A base film for high temperature resistant and aging resistant composite current collector and preparation method thereof

By introducing modified grafted PBT and PEN resins into the PET film, irradiation treatment, combined with trace additives, a high-temperature and aging-resistant PET film was prepared, which solved the problem of easy deformation of the PET film at high temperature, and achieved the The mechanical properties of high strength and high elongation of break reduce the defect rate in composite fluid production.

CN118240250BActive Publication Date: 2024-11-22扬州博恒新能源材料科技有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410460404.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-11-22
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

The PET film used in the existing composite fluids is prone to deform and wrinkle at high temperatures, resulting in low yields in the battery production process and cannot meet the special requirements of the composite fluids industry for organic polymer base films.

Method used

By introducing modified grafted PBT and PEN resins into the PET film, and irradiation treatment is performed at high temperature and combined with trace additives, a high temperature and aging resistance PET film is prepared, avoiding the problem of weak binding force caused by excessive additives. , a stable base film is formed by extrusion and stretching processes.

Benefits of technology

The PET film produced has high strength and high elongation of break at room temperature, and its mechanical properties are maintained well in high temperature environments, reducing base film deformation, low defect rate, and meeting the requirements of the composite fluid collection industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004983856450000081
    Figure GDA0004983856450000081
Patent Text Reader

Abstract

This case involves a base film for high temperature resistant and aging resistant composite current collector and its preparation method. It uses terephthalic acid, calcium dihydroxybenzene sulfonate and butanediol as raw materials, firstly obtains an intermediate product through esterification reaction and polycondensation reaction, and then irradiates and grafts polymethacrylate glycidyl to obtain modified grafted PET on its surface; PEN resin reacts with hexamethylenediamine and then is sent into a mixing bin to mix with PET resin, modified grafted PET, antioxidant and lubricant to obtain a mixture, which is then extruded, biaxially stretched, and pulled and rolled up. The present invention uses low-cost PET resin material as the base material, and combines homemade modified PET and PEN to obtain a high temperature resistant PET film in the presence of trace additives; it has high strength and high elongation at break at room temperature, and has a high retention rate of mechanical properties under high temperature environment. When preparing the composite current collector, the base film is not easy to deform and has a low defect rate, which can meet the special requirements of the composite current collector industry for the base film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite current collectors, in particular to a base film for a high temperature resistant and aging resistant composite current collector and a preparation method thereof. Background Art

[0002] Composite current collectors are new materials with a sandwich structure of metal layer + organic film layer + metal layer formed by depositing a metal layer on the surface of an ultra-thin organic polymer film. They can replace traditional negative metal current collectors and be used in new energy lithium batteries. Composite current collectors have several advantages. The biggest advantage is that the amount of metal materials used is reduced and replaced by some cheap organic films, which has great potential for cost reduction. Secondly, due to the use of organic materials in composite current collectors, the weight of the battery is reduced, the thinning is reduced, and the active materials are increased, thereby effectively increasing the energy density of the battery by 5% to 10%. In addition, the composite current collector can absorb the expansion-contraction stress generated by the pole piece, maintain the long-term integrity of the pole piece interface, and increase the cycle life of the battery by 5%. The application of composite current collector materials can significantly reduce the probability of combustion caused by battery short circuits, and can effectively solve the problem of battery safety.

[0003] The performance of the composite current collector is closely related to the organic polymer film therein. At present, the organic polymer films used in the composite current collector mainly include PP (polypropylene), PET (polyethylene terephthalate), PI (polyimide), etc. Among them, PET film has the lowest price and relatively good adhesion to copper metal, but poor heat resistance. In the preparation process of the composite current collector, metal ions need to be plated on the surface of the film at high temperature and high pressure. However, conventional PET is prone to deformation, wrinkles, warping and other undesirable phenomena when subjected to high temperature, which in turn leads to wrinkles in the process of battery production, resulting in too low a yield. Summary of the invention

[0004] In view of the deficiencies in the prior art, a modification method for a PET film is provided. The prepared PET film has high temperature resistance and aging resistance and can be used as a base film for a composite current collector.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a base film for a high temperature resistant and aging resistant composite current collector comprises the following steps:

