be noted that, in another embodiment of the present invention, step S33 of growing a composite insertion layer can be performed after growing the second nitride barrier layer and before growing the third nitride barrier layer. Of course, in another embodiment of the present invention, step S33 of growing a composite insertion layer can be performed after growing the first nitride barrier layer and before growing the second nitride barrier layer, as well as after growing the second nitride barrier layer and before growing the third nitride barrier layer.

[0090] On the one hand, the composite insertion layer in the present invention can effectively release the stress in the composite insertion layer through relaxation between the internal AlN and SiN polycrystalline interfaces, improve the crystal quality of the AlN layer / AlN microstructure, reduce the scattering of light by defects, and greatly improve the brightness and leakage performance of the epitaxial wafer; on the other hand, the composite insertion layer in the present invention increases the longitudinal extension distance of Si atoms with small atomic radius in the thickness direction, and the lattice constant modulation effect of the Al-containing nitride quantum barrier layer can be utilized by the introduction of Si atoms, and tensile stress can be further introduced into the nitride quantum barrier layer, which can better compensate for the compressive stress of the nitride quantum well layer, reduce the internal stress distribution of the nitride quantum well layer, improve the crystal quality and component uniformity of the nitride quantum well layer, and reduce non-radiative recombination. Furthermore, the surface of the composite insertion layer introduced by the present invention has a surface with a low N vacancy concentration distribution, which reduces the capture of holes, improves the uniformity of carrier distribution in the nitride light-emitting layer, improves the radiative recombination efficiency, and improves the brightness of the epitaxial wafer.

[0091] Specifically, the process adopted in step S334 of preparing the composite insertion layer of the present invention reduces the N vacancy concentration, and the SiN layer (second SiN layer) formed at the same time has a surface roughening effect on the second nitride barrier layer, forming a nitride barrier layer with a surface roughening structure. During the periodic cycle of the nitride light-emitting layer, the nitride quantum well layer also presents a surface roughening structure, which generally increases the light-emitting area of ​​the nitride light-emitting layer, which is beneficial to the improvement of the brightness of the epitaxial wafer. Moreover, the composite insertion layer introduced in the present invention also greatly reduces the stress in the nitride light-emitting layer, provides support for the nitride light-emitting layer with a large light-emitting surface, and does not cause excessive stress due to the increase in the contact area between the nitride quantum barrier and the nitride quantum well layer.

[0092] Example 1

[0093] A method for preparing an LED epitaxial wafer comprises the following steps:

[0094] (1) Provide 6-inch sapphire substrate.

[0095] (2) Under the conditions of temperature of 1050℃ and pressure of 100 torr, a 3μm thick n-type GaN layer was grown on a sapphire substrate, and the doping concentration of n-type impurities was 5×10 18 cm -3.

[0096] (3) Growing a nitride light-emitting layer on the n-type GaN layer, specifically comprising:

[0097] S31: growing an InGaN quantum well layer with a thickness of 5 nm on the n-type GaN layer under the conditions of a temperature of 800° C. and a pressure of 300 torr.

[0098] S32: growing a first AlGaN barrier layer with a thickness of 2 nm on the InGaN quantum well layer under the conditions of a temperature of 800° C. and a pressure of 200 torr.

[0099] S33: growing a composite insertion layer on the first AlGaN barrier layer, comprising at least the following steps:

[0100] S331: Under the conditions of temperature of 600°C, pressure of 250 torr and reducing atmosphere, an Al source is introduced into the reaction chamber at a flow rate of 150 sccm and maintained for 5 seconds to form a first Al deposition layer on the first nitride barrier layer.

[0101] S332: At a temperature of 600°C, a pressure of 250 torr and a reducing gas atmosphere, a Si source is introduced into the reaction chamber at a flow rate of 200 sccm. Heat treatment is performed for 10 seconds to form a Si deposition layer on the first Al deposition layer.

[0102] S333: Under the conditions of temperature of 600°C, pressure of 150 torr and reducing atmosphere, an Al source is introduced into the reaction chamber at a flow rate of 30 sccm. Heat treatment is performed for 10 seconds to form a second Al deposition layer on the Si deposition layer, thereby forming a precursor of a composite insertion layer.

