A method for solidifying nonferrous metal tailings with 4A zeolite and solidified body thereof
By using a composite of 4A zeolite and siliceous and aluminum raw materials for solidification in non-ferrous metal tailings, the problems of high energy consumption and difficult to repair heavy metal pollution in the existing technology are solved, and high-efficiency solidification with low cost and low energy consumption is achieved. The effect ensures the green environmental protection and economic benefits of the environment.
Patent Information
- Application Number
- CN202310102731.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-17
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2043-01-17
AI Technical Summary
When dealing with non-ferrous metal tailings, the existing technology has the problems of high energy consumption, high cost and inability to effectively repair heavy metal pollution, making it difficult to solve environmental pollution.
4A zeolite is mixed with siliceous raw materials and aluminum raw materials, and is uniformly stirred or injected into non-ferrous metal tailings to form a 4A zeolite-non-ferrous metal tailings complex, and reacts at room temperature and normal pressure to generate 4A zeolite-non-ferrous metals. Tailings solidified body uses additives such as sodium hydroxide to improve the solidification effect.
It has achieved low-cost, low-energy consumption solidification of non-ferrous metal tailings with low heavy metal leaching rate, solving the problem of environmental pollution. The 4A zeolite solidified body has a solidification rate of cationic heavy metals of more than 90%, which has green environmental protection and economic benefits.
Smart Images

Figure CN116119680B
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tailings solidification, in particular to a method for solidifying non-ferrous metal tailings with 4A zeolite and a solidified body thereof. Background Art
[0002] With the increase in demand for non-ferrous metal minerals, a large amount of non-ferrous metal tailings will be produced. As solid waste after beneficiation and smelting, non-ferrous metal tailings have small particle size, low particle cohesion, and multiple heavy metal biological toxicity. They are often piled up outdoors, causing environmental pollution such as air pollution, soil pollution and water pollution. The heavy metals in non-ferrous metal tailings can easily migrate from the tailings to the surrounding environment through geochemical reactions, leading to heavy metal pollution in the surrounding soil and water sources, and bringing great pressure to the restoration of the ecological environment around the mining area. The heavy metal pollutants in non-ferrous metal tailings are mainly Fe, Mn, Pb, Zn, Cd, Cu, Ni, Sr, etc. In summary, as a special environmental medium, the management of non-ferrous metal tailings needs to take into account both the restoration of heavy metals and the consolidation of non-ferrous metal tailings particles.
[0003] At present, solidification / stabilization technology is often used to repair non-ferrous metal tailings in situ. The main solidification stabilizers are cement, natural minerals, asphalt, polypropylene, ferrous sulfate and phosphate. However, the above methods have high energy consumption, high cost, easy to produce secondary pollution, and cannot repair the heavy metal pollution caused by non-ferrous metal tailings. A method with low energy consumption and the ability to repair the heavy metal pollution caused by non-ferrous metal tailings is urgently needed. Summary of the invention
[0004] The object of the present invention is to solve at least one of the above-mentioned deficiencies in the prior art. One of the objects of the present invention is to provide a method for solidifying non-ferrous metal tailings.
[0005] To achieve the above objectives, the present invention provides a method for solidifying nonferrous metal tailings with 4A zeolite.
[0006] The method comprises the following steps: mixing siliceous raw materials, aluminum raw materials and non-ferrous metal tailings uniformly, adding water and stirring to obtain a 4A zeolite-non-ferrous metal tailings complex; or mixing siliceous raw materials, aluminum raw materials and water and injecting them into non-ferrous metal tailings to obtain a 4A zeolite-non-ferrous metal tailings complex; and reacting the 4A zeolite-non-ferrous metal tailings complex to obtain a 4A zeolite-non-ferrous metal tailings solidified body.
[0007] According to an exemplary embodiment of the present invention, an auxiliary agent is further added in the step of obtaining the 4A zeolite-nonferrous metal tailings complex.
