A high-fluidity ultra-high performance concrete and preparation method thereof
By using modified silica nano-microspheres and sodium gluconate with hollow porous structures in ultra-high performance concrete, the problems of large viscosity and large shrinkage are solved, the fluidity and mechanical properties are improved, and efficient pumping and Self-healing effect.
Patent Information
- Application Number
- CN202311717761.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-12-13
AI Technical Summary
Ultra-high performance concrete has a high viscosity due to low water-gluing ratio, which increases the difficulty of pumping. The large amount of gelling material leads to a large shrinkage, which is prone to cracking risks. The existing shrinkage agents and porous aggregates will affect the improvement of mechanical properties. Other performance.
Modified silica nano-microspheres and sodium gluconate with hollow porous structures can reduce the viscosity and surface tension of concrete through synergistic effects, improve fluidity, and reduce shrinkage through the self-healing mechanism of grape ions, enhancing the compactness of the interface transition zone. sex.
It achieves high flowability and low shrinkage of ultra-high performance concrete, while improving its mechanical properties, reducing water demand and viscosity, and enhancing pumping convenience and compressive strength.
Smart Images

Figure CN117623694B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete building materials, and in particular to a high-fluidity ultra-high performance concrete and a preparation method thereof. Background Art
[0002] Ultra-high performance concrete (UHPC) has been widely used in transportation, construction, municipal engineering and other projects due to its ultra-high mechanical properties and ultra-high durability. Compared with ordinary concrete, the low water-cement ratio of UHPC leads to high viscosity of UHPC, which increases the difficulty of pumping; in addition, the large amount of UHPC cementitious materials leads to large shrinkage of UHPC and the risk of cracking. The high viscosity and severe shrinkage limit the scope of application of UHPC. Conventional methods to reduce the shrinkage of UHPC include adding shrinkage reducers, expansion agents, and super absorbent resins. However, shrinkage reducers will reduce the mechanical properties of UHPC to a certain extent; expansion agents are difficult to continue to play a role under the condition of low water-cement ratio of UHPC when there is a lack of internal water in the late hydration period; super absorbent resins will also affect the mechanical properties of UHPC and are difficult to disperse evenly inside UHPC. Currently, more and more researchers have achieved the reduction of UHPC shrinkage through porous aggregates. However, porous aggregates such as ceramics have limited water retention. In addition, the mechanical properties of porous aggregates are lower than those of quartz sand, and the particle size is large, often at the millimeter level. The introduction of porous aggregates will become a weak link in UHPC, significantly reducing the mechanical properties of UHPC. Summary of the invention
[0003] The purpose of the present invention is to overcome the deficiencies of the prior art. The present invention provides a highly fluid ultra-high performance concrete with high fluidity, low viscosity, small shrinkage and excellent mechanical properties.
[0004] The present invention also provides a method for preparing ultra-high performance concrete, which has simple preparation steps and can produce ultra-high performance concrete with high fluidity and excellent mechanical properties.
[0005] In order to solve the above problems, the present invention proposes a highly fluid ultra-high performance concrete, comprising the following components in parts by weight:
[0006] 60-85 parts of cement, 20-40 parts of silica fume, 2-15 parts of fly ash, 85-113 parts of quartz machine-made sand, 1-3 parts of steel fiber, 1-4 parts of water reducer, 0.2-0.6 parts of sodium gluconate, 18-26 parts of water and 8-20 parts of modified silica nanospheres;
[0007] The modified silicon dioxide nano-microspheres are hollow and porous structures.
[0008] As an improvement of the above technical solution, the modified silica nanoparticles are made from the following raw materials:
[0009]
[0010] As an improvement of the above technical solution, the modified silica nanospheres are prepared by the following method:
[0011] S1, mixing 0.2-1.0 parts by weight of a cationic surfactant, 1-3 parts by volume of aqueous ammonia, 100-200 parts by volume of deionized water and 200-400 parts by volume of ethanol, and heating to 45-50° C. and stirring well to obtain a first mixture;
[0012] S2, adding 4-10 parts by volume of alkyl orthosilicate dropwise to the first mixture, stirring continuously, and filtering to obtain a second mixture;
[0013] S3, placing the second mixture in a high pressure reactor, heating to 145-160° C. for reaction for 35-45 hours, and then washing the precipitate;
[0014] S4, extracting the precipitate to remove the cationic surfactant, and obtaining modified silica nanoparticles with a hollow porous structure.