[0103] S334: Under the conditions of temperature of 1000°C, pressure of 300 torr and reducing atmosphere, Si source and N source are continuously introduced into the reaction chamber, the flow rate of Si source is 100 sccm, and the flow rate of N source is 10 slm, and the precursor of the composite insertion layer is heat treated for 30 seconds, thereby converting the precursor of the composite insertion layer into a composite insertion layer.

[0104] S34: Under the conditions of temperature of 800°C and pressure of 250 torr, a second AlGaN barrier layer with a thickness of 5 nm is grown on the composite insertion layer. The doping concentration of the second AlGaN barrier layer is 5×10 17 cm -3 ;

[0105] S35: growing a third AlGaN barrier layer with a thickness of 5 nm on the second AlGaN barrier layer under the conditions of a temperature of 800° C. and a pressure of 250 torr, thereby forming a light emitting layer.

[0106] (4) Under the conditions of temperature of 1000°C and pressure of 300 torr, a p-type GaN layer with a thickness of 50 nm is grown on the light-emitting layer. The p-type impurity doping concentration of the p-type GaN layer is 5×10 19 cm -3 , thus forming an LED epitaxial wafer.

[0107] Example 2

[0108] A method for preparing an LED epitaxial wafer comprises the following steps:

[0109] (1) Provide 6-inch sapphire substrate.

[0110] (2) Under the conditions of temperature of 1050℃ and pressure of 100 torr, a 3μm thick n-type GaN layer was grown on a sapphire substrate, and the doping concentration of n-type impurities was 5×10 18 cm -3 .

[0111] (3) Growing a nitride light-emitting layer on the n-type GaN layer, specifically comprising:

[0112] S31: growing an InGaN quantum well layer with a thickness of 5 nm on the n-type GaN layer under the conditions of a temperature of 800° C. and a pressure of 300 torr.

[0113] S32: growing a first AlGaN barrier layer with a thickness of 2 nm on the InGaN quantum well layer under the conditions of a temperature of 800° C. and a pressure of 200 torr.

[0114] S33: Under the conditions of a temperature of 800°C and a pressure of 250 torr, a second AlGaN barrier layer with a thickness of 5 nm is grown on the first AlGaN barrier layer. The doping concentration of the second AlGaN barrier layer is 5×10 17 cm -3 ;

[0115] S34: growing a composite insertion layer on the second AlGaN barrier layer, comprising at least the following steps:

[0116] S341: Under the conditions of temperature of 500°C, pressure of 200 torr and reducing atmosphere, an Al source is introduced into the reaction chamber at a flow rate of 100 sccm and maintained for 5 seconds to form a first Al deposition layer on the first nitride barrier layer.

[0117] S342: At a temperature of 500°C, a pressure of 200 torr and a reducing gas atmosphere, a Si source is introduced into the reaction chamber at a flow rate of 10 sccm. Heat treatment is performed for 15 seconds to form a Si deposition layer on the first Al deposition layer.

[0118] S343: Under the conditions of temperature of 500°C, pressure of 100 torr and reducing atmosphere, Al source is introduced into the reaction chamber with an Al source flow rate of 10 sccm. Heat treatment is performed for 10 seconds to form a second Al deposition layer on the Si deposition layer, thereby forming a precursor of the composite insertion layer.

[0119] S344: Under the conditions of a temperature of 900°C, a pressure of 100 torr and a reducing atmosphere, Si source and N source are continuously introduced into the reaction chamber. The flow rate of Si source is 50 sccm, and the flow rate of N source is 2 slm. The precursor of the composite insertion layer is heat-treated for 30 seconds, thereby converting the precursor of the composite insertion layer into a composite insertion layer.

[0120] S35: Under the conditions of a temperature of 800° C. and a pressure of 250 torr, a third AlGaN barrier layer with a thickness of 5 nm is grown on the composite insertion layer, thereby forming a light-emitting layer.

[0121] (4) Under the conditions of temperature of 1000°C and pressure of 300 torr, a p-type GaN layer with a thickness of 50 nm is grown on the light-emitting layer. The p-type impurity doping concentration of the p-type GaN layer is 5×10 19 cm -3 , thus forming an LED epitaxial wafer.

[0122] Example 3

[0123] A method for preparing an LED epitaxial wafer comprises the following steps:

[0124] (1) Provide a GaN substrate.

