Macroporous alumina and production method thereof
By controlling the grain size and pore structure of alumina under high-pressure and low-temperature conditions through a continuous production method, the problem of unsatisfactory alumina pore structure in the existing technology is solved, and alumina with high specific surface area and large pore volume is achieved, which is suitable for It is used as a hydrogenation catalyst carrier to improve the hydrogenation efficiency of heavy and inferior raw materials.
Patent Information
- Application Number
- CN202111280244.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-10-29
AI Technical Summary
It is difficult to effectively prepare macroporous alumina with high specific surface area using existing technology, resulting in unsatisfactory pore structure and low crystallinity, making it unable to meet the demand as a hydrogenation catalyst carrier.
Adopting a continuous production method, through neutralization gel formation and aging polymerization reaction, organic solvents and polar metal salts are used to control the grain size and pore structure under high pressure and low temperature conditions to form oxidation products with large pore volume, large surface area and high purity. aluminum.
The high specific surface area, large pore volume and concentrated particle size distribution of alumina are achieved, making it suitable as a carrier for hydrogenation catalysts and improving the hydrogenation efficiency of heavy and inferior raw materials.
Smart Images

Figure CN116081664B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of alumina preparation, in particular to a method for continuously producing macroporous alumina. Background Art
[0002] At present, the production methods of pseudo-boehmite are mainly inorganic aluminum salt method and organic aluminum salt method, and the production process mostly adopts intermittent kettle reactor. Pseudo-boehmite is mainly produced by precipitation mechanism, in which precipitation refers to the process of chemical reaction in liquid phase to generate insoluble substances and form new solid phase to settle out of liquid phase. According to the classical precipitation theory, the precipitation formation process is divided into: (1) Nucleation: Due to the continuous collision and movement of molecules or ions, molecules in local areas gather into clusters. The aggregation is not only due to the collision between moving particles in the solution, but also through weak force (van der Waals force) mutual adhesion, and through the formation of chemical bonds in the crystal, the aggregates are solidified; (2) Nucleation growth: The molecular particles of the clusters contact each other, merge and grow; among them, the colloid is uniform and the particles are small, which is very powerful for nucleation and crystal growth.
[0003] Coprecipitation is a typical method for preparing aluminum hydroxide. This method uses water as a medium to make the raw materials into aluminum salts, and then controls a certain solution concentration, solution flow rate, temperature, and reaction time, and then neutralizes with acid / base to obtain aluminum hydroxide. However, during the coprecipitation process, the initial crystal nucleus Al(OH)3 has many hydroxyl groups (and water molecules are also bound to it), a complex structure, a small molecular polarity, and extremely low solubility. Therefore, its aggregation rate is much greater than the orientation rate, and it is easy to generate an amorphous gel-like precipitate, resulting in low crystallinity, incomplete crystal form, and unsatisfactory pore structure.
[0004] CN103787390A discloses a method for preparing pseudo-boehmite, which includes the following processes: (1) an acidic aluminum salt solution and an alkaline solution are subjected to a gelling reaction, and then aging is performed; the gelling reaction and aging are both performed under ultrasonic radiation conditions, and different frequencies of ultrasonic waves are used in the gelling reaction process and the aging process, and the gelling reaction process uses ultrasonic waves with a frequency of 10 to 160 kHz; the aging process uses ultrasonic waves with a frequency higher than that of the gelling reaction process by 1 to 50 kHz; (2) the aged material is filtered and washed; (3) the material obtained in step (2) is dried to obtain pseudo-boehmite. The method is to prepare pseudo-boehmite by using ultrasonic waves of different frequencies to control the grain size during gelling and aging.
[0005] In the prior art, although there are different methods to control the grain size to prepare pseudo-boehmite with different pore structures and properties, how to prepare macroporous alumina with high specific surface area is also an important topic that has been studied in this field. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a macroporous alumina and a production method thereof, in particular a method for continuously producing macroporous alumina. The alumina of the present invention has the characteristics of large particle size and concentrated distribution, high specific surface area, large pore volume, large pore size, high purity, etc., and can be used as a carrier material for hydrogenation catalysts of inferior raw materials.
[0007] The first aspect of the present invention provides an aluminum oxide having the following properties: a pore volume of 2.0 to 3.0 ml / g; a specific surface area of 410 to 550 m 2 / g, the volume of pores with a pore diameter of 200-300 nm accounts for 90.0%-95.0% of the total pore volume.
[0008] The particle size distribution of the aluminum oxide provided by the present invention is as follows: the proportion of grains with a particle size less than 150 μm is 0.5% to 5.0%, the proportion of grains with a particle size of 150 to 250 μm is 2.0% to 5.0%, and the proportion of grains with a particle size greater than 250 μm is 90.0% to 95.0%.
[0009] The relative crystallinity of the aluminum oxide provided by the present invention is ≮90%, preferably 95% to 99%.
[0010] The pore size distribution of the alumina provided by the present invention is as follows: the volume of pores with a pore size less than 200 nm accounts for 1.0% to 5.0% of the total pore volume, the volume of pores with a pore size of 200 to 300 nm accounts for 90.0% to 95.0% of the total pore volume, and the volume of pores with a pore size greater than 300 nm accounts for 2.0% to 5.0% of the total pore volume.
[0011] A second aspect of the present invention provides a method for producing macroporous alumina, comprising:
[0012] (1) adding an organic solvent, a polar metal seed crystal, an acidic aluminate solution I and an alkaline aluminate solution I into a first reaction kettle in parallel to neutralize and form a gel to obtain a generated solution I;
[0013] (2) the resulting liquid I is placed in a sedimentation tank for sedimentation separation to obtain an upper layer, i.e., an organic solvent, and a lower layer, i.e., a sol II;
[0014] (3) the sol II and the acidic or alkaline aluminate solution II flow into the second reaction kettle in parallel to undergo a neutralization and gelation reaction to obtain a generated solution III;
[0015] (4) The generated liquid III enters an aging kettle, and polymerization monomers and initiators are added, and then an aging polymerization reaction is carried out;
[0016] (5) The material obtained in step (4) is dried and calcined to obtain the alumina.
[0017] The aluminum oxide production method of the present invention is preferably carried out in a continuous manner, wherein a plurality of settling tanks used in step (2) and an aging kettle used in step (4) can be provided and switched for use during continuous production.