[0015] As an improvement of the above technical solution, the raw materials of the modified silicon dioxide nano-microspheres further include: 8-15 parts by weight of sodium gluconate, 5-10 parts by volume of a silane coupling agent and 80-200 parts by volume of ethanol.
[0016] As an improvement of the above technical solution, the method for preparing the modified silica nanospheres further comprises the following steps:
[0017] S5, mixing 15-30 parts by weight of the modified silica nanospheres, 80-200 parts by volume of ethanol, 5-10 parts by volume of a silane coupling agent and 8-15 parts by weight of sodium gluconate, stirring continuously at room temperature, filtering and drying to obtain the modified silica nanospheres with sodium gluconate grafted on the inner and outer walls.
[0018] As an improvement of the above technical solution, the particle size of the modified silica nanoparticles is less than 500 nm and the specific surface area is greater than 5.6×10 3 m 2 / kg.
[0019] As an improvement of the above technical solution, the fly ash is fly ash microbeads, the particle size of which is less than 20 μm, the SiO2 content is greater than 60%, and the specific surface area is greater than or equal to 1500 m 2 / kg;
[0020] The particle size of the silica fume is less than 10 μm, the SiO2 content is greater than 95%, and the specific surface area is greater than or equal to 1.5×103 m 2 / kg;
[0021] The steel fiber has a length of 13-20 mm, a diameter of 0.18-0.22 mm, and a tensile strength of 2500-3000 MPa;
[0022] The particle size of the quartz machine-made sand is less than 2.36 mm.
[0023] As an improvement of the above technical solution, the steel fiber is copper-plated steel fiber.
[0024] As an improvement of the above technical solution, the water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 40% and a water reducing rate greater than 25%.
[0025] Accordingly, the present invention also provides a method for preparing the ultra-high performance concrete as described above, comprising the following steps:
[0026] Step 1: Filling the modified silica nanospheres with free water by vacuuming;
[0027] Step 2, cement, silica fume, fly ash, quartz machine-made sand, steel fiber, sodium gluconate, and modified silica nanospheres are weighed according to a predetermined mix ratio, mixed, and stirred to obtain a premix;
[0028] Step 3, mixing the water reducing agent and water according to a predetermined water-binder ratio and slowly adding the premix to the mixture and stirring evenly to obtain a premixed slurry;
[0029] Step 4: adding steel fiber to the premixed slurry and stirring evenly to obtain the ultra-high performance concrete.
[0030] The implementation of the present invention has the following beneficial effects:
[0031] Compared with the prior art, the present invention uses cement, silica fume, fly ash, quartz machine-made sand and steel fiber as the main materials, adds modified silica nano-microspheres and sodium gluconate with a hollow porous structure, and reduces the viscosity and surface tension of ultra-high performance concrete through the synergistic effect of the above two substances, thereby improving the fluidity of the concrete slurry and making it easy to pump. When microcracks are generated, the gluconate ions can enrich calcium ions with the diffusion of free water in the cracks, promote the generation of substances such as calcium hydroxide, calcium carbonate, and calcium silicate, and self-repair microcracks. In addition, the modified silica nano-microspheres have a ball rolling effect, which can reduce the water demand of ultra-high performance concrete, and can improve the compactness of the interface transition zone and improve the mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a SEM display of the modified silica nanospheres of the present invention;
[0033] Figure 2 This is a TEM (0.2 μm) display of the modified silica nanospheres of the present invention;
[0034] Figure 3 This is a TEM (100 nm) display of the modified silica nanospheres of the present invention. DETAILED DESCRIPTION
[0035] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.
[0036] The present invention provides a highly fluid ultra-high performance concrete, comprising the following components in parts by weight:
[0037] 60-85 parts of cement, 20-40 parts of silica fume, 2-15 parts of fly ash, 85-113 parts of quartz machine-made sand, 1-3 parts of steel fiber, 1-4 parts of water reducer, 0.2-0.6 parts of sodium gluconate, 18-26 parts of water and 8-20 parts of modified silica nanospheres;
[0038] The modified silicon dioxide nano-microspheres are hollow and porous structures.
