Embodiment 1
[0016] Example 1 (SAPO-11)
[0017] 14.04g pseudo-boehmite (containing Al 2 o 3 72.6%) powder was dissolved in 74ml deionized water, and 23.06g phosphoric acid (containing H 3 PO 4 85%) and 12.82g silica sol (containing SiO 2 28.1%). Add 4.41g diethylamine (analytical pure) at last, after stirring and mixing evenly, this mixed material is moved into the stainless steel synthesis kettle and seals. Crystallize at 180°C under autogenous pressure for 24 hours, wash the solid product with deionized water until neutral, and dry it in air at 100°C to obtain SAPO-11 molecular sieve, whose XRD analysis is shown in Table 1.
[0018] Table 1
[0019]
[0020]
Embodiment 2
[0021] Example 2 (SAPO-11)
[0022] In Example 1, only the amount of silica sol was changed to 2.14 g, and the remaining components and operating conditions were unchanged. The obtained product was analyzed by XRD diffraction to be SAPO-11 molecular sieve.
Embodiment 3
[0023] Example 3 (SAPO-11)
[0024] In Example 1, only the amount of diethylamine was changed to 5.88 g, and the remaining components and operating conditions were unchanged. The obtained product was analyzed by XRD diffraction to be SAPO-11 molecular sieve.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com