example 1
[0063] The following recipe was used to produce 2 identical grinding bodies of size 300 x 20 x 127. Formulation 1 is a comparative example of Formulation 2 according to the invention. In this and all other examples, a mixture of 50% by weight of glass frit 90158 (iron), 25% by weight of clay and 25% by weight of lapis lazuli was used as the ceramic binder.
[0064]
[0065] The abrasive body composition of Formulation 1 with naphthalene as pore former was pressed, then dried at 80° C. in a drying oven with thermal afterburner and the naphthalene was removed. Subsequently, the grinding bodies were fired at a maximum temperature of 950° C. in a ceramic furnace (Energo furnace).
[0066] The abrasive body composition according to formulation 2 containing fumaric acid as pore former was pressed and then esterified / cured in a curing furnace (Reinhard furnace) at a maximum temperature of up to 165° C. for 24 hours. use figure 1 hardness curve.
[0067] Subsequently, the grind...
example 2
[0074] Highly porous samples (202mm diameter, 100mm height) were produced.
[0075] formula:
[0076]
[0077]
[0078] The formulation components are mixed uniformly and then compressed. Afterwards, the discs are removed in a drying oven with thermal post-combustion equipment. The removal profile included heating at 50°C / h to 200°C, maintaining the maximum temperature at 200°C over 48 hours, and allowing the furnace to cool naturally to room temperature. Such strength is quite sufficient to manufacture discs for ceramic firing on a furnace car. Subsequently, the grinding bodies were fired at a maximum temperature of 950° C. in a ceramic furnace (Energo furnace).
PUM
| Property | Measurement | Unit |
|---|---|---|
| density | aaaaa | aaaaa |
| diameter | aaaaa | aaaaa |
| height | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 