[0039] The present invention uses cement, silica fume, fly ash, quartz machine-made sand and steel fiber as main materials, adds modified silicon dioxide nano-microspheres and sodium gluconate with hollow porous structure, and reduces the viscosity and surface tension of ultra-high performance concrete through the synergistic effect of the above two substances, thereby improving the fluidity of concrete slurry and making it easy to pump. When microcracks are generated, gluconate ions can enrich calcium ions with the diffusion of free water in the cracks, promote the generation of substances such as calcium hydroxide, calcium carbonate, calcium silicate, and self-repair microcracks. In addition, the modified silicon dioxide nano-microspheres have the effect of rolling balls, which can reduce the water demand of ultra-high performance concrete, and can improve the compactness of the interface transition zone and improve the mechanical properties.
[0040] It should be noted that the water reducing agent is a common water reducing agent available in the market. Preferably, the water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 40% and a water reducing rate greater than 25%.
[0041] Preferably, the modified silica nanospheres are made from the following raw materials:
[0042]
[0043]
[0044] It should be noted that the corresponding relationship between the above parts by weight and parts by volume is g / ml.
[0045] The cationic surfactant is a template for preparing silicon dioxide nanospheres; preferably, the cationic surfactant is CTAB, i.e., hexadecyltrimethylammonium bromide.
[0046] The alkyl orthosilicate is at least one selected from ethyl orthosilicate and methyl orthosilicate; preferably, the alkyl orthosilicate is liquid TEOS, that is, ethyl orthosilicate.
[0047] Preferably, the modified silica nanospheres are prepared by the following method:
[0048] S1, mixing 0.2-1.0 parts by weight of a cationic surfactant, 1-3 parts by volume of aqueous ammonia, 100-200 parts by volume of deionized water and 200-400 parts by volume of ethanol, and heating to 45-50° C. and stirring well to obtain a first mixture;
[0049] S2, adding 4-10 parts by volume of alkyl orthosilicate dropwise to the first mixture, stirring continuously for 2-6 hours, and filtering to obtain a second mixture;
[0050] S3, placing the second mixture in a high pressure reactor, heating to 145-160° C. for reaction for 35-45 hours, and then washing the precipitate;
[0051] S4, extracting the precipitate to remove the cationic surfactant, and obtaining modified silica nanoparticles with a hollow porous structure.
[0052] Preferably, the pressure of the high-pressure reactor can be set to 50-150 MPa, and can be adjusted according to the actual situation of the product.
[0053] like Figure 1-3 As shown, the modified silica nanospheres of the present invention are hollow porous structures with a "ball-shaped" effect, which can reduce the water demand of UHPC and further improve the fluidity of ultra-high performance concrete. In addition, the water carrying capacity is large, and the saturated water absorption rate can exceed 80%. During the hydration process of UHPC, the internal dryness reaches a certain degree. Under the action of the capillaries, the free water inside the modified silica nanospheres continues to diffuse to the outside, and continues to replenish the water required for the hydration of the cementitious material, which significantly reduces the capillary pressure and reduces shrinkage. Figure 1 The SEM shows the silica nanospheres. Figure 2 TEM shows that the nanospheres have a hollow surface porous structure. Figure 3 TEM showed that the wall thickness of the hollow porous silica nanospheres was about 20 nm, the diameter was about less than 500 nm, and the surface was porous.
[0054] More preferably, the raw materials of the modified silica nanospheres further include: 8-15 parts by weight of sodium gluconate, 5-10 parts by volume of a silane coupling agent and 80-200 parts by volume of ethanol.
[0055] Accordingly, the method for preparing the modified silica nanospheres further comprises the following steps:
[0056] S5. Mix 15-30 parts by weight of the modified silica nanospheres, 80-200 parts by volume of ethanol, 5-10 parts by volume of a silane coupling agent and 8-15 parts by weight of sodium gluconate, stir continuously at room temperature of 25° C. for 24 hours or more, filter and dry to obtain the modified silica nanospheres with sodium gluconate grafted on the inner and outer walls.
