Skin-feeling, stain-resistant, and wear-resistant UV topcoat and preparation method thereof

By using a combination of polyurethane modified acrylate, thermoset polymethylurea polymer and fluorosilicone curing resin in UV topcoat, the problems of increased viscosity and deterioration of stain resistance are solved, and high matteness and wear resistance are achieved It takes into account both the effect of stain resistance.

CN116463017BActive Publication Date: 2024-11-12TREEZO NEW MATERIAL TECH GRP CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310411871.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-11-12
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

When the existing UV topcoat pursues matte and stain resistance, conventional methods will lead to an increase in the viscosity of the topcoat, making it difficult to maintain low viscosity, resulting in a decrease in the wear resistance after molding, and excessive organic matting powder will lead to a worsening stain resistance effect. , it is difficult to take into account high mattness and wear resistance.

Method used

Polyurethane modified acrylate is used as the main resin, combined with thermoset polymethylurea polymer (PMU) as organic matte powder, and fluorosilicone curing resin and polyether modified silicone are used as leveling agents, through specific formulation combinations and The stirring process ensures that the topcoat maintains low viscosity after drying and improves wear and stain resistance.

Benefits of technology

The high matte, wear and stain resistance of UV topcoat is achieved, avoiding the problems of increasing the viscosity of the topcoat and decreasing the stain resistance effect, ensuring the smoothness of the coating process and the excellent performance of the finished product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004936539290000021
    Figure GDA0004936539290000021
  • Figure GDA0004936539290000041
    Figure GDA0004936539290000041
  • Figure GDA0004936539290000051
    Figure GDA0004936539290000051
Patent Text Reader

Abstract

The present invention discloses a skin-feeling, stain-resistant, and wear-resistant UV topcoat and a preparation method thereof. The skin-feeling, stain-resistant, and wear-resistant UV topcoat of the present invention comprises the following components, each component being measured by mass percentage: 25%-45% UV light-curing main resin, 15%-50% UV light-curing dilution monomer, 5%-25% UV light-curing functional resin, 2%-8% photoinitiator, 8%-15% organic matte powder, and 0.1%-0.5% other auxiliaries. The present invention obtains a UV topcoat with excellent performance by changing the UV-curing main resin in the topcoat formula, replacing conventional matte powder with organic matte powder, and adding fluorosilicone UV resin with excellent stain resistance. While maintaining matte and hand feel, the stain resistance, scratch resistance, and wear resistance of the paint film are also greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of decorative panels, and more specifically to a skin-feeling, stain-resistant, and wear-resistant UV topcoat and a preparation method thereof. Background Art

[0002] Various types of panels are used in building interiors, furniture and other industries. People have increasingly rich demands for surfaces that can be touched by their hands and seen directly by their eyes, and at the same time, the requirements are also getting higher and higher. As a result, various types of finishing processing on the surface of panels have also undergone various expansions, resulting in various finishing materials and finishing processing technologies.

[0003] Paint finishing occupies a large part of finishing processing. As an environmentally friendly manufacturing process in the 21st century, UV finishing technology in paint finishing has been increasingly applied and developed in the field of finishing processing. Through the formulation of formulas and the improvement of processing technology, various finishing products with excellent performance such as high gloss, matte, wear resistance, stain resistance, skin feel, etc. can be made according to consumer needs.

[0004] Skin-feel, matte, stain-resistant and wear-resistant are also several finishing effects that have received good responses in the market in recent years. The industry has also developed various UV topcoats with excellent performance. To achieve matte and skin-feel effects, the conventional practice is to add matting powder to the formula, which can make the finish have a smooth skin-feel effect and the glossiness reach below 30°; to achieve stain-resistant effects, fluorine-silicon modified resins are usually added.

[0005] The matting effect of matting powder and the anti-fouling effect of fluorosilicone resin are both achieved by floating on the surface of the topcoat. There is a competitive relationship between anti-fouling and matte. When fluorosilicone resin is added to UV topcoat, while the surface maintains a relatively good anti-fouling effect, the gloss of the UV topcoat will be relatively high, making it difficult to achieve a high matte finish. The UV topcoat made by adding inorganic matting powder has a high matte finish, but the inorganic matting powder has a relatively obvious thickening effect, and the viscosity of the topcoat will become very large, which is not conducive to leveling during coating. In order to maintain the low viscosity of the UV topcoat, the main resin will be replaced with a small molecule resin with lower viscosity or the amount of the main resin will be reduced and the amount of monomer will be increased, which will lead to a decrease in the wear resistance of the UV topcoat after molding. The presence of a large amount of matting powder will also cause the anti-fouling effect of the topcoat to become very poor after molding. Summary of the invention