[0008] According to an exemplary embodiment of the present invention, the auxiliary agent may include sodium hydroxide.
[0009] According to an exemplary embodiment of the present invention, the mixture of the silicon raw material, the aluminum raw material, the additive and the non-ferrous metal tailings can be uniformly mixed at a mass ratio of 0.01 to 0.5:1.
[0010] According to an exemplary embodiment of the present invention, the siliceous raw material may include one or more of sodium silicate pentahydrate, sodium silicate nonahydrate, orthosilicic acid, water glass, white carbon black and fumed silica.
[0011] According to an exemplary embodiment of the present invention, the aluminum raw material may include one or more of aluminum hydroxide, aluminum powder and sodium aluminate.
[0012] According to an exemplary embodiment of the present invention, the reaction conditions may be room temperature and normal pressure; wherein the room temperature is 2 to 30°C and the normal pressure is 1 atmosphere; the reaction may include a nucleation process, a crystallization process and a solidification process, wherein the reaction time of the nucleation process is 1 to 7 days, and the reaction time of the crystallization and solidification processes is 7 to 60 days.
[0013] According to an exemplary embodiment of the present invention, the molar ratio of SiO2, Al2O3 and Na2O of 4A zeolite in the 4A zeolite-non-ferrous metal tailings complex may be 0.5-1.5: 0.5-2.0: 0.5-2.0; the molar ratio of H2O to Na2O of 4A zeolite in the 4A zeolite-non-ferrous metal tailings complex may be 1-200: 0.8-1.2.
[0014] On the other hand, the present invention provides a 4A zeolite-nonferrous metal tailings solidified body, wherein the solidified body comprises the 4A zeolite-nonferrous metal tailings solidified body solidified by the method described above.
[0015] According to an exemplary embodiment of the present invention, the crystalline zeolite phase in the solidified body is one or more of 4A zeolite and faujasite, with a particle size of 100 to 600 nm; the early product is a spherical aggregate, and after crystallization, the 4A zeolite crystals are cubic; the solidification rate of the 4A zeolite-non-ferrous metal tailings solidified body for cationic heavy metals in non-ferrous metal tailings is above 90%.
[0016] Compared with the prior art, the beneficial effects of the present invention include at least one of the following:
[0017] (1) The method for solidifying nonferrous metals with 4A zeolite of the present invention is simple and convenient, and can effectively reduce the preparation cost.
[0018] (2) It can effectively solidify non-ferrous metal tailings, has good solidification performance, and low heavy metal leaching rate, thus solving the problem of environmental pollution caused by non-ferrous metal tailings.
[0019] (3) The reaction conditions of this method are room temperature and normal pressure, which is green and environmentally friendly, saves energy, and has important environmental and economic benefits.
[0020] (4) The temperature required for synthesizing 4A zeolite in the laboratory is much higher than the outdoor ambient temperature. The present application can make 4A zeolite crystallize at the outdoor ambient temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The above and other objects and features of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:
[0022] Figure 1 The X-ray diffraction pattern of the 4A zeolite-nonferrous metal tailings solidified body prepared in Example 1 of the present invention is shown;
[0023] Figure 2 The scanning electron microscope image of the 4A zeolite-nonferrous metal tailings solidified body prepared in Example 1 of the present invention is shown;
[0024] Figure 3 A schematic diagram showing the solidification rate of heavy metal ions in static leaching of non-ferrous metal tailings solidified by 4A zeolite in Example 1 of the present invention is shown;
[0025] Figure 4 The X-ray diffraction pattern of the 4A zeolite-nonferrous metal tailings solidified body prepared in Example 2 of the present invention is shown;
[0026] Figure 5 A schematic diagram showing the solidification rate of heavy metal ions in static leaching of non-ferrous metal tailings solidified by 4A zeolite in Example 2 of the present invention is shown;
[0027] Figure 6 The X-ray diffraction pattern of the 4A zeolite-nonferrous metal tailings solidified body prepared in Example 3 of the present invention is shown;
[0028] Figure 7 A schematic diagram showing the solidification rate of heavy metal ions in static leaching of non-ferrous metal tailings solidified by 4A zeolite in Example 3 of the present invention is shown. DETAILED DESCRIPTION
[0029] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention.