[0125] (2) Under the conditions of temperature of 1050°C and pressure of 100 torr, a 3 μm thick n-type GaN layer was grown on a GaN substrate, and the doping concentration of n-type impurities was 5×10 18 cm -3 .

[0126] (3) Growing a nitride light-emitting layer on the n-type GaN layer, specifically comprising:

[0127] S31: growing an InGaN quantum well layer with a thickness of 5 nm on the n-type GaN layer under the conditions of a temperature of 800° C. and a pressure of 300 torr.

[0128] S32: growing a first AlGaN barrier layer with a thickness of 2 nm on the InGaN quantum well layer under the conditions of a temperature of 800° C. and a pressure of 200 torr.

[0129] S33: growing a composite insertion layer on the first AlGaN barrier layer, comprising at least the following steps:

[0130] S331: Under the conditions of temperature of 1000°C, pressure of 300 torr and reducing atmosphere, an Al source is introduced into the reaction chamber at a flow rate of 300 sccm and maintained for 2 seconds to form a first Al deposition layer on the first nitride barrier layer.

[0131] S332: At a temperature of 1000°C, a pressure of 300 torr and a reducing gas atmosphere, a Si source is introduced into the reaction chamber at a flow rate of 300 sccm. Heat treatment is performed for 5 seconds to form a Si deposition layer on the first Al deposition layer.

[0132] S333: Under the conditions of temperature of 1000°C, pressure of 100 torr and reducing atmosphere, an Al source is introduced into the reaction chamber at a flow rate of 100 sccm. Heat treatment is performed for 5 seconds to form a second Al deposition layer on the Si deposition layer, thereby forming a precursor of a composite insertion layer.

[0133] S334: Under the conditions of a temperature of 1200°C, a pressure of 500 torr and a reducing atmosphere, Si source and N source are continuously introduced into the reaction chamber. The flow rate of Si source is 300 sccm, and the flow rate of N source is 50 slm. The precursor of the composite insertion layer is heat treated for 40 seconds to transform the precursor into a composite insertion layer.

[0134] S34: Under the conditions of temperature of 800°C and pressure of 250 torr, a second AlGaN barrier layer with a thickness of 5 nm is grown on the composite insertion layer. The doping concentration of the second AlGaN barrier layer is 5×10 17 cm -3 ;

[0135] S35: growing a third AlGaN barrier layer with a thickness of 5 nm on the second AlGaN barrier layer under the conditions of a temperature of 800° C. and a pressure of 250 torr.

[0136] S36: Periodically repeat steps S31 to S36 three times to form a nitride light-emitting layer.

[0137] (4) Under the conditions of temperature of 1000°C and pressure of 300 torr, a p-type GaN layer with a thickness of 50 nm is grown on the light-emitting layer. The p-type impurity doping concentration of the p-type GaN layer is 5×10 19 cm -3 , thus forming an LED epitaxial wafer.

[0138] Comparative Example 1

[0139] A method for preparing an LED epitaxial wafer comprises the following steps:

[0140] (1) Provide a GaN substrate.

[0141] (2) Under the conditions of temperature of 1050°C and pressure of 100 torr, a 3 μm thick n-type GaN layer was grown on a GaN substrate, and the doping concentration of n-type impurities was 5×10 18 cm -3 .

[0142] (3) Growing a nitride light-emitting layer on the n-type GaN layer, specifically comprising:

[0143] S31: growing an InGaN quantum well layer with a thickness of 5 nm on the n-type GaN layer under the conditions of a temperature of 800° C. and a pressure of 300 torr.

[0144] S32: growing a first AlGaN barrier layer with a thickness of 2 nm on the InGaN quantum well layer under the conditions of a temperature of 800° C. and a pressure of 200 torr.

[0145] S33: growing a first AlN layer, a first SiN layer, a second AlN layer, and a second SiN layer on the first AlGaN barrier layer in sequence to form a composite insertion layer, such as Figure 6 shown.

[0146] S34: Under the conditions of temperature of 800°C and pressure of 250 torr, a second AlGaN barrier layer with a thickness of 5 nm is grown on the composite insertion layer. The doping concentration of the second AlGaN barrier layer is 5×10 17 cm -3 ;

[0147] S35: growing a third AlGaN barrier layer with a thickness of 5 nm on the second AlGaN barrier layer under the conditions of a temperature of 800° C. and a pressure of 250 torr, thereby forming a light emitting layer.