[0006] In view of the above problems, the present invention provides a skin-feeling, stain-resistant and wear-resistant UV topcoat and a preparation method thereof. By designing a UV topcoat formula, the problem of matte powder thickening the UV paint is solved, so as to achieve the effect of smooth skin feel and high matte finish, and improve the stain resistance and wear resistance of the high matte UV topcoat.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A skin-feel, stain-resistant, and wear-resistant UV topcoat, comprising the following components, and the mass ratios of the components are as follows:

[0009]

[0010] The UV light-curable main resin is polyurethane-modified acrylate;

[0011] The UV light curing diluent monomer is an ester type cross-linking monomer;

[0012] The UV light-curable functional resin is a fluorosilicone curable resin;

[0013] The organic matte powder is a thermosetting polymethyl urea polymer (PMU).

[0014] Furthermore, the mass ratio of the photoinitiator is 2%-3%, and the mass ratio of the UV light curing dilution monomer is 30%-45%.

[0015] Furthermore, the UV light-curing main resin of the present invention is selected from any one or more of the aliphatic polyurethane modified acrylates CN9013NS and CN9110NS of Sartomer Guangzhou Chemical Company, FSP8300 and LuCure8531 of Runao Chemical.

[0016] Furthermore, the UV light-curing diluent monomer of the present invention is selected from any one or more of trimethylolpropane triacrylate (TMPTA), tripropylene glycol diacrylate (TPGDA), 1,6-hexanediol diacrylate (EM221TF HDDA), and dipropylene glycol diacrylate (EM222TF DPGDA) and mixed; specifically, trimethylolpropane triacrylate (TMPTA) and tripropylene glycol diacrylate (TPGDA) of Shanghai Yinchang New Materials, and 1,6-hexanediol diacrylate (EM221TF HDDA) and dipropylene glycol diacrylate (EM222TF DPGDA) of Changxing Chemical are selected.

[0017] Furthermore, the UV light-curable functional resin of the present invention is fluorosilicone polyurethane acrylate or fluorine-containing stain-resistant resin HY-R7935; specifically, the fluorosilicone polyurethane acrylate LuCure8696 of Runao Chemical or the fluorine-containing stain-resistant resin HY-R7935 of Shanghai Huiyan New Materials is selected.

[0018] Furthermore, the photoinitiator of the present invention is selected from any one or more of 2-hydroxy-2-methyl-1-phenylpropanone (1173), 1-hydroxycyclohexyl phenyl ketone (184), and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO), and specifically selected from the photoinitiator of IGM.

[0019] Furthermore, the organic matte powder of the present invention is a mixture of two kinds of Albemarle M-4 (particle size 5-7 μm) and M-6 (≤3.5 μm) in any proportion.

[0020] Furthermore, the leveling agent of the present invention is polyether-modified silicone, specifically BYK-333 from BYK Chemical.

[0021] The preparation method of the skin-feeling, stain-resistant, and wear-resistant UV topcoat of the present invention comprises the following steps:

[0022] (1) Adding UV light-curing resin and UV light-curing functional resin to UV light-curing diluent monomer, stirring at a dispersing disk speed of 1500 r / min until uniform to obtain colloid A;

[0023] (2) adding a photoinitiator and a leveling agent to the colloid A obtained in the above step (1), stirring at a speed of 1000 r / min until uniform to obtain colloid B, adding an organic matte powder after mixing uniformly, stirring at a speed of 800 r / min for 20-30 minutes to obtain colloid C;

[0024] (3) After standing for two hours to defoam, filter the colloid C with a 10 μm filter screen or filter bag to obtain a finished skin-feeling, stain-resistant, and wear-resistant UV topcoat.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) Choosing polyurethane-modified acrylate as the main resin can improve the toughness of the paint film after the UV topcoat is dried and formed, prevent edge collapse during coating of the veneer large board, and avoid cracking during weather resistance testing. It can also improve the feel of the paint film surface;

[0027] (2) After the addition of fluorosilicone photocurable resin, the stain resistance of the surface after the UV topcoat is dried and formed is improved;

[0028] (3) The organic matte powder component is a thermosetting polymethyl urea polymer (PMU), which is a spherical substance that can improve the surface feel of the paint film. It has no thickening effect on the UV topcoat system and is convenient for adjusting the topcoat formula. The molecule contains reactive hydroxymethyl groups, which participate in cross-linking and have good wear resistance after molding.