[0030] Exemplary Embodiment 1
[0031] This exemplary embodiment provides a method for solidifying nonferrous metal tailings with 4A zeolite. The method comprises the following steps:
[0032] S1. Mix the siliceous raw material, aluminum raw material, additive and non-ferrous metal tailings evenly, then add water and stir to obtain a 4A zeolite-non-ferrous metal tailings complex; or mix the siliceous raw material, aluminum raw material, additive and water and inject them into the non-ferrous metal tailings to obtain a 4A zeolite-non-ferrous metal tailings complex.
[0033] In this embodiment, a mixture of siliceous raw materials, aluminum raw materials, additives and non-ferrous metal tailings is placed in a 20 mm diameter, bottom-sealed plexiglass tube to obtain a 4A zeolite-non-ferrous metal tailings complex, and water is added to the mixture while stirring for reaction, or the siliceous raw materials, aluminum raw materials, additives and water are mixed and then injected into the non-ferrous metal tailings to obtain a 4A zeolite-non-ferrous metal tailings complex and then reacted.
[0034] In this embodiment, the non-ferrous metal tailings include one or more solid wastes such as non-ferrous metal ore dressing tailings and non-ferrous metal tailings contaminated soil.
[0035] In this embodiment, the siliceous raw material may include one or more of sodium silicate pentahydrate, sodium silicate nonahydrate, orthosilicic acid, water glass, white carbon black and fumed silica. For example, the siliceous raw material is sodium silicate pentahydrate, the siliceous raw material is water glass or the siliceous raw material is orthosilicic acid. The siliceous raw material provides a silicon source for synthesizing 4A zeolite.
[0036] In this embodiment, the aluminum raw material may include one or more of aluminum hydroxide, aluminum powder and sodium aluminate. For example, the aluminum raw material is aluminum hydroxide, the aluminum raw material is aluminum powder or the aluminum raw material is sodium aluminate. The aluminum raw material provides an aluminum source for synthesizing 4A zeolite.
[0037] In this embodiment, the auxiliary agent may include sodium hydroxide, or no auxiliary agent is added. The auxiliary agent is used to provide an alkaline environment for synthesizing 4A zeolite.
[0038] In this embodiment, the molar ratio of the chemical components SiO2, Al2O3 and Na2O of the siliceous raw material, aluminum raw material and additive of the 4A zeolite in the 4A zeolite-nonferrous metal tailings complex is 0.5-1.5:0.5-2.0:0.5-2.0. For example, the molar ratio of SiO2, Al2O3 and Na2O may be 1.0:1.0:2.0, 1.0:0.5:2.0, 1.0:2.0:2.0 or 1.0:0.5:0.75.
[0039] In this embodiment, the mass ratio of the mixture of siliceous raw material, aluminum raw material and additives of 4A zeolite to non-ferrous metal tailings in the 4A zeolite-non-ferrous metal tailings complex is 0.01-0.5:1, for example, the mass ratio is 0.5:1, 0.1:1, 0.3:1, 0.01:1.
[0040] In this embodiment, water is added to a mixture of siliceous raw materials, aluminum raw materials, additives and non-ferrous metal tailings while stirring, or siliceous raw materials, aluminum raw materials, additives and water are mixed and injected into non-ferrous metal tailings to obtain a 4A zeolite-non-ferrous metal tailings complex. The molar ratio of H2O to Na2O in the 4A zeolite-non-ferrous metal tailings complex is 1 to 200: 0.8 to 1.2. For example, 4.0: 1.0, 40: 1.0, 50: 0.9, 150: 1.1, 100: 1.0 or 200: 1.0.