[0057] It should be noted that the silane coupling agent in step S5 is a common type on the market, and preferably, the silane coupling agent is KH570.
[0058] On the basis of the modified silica nanospheres with hollow porous structure prepared in S1-S4, ethanol, silane coupling agent and sodium gluconate are used for grafting reaction, so that the inner wall and outer wall of the modified silica nanospheres are grafted with sodium gluconate, so that the surface tension of the paste can be reduced, and it has potential activity, and can undergo secondary hydration reaction with cement, so as to ensure the continuity of the internal structure of ultra-high performance concrete, improve the compactness of the interface transition zone and improve the mechanical properties. In addition, the internally grafted sodium gluconate can enrich calcium ions, and react with the wall material under the action of free water to generate cementitious components such as calcium silicate and calcium hydroxide, which fill the hollow structure of the nanospheres, eliminating the problem of reduced mechanical properties in this area due to the introduction of porous aggregates such as modified hollow porous silica nanospheres.
[0059] Preferably, the particle size of the modified silica nanospheres is less than 500 nm and the specific surface area is greater than 5.6×10 3 m 2 / kg.
[0060] It should be noted that the fly ash is preferably fly ash microspheres, with a particle size of less than 20 μm, a SiO2 content of more than 60%, and a specific surface area of greater than or equal to 1500 m 2 / kg. The fly ash mentioned above has the mechanical property of improving the compressive strength of ultra-high performance concrete.
[0061] Preferably, the particle size of the silica fume is less than 10 μm, the SiO2 content is greater than 95%, and the specific surface area is greater than or equal to 1.5×10 3 m 2 / kg.
[0062] Preferably, the steel fiber has a length of 13-20 mm, a diameter of 0.18-0.22 mm, and a tensile strength of 2500-3000 MPa. The copper-plated steel fiber can enhance the strength of concrete. Its cross section is circular, and it is useful in transmitting and distributing stress in concrete, so that cracks are resolved into scattered micro cracks. More preferably, the steel fiber is a copper-plated steel fiber.
[0063] Preferably, the particle size of the quartz machine-made sand is less than 2.36 mm.
[0064] The present invention also provides a method for preparing the ultra-high performance concrete, comprising the following steps:
[0065] Step 1: Filling the modified silica nanospheres with free water by vacuuming;
[0066] Step 2, cement, silica fume, fly ash, quartz machine-made sand, steel fiber, sodium gluconate, and modified silica nanospheres are weighed according to a predetermined mix ratio, mixed, and slowly stirred for 1-4 minutes to obtain a premix;
[0067] Step 3, mixing the polycarboxylate water-reducing agent and water according to a predetermined water-binder ratio and slowly adding the premix to the premix and stirring slowly for 2-5 minutes to obtain a premixed slurry;
[0068] Step 4: adding steel fiber to the premixed slurry and rapidly stirring for 3-8 minutes to obtain the ultra-high performance concrete.
[0069] The present invention is further described below with specific embodiments:
[0070] Example 1
[0071] This embodiment provides a highly fluid ultra-high performance concrete, which includes the following components in parts by weight:
[0072] 70 parts of cement, 20 parts of silica fume, 10 parts of fly ash, 100 parts of quartz machine-made sand, 1.5 parts of steel fiber, 2 parts of polycarboxylic acid water reducer, 0.5 parts of sodium gluconate, 22 parts of water and 10 parts of modified silica nanospheres. The modified silica nanospheres are hollow and porous.
[0073] Wherein, the modified silica nanospheres are prepared by the following method:
[0074] S1, 0.4 g of CTAB, 3 ml of ammonia water, 150 ml of deionized water and 300 ml of ethanol were mixed, and the mixture was heated to 50° C. and stirred thoroughly to obtain a first mixture;
[0075] S2, adding 6 ml of TEOS dropwise to the first mixture, stirring for 3 h, and filtering to obtain a second mixture;
[0076] S3, placing the second mixture in a high-pressure reactor, heating to 150° C. at a pressure of 100 MPa for 40 hours, and then washing the precipitate with 500 ml of deionized water and 500 ml of methanol;
[0077] S4, extracting the precipitate for 50 hours to remove CTAB, and obtaining the modified silica nanospheres.