[0029] (4) BYK-333 is used as a leveling agent and can also prevent defects such as shrinkage craters and orange peel during the coating process;

[0030] (5) The present invention uses a combination of polyurethane modified acrylate + specific organic matte powder + specific fluorosilicone resin. The organic matte powder participates in the cross-linking reaction of chain formation during the light curing stage, and changes from conventional physical bonding to chemical bonding, which will not increase the viscosity of the topcoat. The main resin can use polyurethane modified acrylate with higher viscosity, and the UV topcoat can maintain good wear resistance while achieving high matte. At the same time, the organic matte powder is chemically bonded to the chain, reducing its competition with the fluorosilicone resin, ensuring that the anti-fouling performance of the UV topcoat will not decrease when a high proportion of addition is added. When the amount of organic matte powder is too high, it will cause the UV topcoat to become a porridge-like viscous substance, which is not conducive to use; when the amount is too low, it will cause the UV topcoat to have insufficient matte after molding.

[0031] The present invention obtains a UV topcoat with excellent performance by changing the UV curing main resin in the topcoat formula, replacing the conventional matte powder with organic matte powder, and adding fluorosilicone UV resin with excellent stain resistance. While maintaining the matte finish and hand feel, the stain resistance, scratch resistance and wear resistance of the paint film are also greatly improved. DETAILED DESCRIPTION

[0032] The topcoat and preparation method of the present invention are described in more detail below by way of examples. These examples are given in an illustrative manner, and their purpose is to enable people familiar with the art to understand the content of the present invention and implement it accordingly, but these examples do not limit the scope of the present invention. Any equivalent changes or modifications made according to the spirit and essence of the present invention should be included in the protection scope of the present invention.

[0033] Embodiment 1:

[0034] A skin-feel, stain-resistant, and wear-resistant UV topcoat, comprising the following components, with the mass fractions of each component being as follows:

[0035]

[0036] The preparation process of the UV topcoat comprises: adding CN9013NS, CN9110NS and HY-R7935 to HDDA and TMPTA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) to start the rotation speed at 1500r / min, and stirring for 1 hour; then adding 184, TPO and BYK-333, starting the rotation speed at 1000r / min, and stirring for 30 minutes; adding M-4 and M-6, rotating at 800r / min, and stirring for 20 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining the UV topcoat of Example 1.

[0037] Embodiment 2:

[0038] A skin-feel, stain-resistant, and wear-resistant UV topcoat, comprising the following components, with the mass fractions of each component being as follows:

[0039]

[0040] The preparation process of the UV topcoat comprises: adding LuCure8531, FSP8300 and LuCure8696 to HDDA, DPGDA and TPGDA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) at a speed of 1500 r / min, and stirring for 1.5 hours; then adding 1173, 184, TPO and BYK-333, turning on the speed of 1000 r / min, and stirring for 20 minutes; adding M-4 and M-6, rotating at a speed of 800 r / min, and stirring for 25 minutes; standing for two hours to defoam, filtering with a 10 μm filter bag, and obtaining the UV topcoat of Example 2.

[0041] Embodiment 3:

[0042] A skin-feel, stain-resistant, and wear-resistant UV topcoat, comprising the following components, with the mass fractions of each component being as follows:

[0043]

[0044]

[0045] The preparation process of the UV topcoat comprises: adding CN9013NS and HY-R7935 to HDDA and TMPTA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) to start the rotation speed at 1500r / min, and stirring for 1 hour; then adding 184, TPO, and BYK-333, starting the rotation speed at 1000r / min, and stirring for 30 minutes; adding M-4 and M-6, rotating at 800r / min, and stirring for 20 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining the UV topcoat of Example 3.

[0046] Embodiment 4:

[0047] A skin-feel, stain-resistant, and wear-resistant UV topcoat, comprising the following components, with the mass fractions of each component being as follows:

[0048]

[0049] The preparation process of the UV topcoat comprises: adding CN9013NS, CN9110NS and HY-R7935 to HDDA and TMPTA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) to start the rotation speed at 1500r / min, and stirring for 1 hour; then adding 184, TPO and BYK-333, starting the rotation speed at 1000r / min, and stirring for 30 minutes; adding M-4 and M-6, rotating at 800r / min, and stirring for 20 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining the UV topcoat of Example 4.

[0050] Embodiment 5:

[0051] A skin-feel, stain-resistant, and wear-resistant UV topcoat, comprising the following components, with the mass fractions of each component being as follows:

[0052]

[0053]

[0054] The preparation process of the UV topcoat comprises: adding LuCure8531, FSP8300 and LuCure8696 to HDDA, DPGDA and TPGDA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) to start the rotation speed at 1500r / min, and stirring for 1.5 hours; then adding 1173, 184, TPO and BYK-333, starting the rotation speed at 1000r / min, and stirring for 20 minutes; adding M-4 and M-6, rotating at 800r / min, and stirring for 25 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining the UV topcoat of Example 5.