[0041] S2, 4A zeolite-nonferrous metal tailings complex react to obtain 4A zeolite-nonferrous metal tailings solidified body.
[0042] In this embodiment, the reaction temperature is room temperature, which is 2-30° C., for example, 5° C., 10° C., 25° C. or 30° C. The reaction pressure is normal pressure, which is one standard atmospheric pressure.
[0043] In this embodiment, the reaction includes the process of 4A zeolite nucleation, crystallization and solidification of non-ferrous metal tailings, wherein the reaction time of the nucleation process is 1 to 7 days, for example, 3 days, 5 days, and 6 days; the reaction time of the crystallization and solidification of the non-ferrous metal tailings is 7 to 60 days, for example, 10 days, 20 days, 28 days, 35 days, 48 days, and 55 days.
[0044] In this embodiment, the method for synthesizing 4A zeolite-nonferrous metal tailings solidified body may further include a step of aging for 1 to 60 days after the water addition reaction, for example, the intermediate product may be aged for 10 days, 28 days or 60 days. Aging can allow the components in the intermediate product to react fully and the nonferrous metal tailings to be fully solidified.
[0045] In this embodiment, the molar ratio of SiO2, Al2O3, Na2O and H2O, the reaction temperature and the reaction time are the key parameter ranges for the synthesis of 4A zeolite. Beyond the parameter range, 4A zeolite cannot be synthesized and the 4A zeolite-non-ferrous metal tailings solidified body cannot be obtained.
[0046] The mixture of silicon, aluminum and additives reacts very quickly when it meets water. A small amount of silicon is dissolved and AlNaO is generated at the dissolved position. x Si y , AlNaO x Si y It should be a zeolite precursor with different silicon-aluminum ratios, that is, a gel containing 4A zeolite crystal nuclei. As the crystallization time increases, the precursor gradually grows and takes shape. If the crystallinity is high, a cubic structure of 4A zeolite will appear.
[0047] In this embodiment, the 4A zeolite-non-ferrous metal tailings solidified body has good solidification performance for heavy metals in non-ferrous metal tailings, and the heavy metal dissolution rate is low in static leaching. The solidification rate of the 4A zeolite-non-ferrous metal tailings solidified body for cationic heavy metals in non-ferrous metal tailings is above 90%.
[0048] Exemplary Embodiment 2
[0049] This exemplary embodiment provides a 4A zeolite-nonferrous metal tailings solidified body, which includes the 4A zeolite-nonferrous metal tailings solidified body solidified by the method described in Exemplary Embodiment 1.
[0050] In this embodiment, the crystalline zeolite phase in the solidified body is one or more of 4A zeolite and faujasite zeolite, with a particle size of 100-600 nm; the early product is a spherical aggregate, and after crystallization, the 4A zeolite crystals are cubic.
[0051] In this embodiment, the microscopic morphology of 4A zeolite in the 4A zeolite-nonferrous metal tailings solidified body may include spheres and cubes.
[0052] In this embodiment, the particle size of 4A zeolite in the 4A zeolite-nonferrous metal tailings solidified body can reach nanometer level.
[0053] In this embodiment, the particle size of 4A zeolite in the 4A zeolite-non-ferrous metal tailings solidified body is extremely small, reaching the nanometer level. The spherical polymer formed after solidifying the non-ferrous metal tailings covers the surface of the non-ferrous metal tailings particles, and has good solidification performance for heavy metals in the non-ferrous metal tailings.
[0054] In order to better understand the exemplary embodiments of the present invention, they are further described below in conjunction with specific examples.
[0055] Example 1
[0056] 9.1 g of sodium silicate pentahydrate, 7.0 g of sodium aluminate and 50 g of nonferrous metal tailings were fully mixed and placed in a 20 mm diameter, bottom-sealed organic glass tube.
[0057] At 25°C and normal pressure, 200 mL of deionized water was added to react to obtain a 4A zeolite-nonferrous metal tailings complex. The molar ratio of the chemical components SiO2, Al2O3, Na2O and H2O of the 4A zeolite in the 4A zeolite-nonferrous metal tailings complex is 1.0:1.0:2.0:40.