[0078] Example 2
[0079] This embodiment provides a highly fluid ultra-high performance concrete, which includes the following components in parts by weight:
[0080] 60 parts of cement, 25 parts of silica fume, 2 parts of fly ash, 85 parts of quartz machine-made sand, 1 part of steel fiber, 1 part of polycarboxylic acid water reducer, 0.2 parts of sodium gluconate, 18 parts of water and 8 parts of modified silica nanospheres. The modified silica nanospheres are hollow and porous.
[0081] Wherein, the modified silica nanospheres are prepared by the following method:
[0082] S1, 0.2 g of CTAB, 2 ml of ammonia water, 120 ml of deionized water and 200 ml of ethanol were mixed, and heated to 45° C. and stirred thoroughly to obtain a first mixture;
[0083] S2, adding 4 ml of TEOS dropwise to the first mixture, stirring for 2 h, and filtering to obtain a second mixture;
[0084] S3, placing the second mixture in a high-pressure reactor, heating to 145° C. at a pressure of 100 MPa for reaction for 35 hours, and then washing the precipitate with 500 ml of deionized water and 500 ml of methanol;
[0085] S4, extracting the precipitate for 50 hours to remove CTAB, and obtaining the modified silica nanospheres.
[0086] Example 3
[0087] This embodiment provides a highly fluid ultra-high performance concrete, which includes the following components in parts by weight:
[0088] 85 parts of cement, 40 parts of silica fume, 15 parts of fly ash, 113 parts of quartz machine-made sand, 3 parts of steel fiber, 4 parts of polycarboxylic acid water reducer, 0.6 parts of sodium gluconate, 26 parts of water and 20 parts of modified silica nanospheres. The modified silica nanospheres are hollow and porous.
[0089] Wherein, the modified silica nanospheres are prepared by the following method:
[0090] S1, mixing 1.0 g of CTAB, 3 ml of ammonia water, 200 ml of deionized water and 400 ml of ethanol, heating to 50° C. and stirring thoroughly to obtain a first mixture;
[0091] S2, adding 8 ml of TEOS dropwise to the first mixture, stirring for 3 h, and filtering to obtain a second mixture;
[0092] S3, placing the second mixture in a high-pressure reactor, heating to 155° C. at a pressure of 100 MPa for 45 h, and then washing the precipitate with 500 ml of deionized water and 500 ml of methanol;
[0093] S4, extracting the precipitate for 50 hours to remove CTAB, and obtaining the modified silica nanospheres.
[0094] Example 4
[0095] This embodiment provides a highly fluid ultra-high performance concrete, which includes the following components in parts by weight:
[0096] 70 parts of cement, 20 parts of silica fume, 10 parts of fly ash, 100 parts of quartz machine-made sand, 1.5 parts of steel fiber, 2 parts of polycarboxylic acid water reducer, 0.5 parts of sodium gluconate, 22 parts of water and 10 parts of modified silica nanospheres. The modified silica nanospheres are hollow and porous.
[0097] Wherein, the modified silica nanospheres are prepared by the following method:
[0098] S1, 0.4 g of CTAB, 3 ml of ammonia water, 150 ml of deionized water and 300 ml of ethanol were mixed, and the mixture was heated to 50° C. and stirred thoroughly to obtain a first mixture;
[0099] S2, adding 6 ml of TEOS dropwise to the first mixture, stirring for 3 h, and filtering to obtain a second mixture;
[0100] S3, placing the second mixture in a high-pressure reactor, heating to 150° C. at a pressure of 100 MPa for 40 hours, and then washing the precipitate with 500 ml of deionized water and 500 ml of methanol;
[0101] S4, extracting the precipitate for 50 hours to remove CTAB, and obtaining the modified silica nanoparticles;
[0102] S5. Mix 20 g of modified silica nanospheres, 100 ml of ethanol, 10 ml of KH570 and 10 g of sodium gluconate, and stir continuously for 24 h at room temperature of 25° C., then filter and dry at 60° C. to obtain the modified silica nanospheres with sodium gluconate grafted on the inner and outer walls.