[0007] 1) Add terephthalic acid, calcium dihydroxybenzene sulfonate, butanediol and a catalyst into a reactor, control the pressure in the reactor at 0.3 MPa, raise the temperature to 230-250° C. and react for 2-3 hours; reduce the pressure in the reactor to normal pressure, then evacuate and reduce the pressure to below 100 Pa, and raise the temperature to 280° C. and react for 3-5 hours. After the reaction, introduce nitrogen, cool the discharged material with cooling water, and cut into pellets;

[0008] 2) dispersing the pelletized product in acetone for 1 to 2 hours, taking it out and drying it, then placing it in a dichloromethane solution containing glycidyl methacrylate, introducing nitrogen to replace the air in the system, and then placing the mixed system in a radiation field for irradiation under a nitrogen atmosphere; after the irradiation is completed, filtering it with suction, and finally washing and drying it to obtain the modified grafted PBT;

[0009] 3) placing the PEN resin and hexamethylenediamine in a reaction kettle and mixing them for a certain period of time to obtain a pretreated PEN resin;

[0010] 4) sending PET resin, modified grafted PBT, pretreated PEN resin, antioxidant and lubricant into a mixing bin to mix and prepare a mixture;

[0011] 5) The mixed material is fed into an extruder, extruded and formed, then biaxially stretched, and finally pulled and rolled up.

[0012] Furthermore, in the step 1), the molar ratio of terephthalic acid, calcium dihydroxybenzene sulfonate and butanediol is 100:20 to 40:100.

[0013] Furthermore, the catalyst is an antimony-based catalyst with a mass fraction of 200 to 300 mg / kg.

[0014] Furthermore, in the step 2), the mass ratio of the pelletized product to glycidyl methacrylate is 1:0.2-0.5; the irradiation source is a cobalt source, and the irradiation dose is 25 kGy.

[0015] Furthermore, the mass ratio of the PEN resin to hexamethylenediamine is 1:3-5; the treatment temperature is 200° C., and the treatment time is 24 hours.

[0016] Furthermore, the antioxidant is antioxidant 1010 or antioxidant 168; and the lubricant is pentaerythritol stearate.

[0017] Furthermore, the feeding amounts of the PET resin, modified grafted PBT, pretreated PEN resin, antioxidant and lubricant are 70-80 parts, 5-20 parts, 2-10 parts, 0.3-0.5 parts and 0.5-1 parts respectively.

[0018] The present invention further provides a base film for a high temperature resistant and aging resistant composite current collector prepared by the preparation method as described above.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention uses low-cost PET resin material as the base material, and combines homemade modified PET and PEN to prepare a high-temperature resistant PET film in the presence of a trace amount of additives; the modified PET is simple to prepare, and the addition amount is small and combined with a trace amount of additives, there is no need to use a compatibilizer, and the problem of weak base film bonding caused by the addition of too many additives is avoided; the prepared PET film has high strength and high elongation at break at room temperature, and has a high retention rate of mechanical properties under high temperature environment. When preparing the composite current collector, the base film is not easy to deform, and the defective rate is low, which can meet the special requirements of the composite current collector industry for organic polymer base films. DETAILED DESCRIPTION

[0020] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0022] Embodiment: A method for preparing a base film for a high temperature resistant and aging resistant composite current collector comprises the following steps:

[0023] 1) Add 100 mol of terephthalic acid, 20-40 mol of calcium dihydroxybenzene sulfonate, 100 mol of butanediol and 300 mg / kg of antimony trioxide as a catalyst into a reactor, control the pressure in the reactor at 0.3 MPa, raise the temperature to 230-250° C. and react for 2-3 hours; reduce the pressure in the reactor to normal pressure, then evacuate and reduce the pressure to below 100 Pa, and raise the temperature to 280° C. and react for 3-5 hours. After the reaction, introduce nitrogen, cool the discharged material with cooling water, and cut into pellets;