[0018] In the method of the present invention, when alumina is produced continuously, preferably, the first reactor in step (1) is operated by overflowing the generated liquid I out of the first reactor. When the first reactor is started, preferably, an organic solvent and polar metal seed crystals are first added as the bottom liquid, and then the acidic aluminate solution I and the alkaline aluminate solution I are added in parallel to neutralize and gelate until the generated liquid I starts to be discharged from the first reactor. The amount of the organic solvent added to the bottom liquid is 1 / 5 to 1 / 2 of the actual effective use volume of the first reactor. When the generated liquid I starts to be discharged from the first reactor, the total mass of the acidic aluminum salt solution I and the alkaline aluminum salt solution I in the first reactor is calculated as Al2O3, and the amount of the polar metal salt seed crystals added accounts for 0.1% to 5.0%, preferably 0.5% to 4.0%.
[0019] In the method of the present invention, when alumina is produced continuously, preferably, in step (3), the second reactor is operated in an overflow manner to discharge the generated liquid III from the second reactor. When the second reactor is started, preferably, bottom water is added first, and then sol II and acidic or alkaline aluminate solution II are added in parallel to neutralize and form a gel, until the generated liquid III begins to be discharged from the second reactor. The amount of bottom water added is 1 / 7 to 1 / 2 of the actual effective use volume of the second reactor, preferably 1 / 6 to 1 / 3.
[0020] In the method of the present invention, the organic solvent in step (1) is an organic substance that is immiscible with water or slightly soluble in water, and the organic substance may be one or more of alkanes, alkenes, organic alcohols, organic acids, etc. Preferably, the carbon number of the organic substance is 5 to 12. The molecular structure of the alkane is C n H 2n+2 (n≥5, preferably n=5~12), at least one of pentane, hexane, dodecane, etc. can be selected; the molecular structure of olefin is C n H 2n (n≥5, preferably n=5~12), at least one of pentene, hexene, etc. can be selected; the organic alcohol is selected from at least one of organic monohydric alcohol and organic polyhydric alcohol, wherein the molecular structure formula of the organic monohydric alcohol is C n H 2n+2 O (n≥6, preferably n=6~12), at least one of n-hexanol, n-heptanol, etc. can be selected; wherein the molecular structure formula of the polyol is C n H 2n+2-x (OH) x(n≥6, preferably n=6~12, x≥3), at least one of the polyols such as pentaerythritol, glycerol, trimethylolethane, xylitol, sorbitol, etc. can be selected; the organic acid can be at least one of the aliphatic or aromatic carboxylic acids, such as benzoic acid, etc.
[0021] In the method of the present invention, the polar metal seed crystals include at least one of metal halogen compounds and metal sulfides, preferably one or more selected from AgCl, ZnS, CuS or HgS.
[0022] In the method of the present invention, the operating conditions of the first reactor described in step (1) are as follows: temperature is -15 to 15°C, preferably 0 to 15°C, pressure is 5 to 20 MPa, preferably 5 to 15 MPa, and the pressure atmosphere can be one or more of air, nitrogen or inert gas. The reaction conditions of the neutralization and gelling in step (1) are as follows: pH value is 2 to 6, preferably 2 to 5, reaction time is 10 to 180 minutes, preferably 10 to 60 minutes (when continuous production is adopted, the reaction time is the residence time of the acidic aluminate solution I and the alkaline aluminate solution I entering the first reactor). The neutralization and gelling reaction is preferably carried out under stirring conditions, and the stirring rate is 100 to 500 rad / min, preferably 150 to 500 rad / min.
[0023] In the method of the present invention, the acidic aluminum salt described in step (1) can be selected from one or more of AlCl3, Al2(SO4)3 or Al(NO)3, preferably one or more of Al2(SO4)3 and AlCl3, and the acidic aluminum salt solution can be an aqueous solution. The concentration of the acidic aluminum salt aqueous solution is 10 to 100 g / 100 ml in terms of Al2O3. The alkaline aluminum salt is selected from one or both of NaAlO2 and KAlO2, preferably NaAlO2. The alkaline aluminum salt solution can be an aqueous solution. The concentration of the alkaline aluminum salt aqueous solution is 10 to 100 g / 100 ml in terms of Al2O3.
[0024] In the method of the present invention, the organic solvent and the polar metal seeds are added to the first reaction kettle in parallel, wherein the ratio of the organic solvent addition rate to the sum of the addition rates of the acidic aluminate solution I and the alkaline aluminate solution I based on their volumes is 0.1:1-10:1, preferably 0.2:1-5:1, and the polar metal seeds addition rate is 1%-10% of the sum of the addition rates of the acidic aluminate solution I and the alkaline aluminate solution I based on their mass of Al2O3, preferably 1%-5%.
[0025] In the method of the present invention, the particle size distribution of the sol II obtained in step (2) is as follows: the proportion of crystal particles with a particle size of less than 50 nm is 0.5% to 5.0%, the proportion of crystal particles with a particle size of 50 to 100 nm is 2% to 5%, and the proportion of crystal particles with a particle size of more than 100 nm is 90% to 95%. The relative crystallinity of the obtained sol II is ≮95%, preferably 95% to 98%.
[0026] In the method of the present invention, the operating conditions of the settling tank in step (2) are as follows: the temperature is -15 to 15°C, preferably 0 to 15°C, and the pressure is 5 to 20 MPa, preferably 5 to 15 MPa.
[0027] In the method of the present invention, after the sedimentation in step (2), the organic solvent in the upper layer can be recycled to the first reaction kettle for continued use.
[0028] In the method of the present invention, the operating conditions of the second reactor described in step (3) are as follows: temperature is 100-300°C, preferably 100-200°C, pressure is 5-20MPa, preferably 5-17MPa, and more preferably 6-17MPa. Preferably, the operating pressure of the second reactor is at least 0.5MPa higher than the operating pressure of the first reactor, preferably 2MPa higher. The reaction conditions of neutralization and gelation in step (3) are as follows: pH value is 7-12, preferably 7.5-10.0, reaction time is 10-180 minutes, preferably 10-120 minutes (when continuous production is adopted, the reaction time is the residence time of sol II and acidic or alkaline aluminate solution II entering the second reactor). The neutralization and gelation reaction is preferably carried out under stirring conditions, and the stirring rate is 100-500rad / min, preferably 200-500rad / min.