[0103] Example 5
[0104] This embodiment provides a highly fluid ultra-high performance concrete, which includes the following components in parts by weight:
[0105] 75 parts of cement, 25 parts of silica fume, 8 parts of fly ash, 110 parts of quartz machine-made sand, 1.5 parts of steel fiber, 2 parts of polycarboxylic acid water reducer, 0.5 parts of sodium gluconate, 22 parts of water and 18 parts of modified silica nanospheres. The modified silica nanospheres are hollow and porous.
[0106] Wherein, the modified silica nanospheres are prepared by the following method:
[0107] S1, 0.4 g of CTAB, 3 ml of ammonia water, 150 ml of deionized water and 300 ml of ethanol were mixed, and the mixture was heated to 50° C. and stirred thoroughly to obtain a first mixture;
[0108] S2, adding 6 ml of TEOS dropwise to the first mixture, stirring for 3 h, and filtering to obtain a second mixture;
[0109] S3, placing the second mixture in a high-pressure reactor, heating to 150° C. at a pressure of 100 MPa for 40 hours, and then washing the precipitate with 500 ml of deionized water and 500 ml of methanol;
[0110] S4, extracting the precipitate for 50 hours to remove CTAB, and obtaining the modified silica nanoparticles;
[0111] S5. Mix 15 g of modified silica nanospheres, 80 ml of ethanol, 5 ml of KH570 and 8 g of sodium gluconate, and stir continuously for 24 h at room temperature of 25 ° C., then filter and dry at 60 ° C. to obtain the modified silica nanospheres with sodium gluconate grafted on the inner and outer walls.
[0112] Example 6
[0113] This embodiment provides a highly fluid ultra-high performance concrete, which includes the following components in parts by weight:
[0114] 80 parts of cement, 30 parts of silica fume, 5 parts of fly ash, 100 parts of quartz machine-made sand, 1.5 parts of steel fiber, 2 parts of polycarboxylic acid water reducer, 0.5 parts of sodium gluconate, 22 parts of water and 15 parts of modified silica nanospheres. The modified silica nanospheres are hollow and porous.
[0115] Wherein, the modified silica nanospheres are prepared by the following method:
[0116] S1, 0.4 g of CTAB, 3 ml of ammonia water, 150 ml of deionized water and 300 ml of ethanol were mixed, and the mixture was heated to 50° C. and stirred thoroughly to obtain a first mixture;
[0117] S2, adding 6 ml of TEOS dropwise to the first mixture, stirring for 3 h, and filtering to obtain a second mixture;
[0118] S3, placing the second mixture in a high-pressure reactor, heating to 150° C. at a pressure of 100 MPa for 40 hours, and then washing the precipitate with 500 ml of deionized water and 500 ml of methanol;
[0119] S4, extracting the precipitate for 50 hours to remove CTAB, and obtaining the modified silica nanoparticles;
[0120] S5. Mix 30 g of modified silica nanospheres, 200 ml of ethanol, 10 ml of KH570 and 15 g of sodium gluconate, and stir continuously for 24 h at room temperature of 25 ° C., then filter and dry at 60 ° C. to obtain the modified silica nanospheres with sodium gluconate grafted on the inner and outer walls.
[0121] Comparative Example 1
[0122] This embodiment provides a highly fluid ultra-high performance concrete, which includes the following components in parts by weight:
[0123] 70 parts of cement, 20 parts of silica fume, 10 parts of fly ash, 100 parts of quartz machine-made sand, 1.5 parts of steel fiber, 2 parts of polycarboxylate water reducer and 22 parts of water.
[0124] Comparative Example 2
[0125] This embodiment provides a highly fluid ultra-high performance concrete, which includes the following components in parts by weight:
[0126] 70 parts of cement, 20 parts of silica fume, 10 parts of fly ash, 100 parts of quartz machine-made sand, 1.5 parts of steel fiber, 2 parts of polycarboxylate water reducer, 0.5 parts of sodium gluconate and 22 parts of water.