[0024] 2) dispersing the pelletized product in acetone for 1 to 2 hours, taking it out and drying it, then placing it in a dichloromethane solution containing glycidyl methacrylate, introducing nitrogen to replace the air in the system, and then placing the mixed system in a radiation field under a nitrogen atmosphere for irradiation (cobalt source, irradiation dose of 25 kGy); after the irradiation is completed, filtering it with suction, and finally washing and drying it to obtain the modified grafted PBT;

[0025] 3) placing the PEN resin and hexamethylenediamine in a reaction kettle and mixing them for a certain period of time to obtain a pretreated PEN resin;

[0026] 4) sending PET resin, modified grafted PBT, pretreated PEN resin, antioxidant and lubricant into a mixing bin to mix and prepare a mixture;

[0027] 5) The mixed material is fed into an extruder, and the extrusion temperature is set at 270-290° C., and the temperature of the cooling roller is set at 15° C. to extrude a cast sheet; the composite cast sheet is first longitudinally stretched 3.5 times at 90-120° C. and then cooled to 50° C., and then transversely stretched 3 times at 110-120° C., and finally pulled and rolled.

[0028] The mixture for preparing the composite current collector base film in this application includes PET resin, modified grafted PBT, pretreated PEN resin, antioxidant and lubricant; among them, PET resin is inexpensive and is one of the commonly used materials for preparing the composite current collector base film, and the modified grafted PBT is a third monomer calcium dihydroxybenzene sulfonate introduced in the conventional PBT preparation process, which can effectively improve the rigidity of the material and improve the heat resistance of the material; then, the polymethacrylate glycidyl polymer chain is introduced on its surface through the irradiation grafting reaction to improve the rigidity of the material and improve the toughness of the material. Since the molecular chain of the modified grafted PBT is still mainly composed of polyethylene terephthalate and ethylene glycol, it has good compatibility with PET resin and reduces the repulsive force between molecular chains. PEN is polyethylene 2,6-naphthalate, which is similar to PET in structure, but its mechanical properties and heat resistance are better than PET. PEN is expensive and not suitable for large-scale applications, but adding a small amount of PEN to PET can also enhance the mechanical properties and heat resistance of the material. The present application introduces amino groups on the surface of PEN by pre-reacting PEN with hexamethylenediamine at high temperature, and then mixes it with PET resin and modified grafted PBT. During the melt extrusion process, the surface amino groups and epoxy groups open the ring to form a cross-linked network structure, which can effectively improve the stability and aging resistance of the final base film.

[0029] Unless otherwise specified, the raw materials and reaction methods used in the examples of the present invention are all common raw materials on the market and conventional technical methods well known to those skilled in the art; with reference to the above preparation process, the following specific examples can be obtained. Among them, the PET and PEN used directly in the examples of the present invention were purchased from BASF.

[0030] Embodiment 1:

[0031] 1) Add 100 mol of terephthalic acid, 20 mol of calcium dihydroxybenzene sulfonate, 100 mol of butanediol and 300 mg / kg of antimony trioxide as a catalyst into a reactor, control the pressure in the reactor at 0.3 MPa, raise the temperature to 230-250° C. and react for 2-3 hours; reduce the pressure in the reactor to normal pressure, then evacuate and reduce the pressure to below 100 Pa, and raise the temperature to 280° C. and react for 3-5 hours. After the reaction, introduce nitrogen, cool the discharged material with cooling water, and cut into pellets;

[0032] 2) dispersing the pelletized product in acetone for 1 to 2 hours, taking it out and drying it, then placing it in a dichloromethane solution containing 3 times the mass of glycidyl methacrylate, introducing nitrogen to replace the air in the system, and then placing the mixed system in a radiation field for irradiation under a nitrogen atmosphere; after the irradiation is completed, filtering it with suction, and finally washing and drying it to obtain the modified grafted PBT;

[0033] 3) placing PEN resin and hexamethylenediamine in a mass ratio of 1:3 in a reaction kettle and heating to 200° C. for reaction for 24 hours to obtain a pretreated PEN resin;

[0034] 4) 75 parts of PET resin, 20 parts of modified grafted PBT, 4 parts of pretreated PEN resin, 0.3 parts of antioxidant 1010 and 0.7 parts of lubricant (pentaerythritol stearate) are sent into a mixing bin and mixed to form a mixture;

[0035] 5) The mixed material is fed into an extruder, and the extrusion temperature is set at 270-290° C., and the temperature of the cooling roller is set at 15° C. to extrude a cast sheet; the composite cast sheet is first longitudinally stretched 3.5 times at 90-120° C. and then cooled to 50° C., and then transversely stretched 3 times at 110-120° C., and finally pulled and rolled.