[0058] The composite was aged at a constant temperature of 25° C. for 14 days to obtain a 4A zeolite-nonferrous metal tailings solidified body.
[0059] Figure 1 and Figure 2They are respectively the X-ray diffraction pattern and scanning electron microscope image of the 4A zeolite-nonferrous metal tailings solidified body synthesized in Example 1. Figure 1 and Figure 2 As shown in the figure, the XRD diffraction peak of the 4A zeolite is sharp, the crystals are complete, and it is a typical 4A zeolite cubic structure. The crystals overlap closely with each other, and the particle size distribution is between 100 and 600 nm. The 4A zeolite covers the surface of the non-ferrous metal tailings. Figure 3 As shown in the figure, after 4A zeolite-nonferrous metal tailings solidified body was leached with deionized water at pH = 4 for 5 times, Mn 2+ and Sr 2 + The curing rate is 99.96%.
[0060] Example 2
[0061] 2.6 g of sodium silicate pentahydrate, 2 g of sodium aluminate and 50 g of nonferrous metal tailings were fully mixed and placed in a 20 mm diameter, bottom-sealed organic glass tube.
[0062] At 25°C and normal pressure, 35 mL of deionized water was added to react to obtain a 4A zeolite-nonferrous metal tailings complex. The molar ratio of the chemical components SiO2, Al2O3, Na2O and H2O of the 4A zeolite in the 4A zeolite-nonferrous metal tailings complex is 1.0:4.0:1.0:20.
[0063] The composite was aged at a constant temperature of 10° C. for 25 days to obtain a 4A zeolite-nonferrous metal tailings solidified body.
[0064] Figure 4 is the X-ray diffraction pattern of the 4A zeolite-nonferrous metal tailings solidified body synthesized in Example 2. Figure 4 As shown in Figure 2, no obvious 4A zeolite diffraction peaks were found in the XRD pattern. Figure 5 As shown, after the 4A zeolite-nonferrous metal tailings solidified body was subjected to 5 times of static leaching with deionized water at pH = 4, Mn 2+ and Sr 2+ The curing rate remains above 90%.
[0065] Example 3
[0066] 13 g of sodium silicate pentahydrate, 10 g of sodium aluminate and 50 g of nonferrous metal tailings were fully mixed and placed in a 20 mm diameter, bottom-sealed organic glass tube.
[0067] At 20°C and normal pressure, 73 mL of deionized water was added to react to obtain a 4A zeolite-nonferrous metal tailings complex. The molar ratio of the chemical components SiO2, Al2O3, Na2O and H2O of the 4A zeolite in the 4A zeolite-nonferrous metal tailings complex is 1.0:1.0:5.0:50.
[0068] The composite was aged at a constant temperature of 20° C. for 32 days to obtain a 4A zeolite-nonferrous metal tailings solidified body.
[0069] Figure 6 is the X-ray diffraction pattern of the 4A zeolite-nonferrous metal tailings solidified body synthesized in Example 3. Figure 6 As shown in FIG. 1 , the XRD diffraction peaks of the 4A zeolite can be observed, but the peaks are weak. Figure 7 As shown, after the 4A zeolite-nonferrous metal tailings solidified body was subjected to 5 times of static leaching with deionized water at pH = 4, Mn 2+ and Sr 2+ The curing rate remains above 95%.
[0070] Although the present invention has been described above by combining with exemplary embodiments, it will be apparent to those skilled in the art that various modifications and changes may be made to the exemplary embodiments of the present invention without departing from the spirit and scope defined in the claims.