[0127] Examples 1-6 are prepared by the following method for preparing ultra-high performance concrete;
[0128] Specifically, the following steps are included:
[0129] Step 1: Filling the modified silica nanospheres with free water by vacuuming;
[0130] Step 2, cement, silica fume, fly ash, quartz machine-made sand, steel fiber, sodium gluconate, and modified silica nanospheres are weighed according to a predetermined mix ratio, mixed, and slowly stirred for 2 minutes to obtain a premix;
[0131] Step 3, mixing the polycarboxylate water-reducing agent and water according to a predetermined water-binder ratio and slowly adding the premix to the premix and stirring slowly for 3 minutes to obtain a premix slurry;
[0132] Step 4: adding steel fiber to the premixed slurry and rapidly stirring for 5 minutes to obtain the ultra-high performance concrete.
[0133] Comparative Example 1 was prepared by the following method for preparing ultra-high performance concrete:
[0134] Specifically, the following steps are included:
[0135] Cement, silica fume, fly ash, quartz machine-made sand and steel fiber are weighed according to a predetermined mix ratio, mixed, and slowly stirred for 2 minutes to obtain a premix; then, polycarboxylate water reducer and water are mixed according to a predetermined water-binder ratio and slowly added to the premix and slowly stirred for 3 minutes to obtain a premixed slurry; finally, steel fiber is added to the premixed slurry and quickly stirred for 5 minutes to obtain ultra-high performance concrete.
[0136] Comparative Example 2 was prepared by the following method for preparing ultra-high performance concrete:
[0137] Specifically, the following steps are included:
[0138] Cement, silica fume, fly ash, quartz machine-made sand, sodium gluconate and steel fiber are weighed according to a predetermined mix ratio, mixed, and slowly stirred for 2 minutes to obtain a premix; then, a polycarboxylate water-reducing agent is mixed with water according to a predetermined water-binder ratio and slowly added to the premix and slowly stirred for 3 minutes to obtain a premixed slurry; finally, steel fiber is added to the premixed slurry and rapidly stirred for 5 minutes to obtain ultra-high performance concrete.
[0139] The ultra-high performance concrete prepared in Examples 1-6 and Comparative Examples 1-2 were tested according to the following test methods.
[0140] The test method for expansion is based on GB / T 2419-2005 "Method for Determination of Fluidity of Cement Mortar"; the dynamic viscosity of UHPC slurry is tested by RST-SST soft solid touch screen rheometer produced by Brookfield, USA, and the slurry is measured by cross shear blade rotors VT40-20 and VT60-30, with a stirring speed of 0.01s -1 , the measurement time is 150s; the mechanical properties test refers to T / CECS 10107-2020 "Ultra-High Performance Concrete (UHPC) Technical Requirements"; the volume stability test refers to GB / T50082-2009 "Standard Test Method for Long-term Performance and Durability of Ordinary Concrete" and ASTMC 1698-09 Standard Test Method for Autogenous Strain of Cement Paste and Mortar. The autogenous shrinkage test adopts the bellows method: first stir the UHPC slurry evenly, and use a vacuum pump to remove the internal bubbles; then inject it into the bellows, seal it with a plug with a test target, and place it on the test bench. Stirring for 30 minutes is required at the beginning of the test. During this period, the same batch of slurry is used to measure the setting time. When processing the data, the length of the bellows at the initial setting of the UHPC slurry is set as the initial length. During the test, the temperature is always maintained at (20±2)℃, and the same sample is tested 3 times and the average is taken.
[0141] The test results are shown in the following table:
[0142]
[0143]
[0144] From the test results of the above-mentioned Examples 1-6 and Comparative Examples 1-2, it can be seen that the ultra-high performance concrete in the embodiments of the present invention can effectively reduce the viscosity of the concrete, and the reduction in viscosity means that the expansion of fluidity is improved. In addition, the compressive strength of the ultra-high performance concrete is improved compared with the prior art. Specifically, compared with Comparative Example 1, the viscosity of the ultra-high performance concrete in Examples 1-6 is reduced by 97.5% at most, and the compressive strength is increased by 58.5% at most.
[0145] In summary, compared with the ultra-high performance concrete in the prior art, the viscosity of Examples 1-6 of the present invention is significantly lower, the fluidity is good, and the compressive strength of the ultra-high performance concrete after drying is higher.