[0055] Comparison sample 1:

[0056] A conventional matte UV topcoat comprises the following components, and the mass fractions of each component are as follows:

[0057]

[0058] The preparation process of the UV topcoat includes: adding LuCure8531, FSP8300, and LuCure8696 to HDDA, DPGDA, and TPGDA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) to start the rotation speed at 1500r / min, and stirring for 1.5 hours; then adding 1173, 184, TPO, and BYK-333, starting the rotation speed at 1000r / min, and stirring for 20 minutes; adding inorganic matting powder, rotating speed at 800r / min, and stirring for 25 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining a comparative example 1 UV topcoat.

[0059] Comparison sample 2:

[0060] A conventional stain-resistant UV topcoat comprises the following components, and the mass fractions of each component are as follows:

[0061]

[0062] The preparation process of the UV topcoat includes: adding CN9013NS, CN9110NS, and HY-R7935 to HDDA and TMPTA, using a high-speed disperser (BGD 740 / 1 of Guangzhou BGD) at a speed of 1500r / min, and stirring for 1 hour; then adding 184, TPO, and BYK-333, turning on the speed of 1000r / min, and stirring for 30 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining comparative example 2 UV topcoat. Comparative sample 3:

[0063] A conventional UV topcoat comprises the following components, and the mass fractions of each component are as follows:

[0064]

[0065] The preparation process of the UV topcoat includes: adding bisphenol A epoxy acrylate and HY-R7935 to HDDA and TMPTA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) to start the rotation speed at 1500r / min, and stirring for 1 hour; then adding 184, TPO, BYK-333, starting the rotation speed at 1000r / min, and stirring for 30 minutes; adding M-4 and M-6, rotating at 800r / min, and stirring for 20 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining comparative example 3 UV topcoat.

[0066] Comparison sample 4:

[0067] A conventional UV topcoat comprises the following components, and the mass fractions of each component are as follows:

[0068]

[0069] The preparation process of the UV topcoat comprises: adding CN9013NS and CN9110NS to HDDA and TMPTA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) at a speed of 1500r / min, and stirring for 1 hour; then adding 184, TPO, and BYK-333, turning on the speed of 1000r / min, and stirring for 30 minutes; adding M-4 and M-6, rotating at a speed of 800r / min, and stirring for 20 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining comparative example 4 UV topcoat.

[0070] Comparison sample 5:

[0071] A conventional UV topcoat comprises the following components, and the mass fractions of each component are as follows:

[0072]

[0073] The preparation process of the UV topcoat includes: adding bisphenol A epoxy acrylate and HY-R7935 to HDDA and TMPTA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) to start the rotation speed at 1500r / min, and stirring for 1 hour; then adding 184, TPO, BYK-333, starting the rotation speed at 1000r / min, and stirring for 30 minutes; adding inorganic matting powder, rotating speed at 800r / min, and stirring for 20 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining a comparative example 5 UV topcoat.

[0074] Comparison sample 6:

[0075] A conventional UV topcoat comprises the following components, and the mass fractions of each component are as follows:

[0076]

[0077] The preparation process of the UV topcoat comprises: adding CN9013NS, CN9110NS and HY-R7935 to HDDA and TMPTA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) to start the rotation speed at 1500r / min, and stirring for 1 hour; then adding 184, TPO and BYK-333, starting the rotation speed at 1000r / min, and stirring for 30 minutes; adding M-4 and M-6, rotating at 800r / min, and stirring for 20 minutes; standing for two hours to defoam, filtering with a 10μm filter bag, and obtaining a comparative example 6 UV topcoat.

[0078] Comparison sample 7:

[0079] A conventional UV topcoat comprises the following components, and the mass fractions of each component are as follows:

[0080]

[0081]

[0082] The preparation process of the UV topcoat comprises: adding CN9013NS, CN9110NS and HY-R7935 to HDDA, using a high-speed disperser (BGD 740 / 1 of Guangzhou Biaogeda) at a speed of 1500 r / min, and stirring for 1 hour; then adding 184, TPO and BYK-333, turning on the speed of 1000 r / min, and stirring for 30 minutes; adding M-4 and M-6, rotating at a speed of 800 r / min, and stirring for 20 minutes; standing for two hours to defoam, filtering with a 10 μm filter bag, and obtaining a comparative example 7 UV topcoat.