[0148] (4) Under the conditions of temperature of 1000°C and pressure of 300 torr, a p-type GaN layer with a thickness of 50 nm is grown on the light-emitting layer. The p-type impurity doping concentration of the p-type GaN layer is 5×10 19 cm -3 , thus forming an LED epitaxial wafer.

[0149] The epitaxial wafers with a wavelength of 460±0.5 nm obtained in Examples 1-3 and Comparative Example 1 were respectively subjected to photoluminescence test wavelength uniformity std and X-ray diffractometer (XRD) test (102) plane half-width test, and the same chip processing technology was used to process the nitride light-emitting layers obtained in Examples 1-3 and Comparative Example 1 to obtain Micro-LED chips with a size of 4 mil*6 mil, and the brightness and leakage test results of the obtained Micro-LED chips were respectively performed, as shown in Table 1.

[0150] Table 1 Brightness and leakage test results of each Micro-LED chip

[0151]

[0152] It can be seen from Table 1 that, compared with the prior art, the present invention reduces the stress of the light-emitting layer in the epitaxial wafer, improves the crystal quality of the epitaxial wafer, enhances the radiation recombination efficiency in the light-emitting layer, improves the brightness of the LED epitaxial wafer, and improves the leakage performance of the epitaxial wafer.

[0153] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite insert layer structure, characterized in that include: At least one composite insertion layer unit, the composite insertion layer unit comprising a first AlN layer, a first SiN layer, a second AlN layer and a second SiN layer stacked in sequence along a selected direction, wherein the interior of the stacked structure layer formed by the first AlN layer, the first SiN layer and the second AlN layer has a plurality of AlN microstructures and a plurality of SiN microstructures that are intertwined and distributed.

2. The composite insert layer structure according to claim 1, characterized in that: The plurality of AlN microstructures include a plurality of first AlN microstructures and a plurality of second AlN microstructures, and the plurality of first AlN microstructures and the plurality of second AlN microstructures are distributed in the first SiN layer at intervals; And / or, the plurality of SiN microstructures include a plurality of first SiN microstructures and a plurality of second SiN microstructures, the plurality of first SiN microstructures are spaced apart and distributed in the first AlN layer, and the plurality of second SiN microstructures are spaced apart and distributed in the second AlN layer; Preferably, the plurality of first AlN microstructures are integrated with the first AlN layer, and the plurality of second AlN microstructures are integrated with the second AlN layer; Preferably, the plurality of first SiN microstructures and the plurality of second SiN microstructures are integrated with the first SiN layer.

3. The composite insert layer structure according to claim 1, characterized in that: The second SiN layer also has a plurality of nanopore structures; Preferably, the nanopore structure is a through hole within a through hole that penetrates the second SiN layer along the selected direction; Preferably, the nanopore structure is formed by the discontinuity of the membrane structure of the second SiN layer itself.

4. The composite insert layer structure according to claim 1, characterized in that: include: A plurality of the composite insertion layer units are stacked in sequence along the selected direction.

5. A method for preparing a composite insert layer structure, characterized in that: include: The step of making a precursor for forming a composite insert layer structure, the precursor comprising a first Al layer, a Si layer, and a second Al layer stacked in a selected direction; At least under the condition that a Si source and a N source coexist, the precursor is heat-treated to make at least some Al atoms in the first Al layer and the second Al layer dissolve and diffuse with some Si atoms in the Si layer, and at least some Al atoms and at least some Si atoms in the precursor are combined with N atoms provided by the N source to form AlN and SiN respectively, and some Si atoms in the Si source are also combined with some Si atoms in the N source to form SiN, thereby forming a composite insertion layer unit.