[0146] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. A highly fluid ultra-high performance concrete, characterized in that: The composition comprises the following components in parts by weight: 60-85 parts of cement, 20-40 parts of silica fume, 2-15 parts of fly ash, 85-113 parts of quartz machine-made sand, 1-3 parts of steel fiber, 1-4 parts of water reducer, 0.2-0.6 parts of sodium gluconate, 18-26 parts of water and 8-20 parts of modified silica nanospheres; The modified silicon dioxide nano-microspheres are hollow and porous structures, and sodium gluconate is grafted on the inner wall and the outer wall.
2. The ultra-high performance concrete according to claim 1, characterized in that: The modified silica nanospheres are made from the following raw materials: 0.2-1.0 parts by weight of a cationic surfactant, 1-3 parts by volume of ammonia water, 100-200 parts by volume of deionized water, 280-600 parts by volume of ethanol, 4-10 parts by volume of alkyl orthosilicate, 8-15 parts by weight of sodium gluconate, and 5-10 parts by volume of a silane coupling agent; The corresponding relationship between parts by weight and parts by volume is g / ml.
3. The ultra-high performance concrete according to claim 2, characterized in that: The modified silica nanospheres are prepared by the following method: S1, mixing 0.2-1.0 parts by weight of a cationic surfactant, 1-3 parts by volume of aqueous ammonia, 100-200 parts by volume of deionized water and 200-400 parts by volume of ethanol, and heating to 45-50° C. and stirring well to obtain a first mixture; S2, adding 4-10 parts by volume of alkyl orthosilicate dropwise to the first mixture, stirring continuously, and filtering to obtain a second mixture; S3, placing the second mixture in a high pressure reactor, heating to 145-160° C. for reaction for 35-45 hours, and then washing the precipitate; S4, extracting the precipitate to remove the cationic surfactant to obtain modified silica nanoparticles with a hollow porous structure; S5, mixing 15-30 parts by weight of the modified silica nanospheres, 80-200 parts by volume of ethanol, 5-10 parts by volume of a silane coupling agent and 8-15 parts by weight of sodium gluconate, stirring continuously at room temperature, filtering and drying to obtain the modified silica nanospheres with sodium gluconate grafted on the inner and outer walls.
4. The ultra-high performance concrete according to any one of claims 2 to 3, characterized in that: The particle size of the modified silicon dioxide nanospheres is less than 500 nm, and the specific surface area is greater than 5.6×10 3 m 2 / kg.
5. The ultra-high performance concrete according to claim 4, characterized in that: The fly ash is fly ash microbeads, the particle size of which is less than 20 μm, the SiO2 content is greater than 60%, and the specific surface area is greater than or equal to 1500 m 2 / kg; The particle size of the silica fume is less than 10 μm, the SiO2 content is greater than 95%, and the specific surface area is greater than or equal to 1.5×10 3 m 2 / kg; The steel fiber has a length of 13-20 mm, a diameter of 0.18-0.22 mm, and a tensile strength of 2500-3000 MPa; The particle size of the quartz machine-made sand is less than 2.36 mm.
6. The ultra-high performance concrete according to claim 5, characterized in that: The steel fiber is copper-plated steel fiber.
7. The ultra-high performance concrete according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid water reducing agent with a solid content of 40% and a water reducing rate greater than 25%.
8. The method for preparing ultra-high performance concrete according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1: Filling the modified silica nanospheres with free water by vacuuming; Step 2, cement, silica fume, fly ash, quartz machine-made sand, steel fiber, sodium gluconate, and modified silica nanospheres are weighed according to a predetermined mix ratio, mixed, and stirred to obtain a premix; Step 3, mixing the water reducing agent and water according to a predetermined water-binder ratio and slowly adding the premix to the mixture and stirring evenly to obtain a premixed slurry; Step 4: adding steel fiber to the premixed slurry and stirring evenly to obtain the ultra-high performance concrete.
Citation Information
Patent Citations
Low-viscosity large-flow-state C150 ultra-high-performance concrete
CN112521108A
Water-based permeable inorganic nano waterproof material and preparation method thereof
CN114988746A