[0029] In the method of the present invention, the acidic aluminum salt described in step (3) is selected from at least one of AlCl3, Al2(SO4)3 or Al(NO)3, etc., preferably at least one of Al2(SO4)3, AlCl3, etc., and the acidic aluminum salt solution can be an aqueous solution. The concentration of the acidic aluminum salt aqueous solution is 10 to 100 g / 100 ml in terms of Al2O3. The basic aluminum salt is selected from one or both of NaAlO2 and KAlO2, preferably NaAlO2, and the basic aluminum salt solution can be an aqueous solution. The concentration of the basic aluminum salt aqueous solution is 10 to 100 g / 100 ml in terms of Al2O3.
[0030] In the method of the present invention, the polymer monomer in step (4) is at least one of an organic alcohol or an organic acid; the organic alcohol is at least one of a monohydric alcohol or a polyhydric alcohol, and the monohydric alcohol is C6-C 10The higher fatty alcohol is one or more of ethylene glycol, pentaerythritol, 2-propylene glycol, 1,4-butanediol, neopentyl glycol, sorbitol, dipropylene glycol, glycerol, xylitol, trimethylolpropane or diethylene glycol; the organic acid is one or more of tartaric acid, oxalic acid, malic acid, citric acid, acetic acid, oxalic acid, succinic acid, ascorbic acid, benzoic acid, salicylic acid, caffeic acid, aspartic acid, glutamic acid, glycine, alanine, valine, leucine, isoleucine, phenylalanine, proline, tryptophan, serine, tyrosine, cysteine, methionine, asparagine, glutamine or threonine.
[0031] In the method of the present invention, the initiator described in step (4) can be selected from at least one of a peroxide compound initiator, an azo initiator, and a redox initiator according to the reaction requirements. Among them, the peroxide initiator is selected from one or more of benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, diisopropyl perbenzoate, tert-butyl pervalerate, methyl ethyl ketone peroxide, cyclohexanone peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, ammonium persulfate, and potassium persulfate; the azo initiator is selected from azobisisobutyronitrile and / or azobisisoheptylonitrile, preferably azobisisobutyronitrile. The redox initiator is selected from one of benzoyl peroxide / sucrose, tert-butyl hydroperoxide / rongalite, tert-butyl hydroperoxide / sodium pyrosulfite, benzoyl peroxide / N,N-dimethylaniline, ammonium persulfate / sodium bisulfite, potassium persulfate / sodium bisulfite, hydrogen peroxide / tartaric acid, hydrogen peroxide / rongalite, ammonium persulfate / ferrous sulfate, hydrogen peroxide / ferrous sulfate, benzoyl peroxide / N,N-diethylaniline, benzoyl peroxide / ferrous pyrophosphate, potassium persulfate / silver nitrate, persulfate / thiol, cumene hydroperoxide / ferrous chloride, potassium persulfate / ferrous chloride, hydrogen peroxide / ferrous chloride, cumene hydroperoxide / tetraethyleneimine, etc.
[0032] In the method of the present invention, the conditions of the aging polymerization reaction in step (4) are as follows: temperature 200-400°C, pressure 15-20MPa, time 100-360min, preferably 150-250min; the reaction is carried out under stirring conditions, and the stirring speed is preferably 500-800r / min.
[0033] In the method of the present invention, the degree of polymerization of the polymer formed by the polymerization reaction in step (4) is 5 to 100, preferably 5 to 50, and the degree of polymerization of the polymer can be controlled by selecting an initiator and adjusting the reaction conditions.
[0034] In the method of the present invention, the molar ratio of the generated liquid III in step (4) to the polymer monomer is 20:1 to 1:1, preferably 15:1 to 1:1. The amount of the initiator added is 0.01% to 3.5% of the mass of the polymer monomer.
[0035] In the method of the present invention, the drying temperature in step (5) is 100-450°C, preferably 150-400°C, the drying time is 1-10 hours, and the drying method can be flash drying, cyclone drying, oven drying, spray drying, etc. The roasting temperature is 300-800°C, preferably 350-550°C, and the roasting time is 2-5 hours, preferably 2-4 hours. The roasting atmosphere is one or more of air, nitrogen or water vapor.
[0036] The third aspect of the present invention provides alumina produced by the above method.
[0037] The fourth aspect of the present invention provides the use of the above-mentioned alumina in a hydrogenation catalyst carrier.
[0038] In the application of the present invention, the hydrogenation catalyst can be a hydrogenation catalyst used for treating inferior heavy oil, such as a protective agent and / or a hydrogenation refining agent in the hydrogenation of residual oil, wax oil, coal tar, and coal liquefaction oil.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] 1. In the method for producing aluminum oxide provided by the present invention, an organic solvent immiscible with water is first used as a reaction medium, and a polar metal salt is used as a seed crystal, and a neutralization reaction is carried out at a relatively high pressure and a relatively low reaction temperature. On the one hand, the sol-gel particles generated by the neutralization will not adhere to each other in the organic solvent immiscible with water due to the encapsulation of hydrophilic hydroxyl groups on the surface, and under the action of the polar seed crystals, the sol-gel particles will be easily formed into crystal precipitation or colloidal particles with a crystal structure by utilizing the characteristics of small molecules, large polarity, and large orientation rate. On the other hand, under a relatively high pressure and a relatively low temperature, the Brownian motion of the sol-gel molecules or ions is reduced, and the aggregation into clusters due to continuous collision of the particles is reduced, and at a relatively high temperature, the reaction temperature is relatively low. Amorphous aluminum hydroxide is dissolved under low pH value, i.e. acidic conditions, while the generated pseudo-boehmite is retained, thereby effectively controlling the grain size in Sol II to be suitable and complete. Then, the sol-gel particles with complete crystal form are placed under high temperature, high pressure, and relatively high pH value, i.e. alkaline conditions, to accelerate the Brownian motion of the particles, so that a large number of particles with complete crystal form are aggregated to form pseudo-boehmite precipitation. After aging and polymerization reaction, the formed polymer is embedded in the large alumina particles. After calcination, through-type channels with a spatial network structure are formed, which can provide diffusion channels for macromolecular reactions, so that the final alumina has the characteristics of large surface area, large pore volume, concentrated particle size distribution, high crystallinity, etc.