6. The method for preparing the composite insert layer structure according to claim 5, characterized in that: The composite insertion layer unit comprises a first AlN layer, a first SiN layer, a second AlN layer and a second SiN layer sequentially stacked in a selected direction, wherein the stacked structure layer formed by the first AlN layer, the first SiN layer and the second AlN layer has a plurality of AlN microstructures and a plurality of SiN microstructures interlaced and distributed inside; wherein the first AlN layer is formed by combining a portion of Al atoms in the first Al layer with N atoms provided by the N source, the second AlN layer is formed by combining a portion of Al atoms in the second Al layer with N atoms provided by the N source, the first SiN layer is formed by combining a portion of Si in the Si layer with N atoms provided by the N source, a plurality of AlN microstructures are formed by combining a portion of Al atoms diffused from the first Al layer or the second Al layer into the Si layer or the first SiN layer with N atoms provided by the N source, and a plurality of SiN microstructures are formed by combining a portion of Si atoms diffused from the Si layer into the first Al layer / the first AlN layer, the second Al layer / the second AlN layer with N atoms provided by the N source; Preferably, the plurality of AlN microstructures include a plurality of first AlN microstructures and a plurality of second AlN microstructures, the plurality of first AlN microstructures and the plurality of second AlN microstructures are spaced apart and distributed in the first SiN layer, the first AlN microstructure is formed by combining a portion of Al atoms diffused from the first Al layer into the Si layer or the first SiN layer with N atoms provided by the N source, and the second AlN microstructure is formed by combining a portion of Al atoms diffused from the second Al layer into the Si layer or the first SiN layer with N atoms provided by the N source; Preferably, the plurality of SiN microstructures include a plurality of first SiN microstructures and a plurality of second SiN microstructures, the plurality of first SiN microstructures are spaced apart and distributed in the first AlN layer, the plurality of second SiN microstructures are spaced apart and distributed in the second AlN layer, the first SiN microstructure is formed by combining a portion of Si atoms diffused from the Si layer into the first Al layer / the first AlN layer with N atoms provided by the N source, and the second SiN microstructure is formed by combining a portion of Si atoms diffused from the Si layer into the second Al layer / the second AlN layer with N atoms provided by the N source; Preferably, the plurality of first AlN microstructures are integrated with the first AlN layer, and the plurality of second AlN microstructures are integrated with the second AlN layer; Preferably, the plurality of the first SiN microstructures and the plurality of the second SiN microstructures are integrated with the first SiN layer; Preferably, the heat treatment temperature is 900°C to 1200°C and the pressure is 100 torr to 500 torr; Preferably, when the precursor is heat treated, the supply flow rate of the Si source is 10 scc to 300 sccm, and the supply flow rate of the N source is 2 slm to 50 slm; Preferably, the heat treatment time is 15s to 45s; Preferably, the second SiN layer has a plurality of nanopore structures; Preferably, the nanopore structure is a through hole within a through hole that penetrates the second SiN layer along the selected direction; Preferably, the nanopore structure is formed by the discontinuity of the membrane structure of the second SiN layer itself.

7. A light-emitting layer structure, comprising at least one quantum well layer and at least one quantum barrier layer stacked in sequence along a selected direction, characterized in that: The quantum barrier layer comprises at least two barrier layers stacked along the selected direction and at least one composite insertion layer, wherein at least one composite insertion layer is arranged between two adjacent barrier layers, and the composite insertion layer comprises the composite insertion layer structure according to any one of claims 1-4.

8. The light-emitting layer structure according to claim 7, characterized in that: The quantum barrier layer comprises a first barrier layer, a second barrier layer and a third barrier layer stacked along the selected direction, and the composite insertion layer is stacked and arranged between the second barrier layer and at least one of the first barrier layer and the third barrier layer; Preferably, the quantum well layer and the quantum barrier layer are periodically and repeatedly stacked; Preferably, the materials of the quantum well layer and the quantum barrier layer are both nitride; Preferably, the materials of the quantum well layer and the quantum barrier layer are both III-V group nitrides, wherein the material of the quantum barrier layer is a nitride containing Al.

9. An epitaxial wafer, characterized in that: The light-emitting layer structure comprises the light-emitting layer structure according to any one of claims 7 to 8.

10. A light emitting device, characterized in that: Comprising the epitaxial wafer according to claim 9.

Citation Information

Patent Citations

  • GaN-based epitaxial structure and preparation method thereof

    CN112233972A

  • Light-emitting diode epitaxial wafer and preparation method thereof

    CN113113518A

  • Epitaxial wafer, epitaxial wafer preparation method and blue-green light emitting diode

    CN114784157A

  • Composite N-type GaN layer, light-emitting diode epitaxial wafer and preparation method of light-emitting diode epitaxial wafer

    CN115064622A

  • High-luminous-efficiency light-emitting diode epitaxial wafer and preparation method thereof

    CN116344693A