[0083] Performance Testing

[0084] Finish preparation: The above 12 samples were coated on the eco-board with a 5μm wire rod and cured with a handheld UV curing lamp to obtain 12 decorative panels. The performance was tested and the results are shown in Table 1. The wear test grading standard in Table 1 is: 1-no whitening of the paint film, 2-slight whitening of the paint film locally, 3-obvious whitening of the paint film locally, and 4-serious whitening of the paint film.

[0085] Table 1 Test results of plate properties using topcoats of various embodiments and comparative examples

[0086]

[0087] From the data in Table 1, it can be found that compared with the embodiment, after the organic matt powder in comparison sample 1 is replaced by inorganic matt powder, the wear resistance and stain resistance are significantly reduced; in comparison sample 2, the organic matt powder is removed, the glossiness increases significantly, and the matte effect becomes worse; in comparison sample 3, the main resin is replaced by conventional resin, and the glossiness increases while the wear resistance decreases significantly; in comparison sample 4, after the UV light-curing functional resin is lacking, the stain resistance decreases significantly; in comparison sample 5, conventional main resin and conventional matt powder are selected, and the wear resistance decreases significantly; in comparison sample 6, when the amount of organic matt powder used is too low, the glossiness increases significantly and the matte effect is insufficient; in comparison sample 7, the amount of organic matt powder used is too high, the UV paint is unevenly mixed, the organic matt powder is difficult to be completely dispersed, and the UV paint cannot be coated and used.

Claims

1. A skin-feeling, stain-resistant, and wear-resistant UV topcoat, characterized in that: It is composed of the following components, and the mass percentage of each component is as follows: UV light curing main resin 25%-45%, UV light curing dilution monomer 15%-50%, UV light curing functional resin 5%-25%, Photoinitiator 2%-8%, Organic matte powder 8%-15%, Leveling agent 0.1%-0.5%; The sum of the mass percentages of each component is 100%; The UV light-curable main resin is polyurethane-modified acrylate; the UV light-curable main resin is selected from any one or more of the aliphatic polyurethane-modified acrylate CN9013NS, CN9110NS of Sartomer Guangzhou Chemical Company, FSP8300 and LuCure8531 of Runao Chemical; The UV light-curing diluent monomer is an ester-type cross-linking monomer; the UV light-curing diluent monomer is selected from a mixture of any one or more of trimethylolpropane triacrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, and dipropylene glycol diacrylate; The UV light-curable functional resin is fluorosilicone polyurethane acrylate or fluorine-containing stain-resistant resin HY-R7935; The organic matte powder is a thermosetting polymethylurea polymer; the organic matte powder is a mixture of two kinds of Albemarle M-4 with a particle size of 5-7 μm and M-6 with a particle size of ≤3.5 μm in any proportion.

2. The skin-feeling, stain-resistant, and wear-resistant UV topcoat according to claim 1, characterized in that: The mass percentage of the photoinitiator is 2%-3%, and the mass percentage of the UV light curing dilution monomer is 30%-45%.

3. A skin-feel, stain-resistant, and wear-resistant UV topcoat according to claim 1 or 2, characterized in that: The photoinitiator is selected from any one or more of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

4. A skin-feel, stain-resistant, and wear-resistant UV topcoat according to claim 1 or 2, characterized in that: The leveling agent is polyether modified silicone.

5. The skin-feeling, stain-resistant, and wear-resistant UV topcoat according to claim 4, characterized in that: The leveling agent is BYK-333 produced by BYK Chemical.

6. The method for preparing a skin-feeling, stain-resistant, and wear-resistant UV topcoat according to any one of claims 1 to 5, characterized in that: The steps include: (1) Add UV light-curing resin and UV light-curing functional resin to UV light-curing diluent monomer, and stir at a dispersing disk speed of 1500 r / min until uniform to obtain colloid A; (2) Add a photoinitiator and a leveling agent to the colloid A obtained in the above step (1), stir at a speed of 1000 r / min until uniform to obtain colloid B, add organic matte powder after mixing uniformly, stir at a speed of 800 r / min for 20-30 minutes to obtain colloid C; (3) After standing for two hours to defoam, filter colloid C with a 10 μm filter screen or filter bag to obtain a finished skin-feeling, stain-resistant, and wear-resistant UV topcoat.

Citation Information

Cited By

  • High-stain-resistance skin feeling plate and manufacturing method thereof

    CN118060155A

  • A highly stain-resistant, skin-feeling board and its manufacturing method

    CN118060155B