[0041] 2. The alumina provided by the present invention has the characteristics of large surface area, large pore volume, concentrated particle size distribution, high crystallinity, etc., and is particularly suitable as a carrier of hydrogenation catalyst, and is used as a protective agent and / or hydrogenation refining agent for the hydrogenation of heavy and inferior raw materials such as residual oil, wax oil, coal liquefied oil, and coal tar. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a schematic diagram of the process for continuous production of alumina;
[0043] Among them, the accompanying drawings are marked as follows: I-first reactor; II, III-sedimentation tanks; IV-second reactor; V-aging reactor; A-acidic aluminate solution I; B-alkaline aluminate solution I; C-polar metal seed; D-organic solvent; E-sedimentation tank II control valve; F-sedimentation tank III control valve; G-sol II; H-acidic or alkaline aluminate solution II; I-second reactor drain valve; J-overflow liquid; K-aging reactor drain valve; L-polymer monomer and initiator. DETAILED DESCRIPTION
[0044] The following is a more detailed description of the preparation method of aluminum oxide of the present invention through specific examples. The examples are only illustrative of the specific implementation of the method of the present invention and do not constitute a limitation on the protection scope of the present invention.
[0045] The process for continuous production of aluminum oxide provided by the present invention (such as Figure 1 ),include:
[0046] (1) adding an organic solvent D, a polar metal seed crystal C, an acidic aluminate solution IA and an alkaline aluminate solution IB into a first reaction kettle I in parallel to neutralize and form a gel to obtain a generated solution I;
[0047] (2) the resulting liquid I enters a settling tank II or III for settling, and is separated by a control valve E of the settling tank II or a control valve F of the settling tank III to obtain a lower layer, namely, sol II G, and an upper layer, namely, an organic solvent;
[0048] (3) The sol II and the acidic or alkaline aluminate solution II H flow into the second reactor IV in parallel to undergo a neutralization and gelation reaction to obtain a generated solution III;
[0049] (4) The generated liquid III passes through the second reactor discharge valve I, and the overflow liquid J enters the aging reactor V, where polymer monomers and initiator L are added, and then an aging polymerization reaction is carried out;
[0050] (5) The material obtained in step (4) is discharged through the aging kettle liquid discharge valve K, and then dried and roasted to obtain the alumina.
[0051] In the present invention, the specific surface area and pore volume are measured by low-temperature liquid nitrogen adsorption method; and the particle size distribution is measured by a laser particle size distribution analyzer.
[0052] In the present invention, the crystallinity is measured by X-ray diffraction (XRD), wherein the crystallinity of SB powder (Condea, Germany) is 100%. XRD characterization uses a Japanese Rigaku D / max2500 X-ray diffractometer: Cu Kα ray, graphite monochromator, tube voltage 40kV, tube current 80mA, scanning range 10° to 70°, step length 0.01°, scanning frequency 1(°) / min.
[0053] Example 1
[0054] The process of producing aluminum oxide in this embodiment is as follows Figure 1 shown.
[0055] 2 L of n-hexanol was added as a reaction medium to a 10 L first reaction kettle I, and 1.6 g of AgCl was added. The pressure of the first reaction kettle I was adjusted to 5 MPa, the temperature to 10° C., the atmosphere to air, and the stirring rate to 200 rad / min. After stirring evenly, the acid solution feed port and the alkali solution feed port at the upper end of the first reactor were opened, and the flow rates of the aluminum sulfate solution with a concentration of 20g / 100mL and the sodium aluminate solution with a concentration of 10g / 100mL were controlled to be 20mL / min and 15mL / min, respectively. The reaction pH value was 2.5. After 15 minutes of neutralization reaction, the overflow port control valve at the lower end was opened to allow the generated liquid I to flow into the settling tank II. At the same time, n-hexanol and AgCl were added to the first reactor I at a rate of 10ml / min and 0.1g / min, respectively. After the volume of the generated liquid in the settling tank II reached 1 / 2 of that, it was switched to the settling tank III, and the organic solvent and sol II in the settling tank II were separated. The organic solvent can be recycled to the first reactor I. The properties of sol IIA are shown in Table 1.
[0056] Add 2.5L of pure water to the second reactor IV, adjust the pressure of the second reactor to 10MPa, the temperature to 180°C, and the stirring rate to 300rad / min. Open the sol II feed port and the alkali solution feed port at the upper end of the second reactor, control the flow rates of the sol II and the sodium aluminate solution with a concentration of 30g / 100mL to 15mL / min and 20mL / min respectively, adjust the reaction pH to 7.5, and after 60min of neutralization reaction, the generated liquid III is discharged from the second reactor.
[0057] The generated liquid III enters the aging kettle, and 5.9g of methyl ethyl ketone peroxide and 20g of oxalic acid are added, wherein the molar ratio of the generated liquid III to the polymer monomer is 15:1 in terms of Al2O3, and the amount of the initiator added is 2% of the amount of the polymer monomer. The pressure of the aging kettle is adjusted to 15MPa, the temperature to 280°C, and the stirring rate to 500rad / min. After polymerization aging for 150min, it is filtered, dried at 150°C for 4h, and calcined at 400°C for 3h in an air atmosphere to obtain aluminum oxide A, the properties of which are shown in Table 2. After the polymerization reaction, the degree of polymerization of the polymer in the obtained product is 50.
[0058] Example 2
[0059] The process of producing aluminum oxide in this embodiment is as follows Figure 1 shown.
[0060] 2.5 L of hexene was added as a reaction medium to a 10 L first reactor I, and 9 g of ZnS was added. The pressure of the first reactor I was adjusted to 7 MPa, the temperature to 0° C., the atmosphere to air, and the stirring rate to 300 rad / min. After stirring evenly, the acid solution feed port and the alkali solution feed port at the upper end of the first reactor were opened, and the flow rates of the aluminum sulfate solution with a concentration of 30g / 100mL and the sodium aluminate solution with a concentration of 25g / 100mL were controlled to be 30mL / min and 25mL / min, respectively. The reaction pH value was 3.5. After 30 minutes of neutralization reaction, the overflow port control valve at the lower end was opened to allow the generated liquid I to flow into the settling tank II. At the same time, cyclohexane and ZnS were added to the first reactor I at a rate of 15ml / min and 0.2g / min, respectively. After the volume of the generated liquid in the settling tank II reached 3 / 4 of it, it was switched to the settling tank III, and the organic solvent and sol II in the settling tank II were separated. The organic solvent can be recycled to the first reactor I. The properties of sol IIB are shown in Table 1.