Claims
1. A method for solidifying non-ferrous metal tailings using 4A zeolite, characterized in that: The method comprises the following steps: The siliceous raw material, the aluminum raw material and the non-ferrous metal tailings are mixed evenly, and then water is added while stirring to obtain a 4A zeolite-non-ferrous metal tailings complex; or The silicon raw material, the aluminum raw material and water are mixed and injected into the non-ferrous metal tailings to obtain a 4A zeolite-non-ferrous metal tailings complex; The 4A zeolite-nonferrous metal tailings complex is reacted to obtain a 4A zeolite-nonferrous metal tailings solidified body; At least one of the silicon raw material and the aluminum raw material contains sodium, and can make the molar ratio of SiO2, Al2O3 and Na2O of 4A zeolite in the 4A zeolite-nonferrous metal tailings complex be 0.5-1.5:0.5-2.0:0.5-2.0; The reaction conditions are room temperature and normal pressure; The reaction includes a nucleation process, a crystallization process and a solidification process, wherein the reaction time of the nucleation process is 1 to 7 days, and the reaction time of the crystallization and solidification process is 7 to 60 days.
2. A method for solidifying nonferrous metal tailings using 4A zeolite, characterized in that: The method comprises the following steps: The siliceous raw material, the aluminum raw material, the auxiliary agent and the non-ferrous metal tailings are mixed uniformly, and then water is added while stirring to obtain a 4A zeolite-non-ferrous metal tailings complex, wherein the auxiliary agent includes sodium hydroxide; or A siliceous raw material, an aluminum raw material, an additive and water are mixed and injected into the non-ferrous metal tailings to obtain a 4A zeolite-non-ferrous metal tailings complex, wherein the additive includes sodium hydroxide; The 4A zeolite-nonferrous metal tailings complex is reacted to obtain a 4A zeolite-nonferrous metal tailings solidified body; The silicon raw material, aluminum raw material and additive can make the molar ratio of SiO2, Al2O3 and Na2O of 4A zeolite in the 4A zeolite-nonferrous metal tailings complex be 0.5-1.5:0.5-2.0:0.5-2.0; The reaction conditions are room temperature and normal pressure; The reaction includes a nucleation process, a crystallization process and a solidification process, wherein the reaction time of the nucleation process is 1 to 7 days, and the reaction time of the crystallization and solidification process is 7 to 60 days.
3. The method for solidifying nonferrous metal tailings with 4A zeolite according to claim 2, characterized in that: The mixture of the silicon raw material, the aluminum raw material and the auxiliary agent is evenly mixed with the non-ferrous metal tailings at a mass ratio of 0.01 to 0.5:
1.
4. The method for solidifying nonferrous metal tailings with 4A zeolite according to claim 1 or 2, characterized in that: The siliceous raw material includes one or more of sodium silicate pentahydrate, sodium silicate nonahydrate, orthosilicic acid, water glass, white carbon black and fumed silica.
5. The method for solidifying nonferrous metal tailings with 4A zeolite according to claim 1 or 2, characterized in that: The aluminum raw material includes one or more of aluminum hydroxide, aluminum powder and sodium aluminate.
6. The method for solidifying nonferrous metal tailings with 4A zeolite according to claim 1 or 2, characterized in that: The room temperature is 2-30° C., and the normal pressure is 1 atmosphere.
7. The method for solidifying nonferrous metal tailings with 4A zeolite according to claim 1 or 2, characterized in that: The molar ratio of H2O to Na2O in the 4A zeolite-nonferrous metal tailings complex is 1-200:0.8-1.
2.
8. A 4A zeolite-nonferrous metal tailings solidified body, characterized in that: The solidified body comprises a 4A zeolite-nonferrous metal tailings solidified body solidified by the method according to any one of claims 1 to 7.
9. The 4A zeolite-nonferrous metal tailings solidified body according to claim 8, characterized in that: The crystalline zeolite phase in the solidified body is 4A zeolite, and the particle size is 100 to 600 nm; The early products are spherical aggregates, and after the crystallization is completed, the 4A zeolite crystals are cubic; The 4A zeolite-nonferrous metal tailings solidification body has a solidification rate of more than 90% for cationic heavy metals in nonferrous metal tailings.