[0061] Add 3L of pure water to the second reactor IV, adjust the pressure of the second reactor to 10MPa, the temperature to 180°C, and the stirring rate to 300rad / min. Open the sol II feed port and the alkali solution feed port at the upper end of the second reactor, control the flow rates of 30g / 100mL sol II and 25g / 100mL aluminum sulfate solution to 20mL / min and 30mL / min respectively, the reaction pH value is 9.5, and after 120min of neutralization reaction, the generated liquid III is discharged from the second reactor.
[0062] The generated liquid III enters the aging kettle, and 5g of methyl ethyl ketone peroxide and 40g of succinic acid are added, wherein the molar ratio of the generated liquid III to the polymer monomer is 13:1 in terms of Al2O3, and the amount of the initiator added is 1.1% of the amount of the polymer monomer. The pressure of the aging kettle is adjusted to 20MPa, the temperature is 250°C, and the stirring rate is 500rad / min. After polymerization aging for 180min, it is filtered, dried at 180°C for 5h, and calcined at 350°C for 4h in an air atmosphere to obtain aluminum oxide B, the properties of which are shown in Table 2. After the polymerization reaction, the degree of polymerization of the polymer in the obtained product is 10.
[0063] Example 3
[0064] The process of producing aluminum oxide in this embodiment is as follows Figure 1 shown.
[0065] 5 L of benzoic acid was added as a reaction medium to a 10 L first reactor I, and 13 g of CuS was added. The pressure of the first reactor I was adjusted to 8 MPa, the temperature to 15° C., the atmosphere to air, and the stirring rate to 250 rad / min. After stirring evenly, the acid solution feed port and the alkali solution feed port at the upper end of the first reactor were opened, and the flow rates of the aluminum sulfate solution with a concentration of 40g / 100mL and the sodium aluminate solution with a concentration of 35g / 100mL were controlled to be 20mL / min and 10mL / min, respectively. The reaction pH value was 4.5. After 60 minutes of neutralization reaction, the overflow port control valve at the lower end was opened to allow the generated liquid I to flow into the settling tank II. At the same time, benzoic acid and CuS were added to the first reactor I at a rate of 20ml / min and 0.5g / min, respectively. After the volume of the generated liquid in the settling tank II reached 2 / 3 of it, it was switched to the settling tank III, and the organic solvent and sol II in the settling tank II were separated. The organic solvent can be recycled to the first reactor I. The properties of sol II C are shown in Table 1.
[0066] Add 3L of pure water to the second reactor IV, adjust the pressure of the second reactor to 12MPa, the temperature to 200°C, and the stirring rate to 450rad / min. Open the sol II feed port and the alkali solution feed port at the upper end of the second reactor, control the flow rates of the sol II and the sodium metaaluminate solution with a concentration of 30g / 100mL to 10mL / min and 25mL / min respectively, adjust the reaction pH to 9.5, and after 100min of neutralization reaction, the generated liquid III is discharged from the second reactor.
[0067] The generated liquid III was added to the aging kettle, and 7g of hydrogen peroxide / ferrous chloride and 52g of ethylene glycol were added, wherein the molar ratio of the generated liquid III to the polymer monomer was 10:1 in terms of Al2O3, and the amount of the initiator added was 1.2% of the amount of the polymer monomer. The pressure of the aging kettle was adjusted to 15MPa, the temperature to 300°C, and the stirring rate to 400rad / min. After aging for 240min, it was filtered, dried at 200°C for 3h, and calcined at 500°C for 4h in an air atmosphere to obtain aluminum oxide C, the properties of which are shown in Table 2. After the polymerization reaction, the degree of polymerization of the polymer in the obtained product was 20.
[0068] Example 4
[0069] The process of producing aluminum oxide in this embodiment is as follows Figure 1 shown.
[0070] 4 L of styrene was added as a reaction medium into a 10 L first reactor I, and 7 g of HgS was added. The pressure of the first reactor I was adjusted to 9 MPa, the reaction temperature to 5° C., the atmosphere to air, and the stirring rate to 500 rad / min. After stirring evenly, the acid solution feed port and the alkali solution feed port at the upper end of the first reactor were opened, and the aluminum sulfate solution with a concentration of 50g / 100mL and the sodium aluminate solution with a concentration of 25g / 100mL were added at a flow rate of 20mL / min and 15mL / min, respectively. The reaction pH value was 4.5. After 45 minutes of neutralization reaction, the overflow port control valve at the lower end was opened to allow the generated liquid I to flow into the high-pressure sedimentation tank II. At the same time, styrene and HgS were added to the high-pressure reactor I at a rate of 30ml / min and 0.5g / min, respectively. After the volume of the generated liquid in the high-pressure sedimentation tank II reached 4 / 5 of it, it was switched to the high-pressure sedimentation tank III, and the organic solvent and sol II in the high-pressure sedimentation tank II were separated. The organic solvent can be recycled to the first reactor I. The properties of sol IID are shown in Table 1.
[0071] Add 3L of pure water to the second reactor IV, adjust the pressure of the second reactor to 15MPa, the temperature to 190°C, and the stirring rate to 450rad / min. Open the sol II feed port and the alkali solution feed port at the upper end of the second reactor, control the flow rates of the sol II and the aluminum sulfate solution with a concentration of 45g / 100mL to 25mL / min and 40mL / min respectively, adjust the reaction pH to 7.5, and after 80min of neutralization reaction, the generated liquid III is discharged from the second reactor.
[0072] The generated liquid III flows into the aging kettle, and 10g of methyl ethyl ketone peroxide and 30g of neopentyl glycol are added, wherein the molar ratio of the generated liquid III to the polymer monomer is 12:1 in terms of Al2O3, and the amount of the initiator added is 3% of the amount of the polymer monomer. The pressure of the aging kettle is adjusted to 12MPa, the temperature to 400°C, and the stirring rate to 500rad / min. After aging for 240min, it is filtered, dried at 180°C for 2h, and calcined at 400°C for 3h in an air atmosphere to obtain aluminum oxide D, the properties of which are shown in Table 2. After the polymerization reaction, the degree of polymerization of the polymer in the obtained product is 40.
[0073] Comparative Example 1
[0074] The process of producing aluminum oxide in this embodiment is as follows Figure 1 shown.
[0075] 5L of benzoic acid was added as the reaction medium to the 10L first reactor I, and 13g of CuS was added. The pressure of the first reactor I was adjusted to normal pressure, the temperature was 75°C, and the stirring rate was 250rad / min. After stirring evenly, the acid solution feed port and the alkali solution feed port at the upper end of the first reactor were opened, and the flow rates of the aluminum sulfate solution with a concentration of 40g / 100mL and the sodium metaaluminate solution with a concentration of 35g / 100mL were controlled to be 20mL / min and 10mL / min, respectively. The reaction pH value was 4.5. After the neutralization reaction for 60min, the overflow port control valve at the lower end was opened to allow the generated liquid I to flow into the settling tank II. At the same time, benzoic acid and CuS were added to the first reactor I at a rate of 20ml / min and 0.5g / min, respectively. After the volume of the generated liquid in the settling tank II reached 2 / 3 of it, it was switched to the settling tank III, and the organic solvent and sol II in the settling tank II were separated. The organic solvent can be recycled to the first reactor I. The properties of sol IIE are shown in Table 1.
[0076] Add 3L of pure water to the second reactor IV, adjust the pressure of the second reactor to normal pressure, the temperature to 75°C, and the stirring rate to 450rad / min. Open the sol II feed port and the alkali solution feed port at the upper end of the second reactor, control the flow rates of the sol II and the sodium aluminate solution with a concentration of 30g / 100mL to 10mL / min and 25mL / min respectively, adjust the reaction pH to 9.5, and after 100min of neutralization reaction, the generated liquid III is discharged from the second reactor.
[0077] The generated liquid III was added to the aging kettle, and 7g of hydrogen peroxide / ferrous chloride and 52g of ethylene glycol were added, wherein the molar ratio of the generated liquid III to the polymer monomer was 10:1 in terms of Al2O3, and the amount of the initiator added was 1.2% of the amount of the polymer monomer. The pressure of the aging kettle was adjusted to 15MPa, the temperature to 300°C, and the stirring rate to 400rad / min. After aging for 240min, it was filtered, dried at 200°C for 3h, and calcined at 500°C for 4h in an air atmosphere to obtain aluminum oxide E, the properties of which are shown in Table 2. After the polymerization reaction, the degree of polymerization of the polymer in the obtained product was 20.
[0078] Comparative Example 2
[0079] The process of producing aluminum oxide in this embodiment is as follows Figure 1 shown.
[0080] 5 L of pure water was added as a reaction medium to a 10 L first reactor I, and 13 g of CuS was added. The pressure of the first reactor I was adjusted to 8 MPa, the temperature to 15° C., the atmosphere to air, and the stirring rate to 250 rad / min. After stirring evenly, the acid solution feed port and the alkali solution feed port at the upper end of the first reactor were opened, and the flow rates of the aluminum sulfate solution with a concentration of 40g / 100mL and the sodium aluminate solution with a concentration of 35g / 100mL were controlled to be 20mL / min and 10mL / min, respectively. The reaction pH value was 4.5. After 60 minutes of neutralization reaction, the overflow port control valve at the lower end was opened to allow the generated liquid I to flow into the settling tank II. At the same time, benzoic acid and CuS were added to the first reactor I at a rate of 20ml / min and 0.5g / min, respectively. After the volume of the generated liquid in the settling tank II reached 2 / 3 of it, it was switched to the settling tank III, and the organic solvent and sol II in the settling tank II were separated. The organic solvent can be recycled to the first reactor I. The properties of sol IIF are shown in Table 1.
[0081] Add 3L of pure water to the second reactor IV, adjust the pressure of the second reactor to 12MPa, the temperature to 200°C, and the stirring rate to 450rad / min. Open the sol II feed port and the alkali solution feed port at the upper end of the second reactor, control the flow rates of the sol II and the sodium metaaluminate solution with a concentration of 30g / 100mL to 10mL / min and 25mL / min respectively, adjust the reaction pH to 9.5, and after 100min of neutralization reaction, the generated liquid III is discharged from the second reactor.
[0082] The generated liquid III was added to the aging kettle, and the pressure of the aging kettle was adjusted to 15 MPa, the temperature to 300°C, and the stirring rate to 400 rad / min. After aging for 240 minutes, it was filtered, dried at 200°C for 3 hours, and calcined at 500°C for 4 hours in an air atmosphere to obtain alumina F. Its properties are shown in Table 2.
[0083] Comparative Example 3
[0084] The process of producing aluminum oxide in this embodiment is as follows Figure 1 shown.
[0085] Add 5L of benzoic acid as the reaction medium to the 10L first reactor I, adjust the pressure of the first reactor I to 8MPa, the temperature to 15°C, the atmosphere to air, and the stirring rate to 250rad / min. After stirring evenly, open the acid solution feed port and the alkali solution feed port at the upper end of the first reactor, control the flow rates of the aluminum sulfate solution with a concentration of 40g / 100mL and the sodium metaaluminate solution with a concentration of 35g / 100mL to 20mL / min and 10mL / min respectively, and the reaction pH value is 4.5. After 60min of neutralization reaction, open the overflow control valve at the lower end to allow the generated liquid I to flow into the settling tank II, and at the same time, add benzoic acid to the first reactor I at a rate of 20ml / min. After the volume of the generated liquid in the settling tank II reaches 2 / 3 of it, switch to the settling tank III, and separate the organic solvent and sol II in the settling tank II, and the organic solvent can be recycled to the first reactor I. The properties of sol II G are shown in Table 1.
[0086] Add 3L of pure water to the second reactor IV, adjust the pressure of the second reactor to 12MPa, the temperature to 200°C, and the stirring rate to 450rad / min. Open the sol II feed port and the alkali solution feed port at the upper end of the second reactor, control the flow rates of the sol II and the sodium metaaluminate solution with a concentration of 30g / 100mL to 10mL / min and 25mL / min respectively, adjust the reaction pH to 9.5, and after 100min of neutralization reaction, the generated liquid III is discharged from the second reactor.
[0087] The generated liquid III was added to the aging kettle, and 7g of hydrogen peroxide / ferrous chloride and 52g of ethylene glycol were added, wherein the molar ratio of the generated liquid III to the polymer monomer was 10:1 in terms of Al2O3, and the amount of the initiator added was 1.2% of the amount of the polymer monomer. The pressure of the aging kettle was adjusted to 15MPa, the temperature to 300°C, and the stirring rate to 400rad / min. After aging for 240min, it was filtered, dried at 200°C for 3h, and calcined at 500°C for 4h in an air atmosphere to obtain aluminum oxide G, the properties of which are shown in Table 2. After the polymerization reaction, the degree of polymerization of the polymer in the obtained product was 20.
[0088] Comparative Example 4
[0089] The process of producing aluminum oxide in this embodiment is as follows Figure 1 shown.
[0090] 5 L of benzoic acid was added as a reaction medium to a 10 L first reactor I, and 13 g of CuS was added. The pressure of the first reactor I was adjusted to 8 MPa, the temperature to 15° C., the atmosphere to air, and the stirring rate to 250 rad / min. After stirring evenly, the acid solution feed port and the alkali solution feed port at the upper end of the first reactor were opened, and the flow rates of the aluminum sulfate solution with a concentration of 40g / 100mL and the sodium aluminate solution with a concentration of 35g / 100mL were controlled to be 20mL / min and 10mL / min, respectively. The reaction pH value was 4.5. After 60 minutes of neutralization reaction, the overflow port control valve at the lower end was opened to allow the generated liquid I to flow into the settling tank II. At the same time, benzoic acid and CuS were added to the first reactor I at a rate of 20ml / min and 0.5g / min, respectively. After the volume of the generated liquid in the settling tank II reached 2 / 3 of it, it was switched to the settling tank III, and the organic solvent and sol II in the settling tank II were separated. The organic solvent can be recycled to the first reactor I. The properties of sol IIH are shown in Table 1.
[0091] Add 3L of pure water to the second reactor IV, adjust the pressure of the second reactor to 12MPa, the temperature to 200°C, and the stirring rate to 450rad / min. Open the sol II feed port and the alkali solution feed port at the upper end of the second reactor, control the flow rates of the sol II and the sodium metaaluminate solution with a concentration of 30g / 100mL to 10mL / min and 25mL / min respectively, adjust the reaction pH to 9.5, and after 100min of neutralization reaction, the generated liquid III is discharged from the second reactor.
[0092] The generated liquid III was added to the aging kettle, and the pressure of the aging kettle was adjusted to 15 MPa, the temperature to 300°C, and the stirring rate to 400 rad / min. After aging for 240 minutes, it was filtered, dried at 200°C for 3 hours, and calcined at 500°C for 4 hours in an air atmosphere to obtain alumina H. Its properties are shown in Table 2.
[0093] Table 1 Properties of Sol II obtained in Examples and Comparative Examples
[0094]
[0095]
[0096] Table 2 Properties of aluminum oxide obtained in Examples and Comparative Examples
[0097] A B C D E F G H <![CDATA[Specific surface area, m 2 / g]]> 420 450 519 457 290 265 241 315 Pore volume, mL / g 2.0 2.9 2.5 3.0 0.93 0.88 0.79 0.98 Relative crystallinity, % 98 98 99 97 92 87 85 97 Particle size distribution, % <150μm 3.6 4.2 2.9 4.9 30.5 21.9 15.9 0.6 150~250μm 4.8 5.0 3.6 2.9 45.8 32.9 22.7 14.7 >250μm 91.6 90.8 93.5 92.2 23.7 45.2 61.4 84.7 Pore size distribution, % <200nm 1.5 2.5 1.7 4.3 95.2 96.3 98.6 84.3 200~300nm 93.7 92.5 94.3 91.9 0.5 1.2 0.3 10.2 >300nm 4.8 5.0 4.0 3.8 4.3 2.5 1.1 5.5
Claims
1. Alumina, characterized in that: The properties of the alumina are as follows: pore volume of 2.0-3.0 ml / g; specific surface area of 410-550 m 2 / g, the volume of pores with a pore size of 200-300 nm accounts for 90.0%-95.0% of the total pore volume; The particle size distribution of the aluminum oxide is as follows: the proportion of grains with a particle size less than 150 μm is 0.5% to 5.0%, the proportion of grains with a particle size of 150 to 250 μm is 2.0% to 5.0%, and the proportion of grains with a particle size greater than 250 μm is 90.0% to 95.0%.
2. Aluminum oxide according to claim 1, characterized in that The relative crystallinity of the aluminum oxide is ≮90%.
3. Aluminum oxide according to claim 1, characterized in that The relative crystallinity of the aluminum oxide is 95% to 99%.
4. A method for producing aluminum oxide, comprising: (1) Adding an organic solvent, polar metal seed crystals, acidic aluminum salt solution I and alkaline aluminum salt solution I to a first reaction kettle in parallel for neutralization to form a gel, thereby obtaining a generated solution I; the polar metal seed crystals are selected from one or more of AgCl, ZnS, CuS or HgS; the organic solvent is an organic substance that is immiscible with water or slightly soluble in water, and is selected from one or more of alkanes, olefins, organic alcohols and organic acids; (2) The resulting liquid I enters a sedimentation tank for sedimentation separation to obtain an upper layer, i.e., an organic solvent, and a lower layer, i.e., a sol II; (3) The sol II and the acidic or alkaline aluminum salt solution II flow into the second reaction kettle in parallel to undergo a neutralization and gelation reaction to obtain a generated solution III; (4) The generated liquid III enters an aging kettle, and a polymerization monomer and an initiator are added, and then an aging polymerization reaction is carried out; the polymerization monomer is at least one of an organic alcohol or an organic acid, and the initiator is selected from at least one of a peroxide compound initiator, an azo initiator, and a redox initiator; (5) drying and calcining the material obtained in step (4) to obtain the alumina; The operating conditions of the first reaction kettle in step (1) are as follows: temperature of -15 to 15°C, pressure of 5 to 20 MPa; the reaction conditions of the neutralization to gelatinization in step (1) are as follows: pH value of 2 to 6, reaction time of 10 to 180 minutes; The operating conditions of the second reactor described in step (3) are as follows: temperature of 100-300° C., pressure of 5-20 MPa; the reaction conditions of the neutralization and gelling in step (3) are as follows: pH value of 7-12, reaction time of 10-180 minutes.
5. The production method according to claim 4, characterized in that: The production method is carried out in a continuous manner.
6. The production method according to claim 4 or 5, characterized in that: The settling tank used in step (2) and the aging kettle used in step (4) are both provided in plurality for switching use; in step (1), the first reactor adopts an overflow operation mode to discharge the generated liquid I from the first reactor, and in step (3), the second reactor adopts an overflow operation mode to discharge the generated liquid III from the second reactor.
7. The production method according to claim 4, characterized in that: When continuous production of alumina is adopted, when the first reactor is started, an organic solvent and polar metal seeds are first added as a base liquid, and then acidic aluminum salt solution I and alkaline aluminum salt solution I are added in parallel for neutralization into gel, until the generated liquid I begins to be discharged from the first reactor; wherein, the amount of the organic solvent added in the base liquid is 1 / 5 to 1 / 2 of the actual effective use volume of the first reactor, and when the generated liquid I begins to be discharged from the first reactor, the total mass of the acidic aluminum salt solution I and the alkaline aluminum salt solution I in the first reactor is calculated as Al2O3, and the amount of the polar metal seeds added accounts for 0.1% to 5.0%.
8. The production method according to claim 7, characterized in that: When alumina is produced continuously, when the generated liquid I begins to be discharged from the first reactor, the total mass of the acidic aluminum salt solution I and the alkaline aluminum salt solution I in the first reactor is based on Al2O3, and the added amount of the polar metal seed crystal accounts for 0.5% to 4.0%.
9. The production method according to claim 4, characterized in that: When continuous production of alumina is adopted, when the second reactor is started, bottom water is added first, and then sol II and acidic aluminum salt solution II or alkaline aluminum salt solution II are added in parallel to neutralize into gel, until the generated liquid III begins to discharge from the second reactor; wherein, the amount of bottom water added is 1 / 7 to 1 / 2 of the actual effective use volume of the second reactor.
10. The production method according to claim 9, characterized in that: When continuous production of alumina is adopted, the amount of bottom water added is 1 / 6 to 1 / 3 of the actual effective use volume of the second reactor.
11. The production method according to claim 4, characterized in that: The organic solvent in step (1) is an organic substance that is immiscible with water or slightly soluble in water, and the carbon number of the organic substance is 5 to 12.
12. The production method according to claim 4, characterized in that: The operating conditions of the first reactor described in step (1) are as follows: temperature is -0 to 15°C, and pressure is 5 to 15 MPa; the reaction conditions of the neutralization gelation in step (1) are as follows: pH value is 2 to 5, and reaction time is 10 to 60 minutes.
13. The production method according to claim 12, characterized in that: The neutralization and gelling reaction in step (1) is carried out under stirring conditions, and the stirring rate is 100 to 500 rad / min.
14. The production method according to claim 4, characterized in that: In step (1) or step (3), the acidic aluminum salt is selected from one or more of AlCl3, Al2(SO4)3 or Al(NO)3, the acidic aluminum salt solution is an aqueous solution, and the concentration of the acidic aluminum salt aqueous solution is 10 to 100 g / 100 mL calculated as Al2O3; the alkaline aluminum salt is selected from one or both of NaAlO2 and KAlO2, the alkaline aluminum salt solution is an aqueous solution, and the concentration of the alkaline aluminum salt aqueous solution is 10 to 100 g / 100 mL calculated as Al2O3.
15. The production method according to claim 4, characterized in that: The organic solvent and polar metal seeds are added to the first reaction kettle in parallel, wherein the ratio of the organic solvent addition rate to the sum of the addition rates of the acidic aluminum salt solution I and the alkaline aluminum salt solution I based on their volumes is 0.1:1-10:1, and the polar metal seeds addition rate is 1%-10% of the sum of the addition rates of the acidic aluminum salt solution I and the alkaline aluminum salt solution I based on the mass of Al2O3.
16. The production method according to claim 15, characterized in that The organic solvent and polar metal seeds are added to the first reaction kettle in parallel, wherein the ratio of the organic solvent addition rate to the sum of the addition rates of the acidic aluminum salt solution I and the alkaline aluminum salt solution I based on their volumes is 0.2:1-5:1, and the polar metal seeds addition rate is 1%-5% of the sum of the addition rates of the acidic aluminum salt solution I and the alkaline aluminum salt solution I based on the mass of Al2O3.
17. The production method according to claim 4, characterized in that: The particle size distribution of the sol II obtained in step (2) is as follows: the proportion of grains with a particle size of less than 50 nm is 0.5% to 5.0%, the proportion of grains with a particle size of 50 to 100 nm is 2% to 5%, and the proportion of grains with a particle size of more than 100 nm is 90% to 95%; the relative crystallinity of the obtained sol II is ≮95%.
18. The production method according to claim 17, characterized in that: The relative crystallinity of the sol II obtained in step (2) is 95% to 98%.
19. The production method according to claim 4, characterized in that: The operating conditions of the settling tank in step (2) are as follows: temperature is -15 to 15°C, and pressure is 5 to 20 MPa.
20. The production method according to claim 19, characterized in that The operating conditions of the settling tank in step (2) are as follows: temperature of 0-15°C and pressure of 5-15MPa.
21. The production method according to claim 4, characterized in that: The operating conditions of the second reactor described in step (3) are as follows: temperature of 100-200° C., pressure of 5-17 MPa; the reaction conditions of the neutralization and gelling in step (3) are as follows: pH value of 7.5-10.0, reaction time of 10-120 minutes.
22. The production method according to claim 21, characterized in that The neutralization and gelling reaction in step (3) is carried out under stirring conditions, and the stirring rate is 100 to 500 rad / min.
23. The production method according to claim 4, characterized in that: In step (4), the molar ratio of the generated solution III to the polymerizable monomer is 20:1 to 1:1 in terms of Al2O3; and the amount of the initiator added is 0.01% to 3.5% of the mass of the polymerizable monomer.
24. The production method according to claim 23, characterized in that In step (4), the molar ratio of the generated solution III to the polymerizable monomer is 15:1 to 1:1, calculated as Al2O3.
25. The production method according to claim 4, characterized in that: In step (4), the degree of polymerization of the polymer formed by the aging polymerization reaction is 5 to 100.
26. The production method according to claim 25, characterized in that In step (4), the degree of polymerization of the polymer formed by the aging polymerization reaction is 5 to 50.
27. The production method according to claim 4, characterized in that: In step (4), the aging polymerization reaction conditions are: temperature 200-400°C, pressure 15-20MPa, aging polymerization time 100-360min; The aging polymerization is carried out under stirring conditions with a stirring speed of 500 to 800 r / min.
28. The production method according to claim 27, characterized in that In step (4), the aging polymerization time is 150 to 250 minutes.
29. The production method according to claim 4, characterized in that: In step (5), the drying temperature is 100-450° C., and the drying time is 1-10 hours; the roasting temperature is 300-800° C., and the roasting time is 2-5 hours. The roasting atmosphere is one or more of air, nitrogen or water vapor.
30. The production method according to claim 29, characterized in that In step (5), the drying temperature is 150-400° C.; the roasting temperature is 350-550° C., and the roasting time is 2-4 hours.