[0036] Embodiment 2:

[0037] 1) Add 100 mol of terephthalic acid, 20 mol of calcium dihydroxybenzene sulfonate, 100 mol of butanediol and 300 mg / kg of antimony trioxide as a catalyst into a reactor, control the pressure in the reactor at 0.3 MPa, raise the temperature to 230-250° C. and react for 2-3 hours; reduce the pressure in the reactor to normal pressure, then evacuate and reduce the pressure to below 100 Pa, and raise the temperature to 280° C. and react for 3-5 hours. After the reaction, introduce nitrogen, cool the discharged material with cooling water, and cut into pellets;

[0038] 2) dispersing the pelletized product in acetone for 1 to 2 hours, taking it out and drying it, then placing it in a dichloromethane solution containing 3 times the mass of glycidyl methacrylate, introducing nitrogen to replace the air in the system, and then placing the mixed system in a radiation field for irradiation under a nitrogen atmosphere; after the irradiation is completed, filtering it with suction, and finally washing and drying it to obtain the modified grafted PBT;

[0039] 3) placing PEN resin and hexamethylenediamine in a mass ratio of 1:5 in a reaction kettle and heating to 200° C. for reaction for 24 hours to obtain a pretreated PEN resin;

[0040] 4) 75 parts of PET resin, 17 parts of modified grafted PBT, 7 parts of pretreated PEN resin, 0.3 parts of antioxidant 1010 and 0.7 parts of lubricant (pentaerythritol stearate) are sent into a mixing bin and mixed to form a mixture;

[0041] 5) The mixed material is fed into an extruder, and the extrusion temperature is set at 270-290° C., and the temperature of the cooling roller is set at 15° C. to extrude a cast sheet; the composite cast sheet is first longitudinally stretched 3.5 times at 90-120° C. and then cooled to 50° C., and then transversely stretched 3 times at 110-120° C., and finally pulled and rolled.

[0042] Embodiment 3:

[0043] 1) Add 100 mol of terephthalic acid, 20 mol of calcium dihydroxybenzene sulfonate, 100 mol of butanediol and 300 mg / kg of antimony trioxide as a catalyst into a reactor, control the pressure in the reactor at 0.3 MPa, raise the temperature to 230-250° C. and react for 2-3 hours; reduce the pressure in the reactor to normal pressure, then evacuate and reduce the pressure to below 100 Pa, and raise the temperature to 280° C. and react for 3-5 hours. After the reaction, introduce nitrogen, cool the discharged material with cooling water, and cut into pellets;

[0044] 2) dispersing the pelletized product in acetone for 1 to 2 hours, taking it out and drying it, then placing it in a dichloromethane solution containing 3 times the mass of glycidyl methacrylate, introducing nitrogen to replace the air in the system, and then placing the mixed system in a radiation field for irradiation under a nitrogen atmosphere; after the irradiation is completed, filtering it with suction, and finally washing and drying it to obtain the modified grafted PBT;

[0045] 3) placing PEN resin and hexamethylenediamine in a mass ratio of 1:5 in a reaction kettle and heating to 200° C. for reaction for 24 hours to obtain a pretreated PEN resin;

[0046] 4) 75 parts of PET resin, 14 parts of modified grafted PBT, 10 parts of pretreated PEN resin, 0.3 parts of antioxidant 1010 and 0.7 parts of lubricant (pentaerythritol stearate) are sent into a mixing bin and mixed to form a mixture;

[0047] 5) The mixed material is fed into an extruder, and the extrusion temperature is set at 270-290° C., and the temperature of the cooling roller is set at 15° C. to extrude a cast sheet; the composite cast sheet is first longitudinally stretched 3.5 times at 90-120° C. and then cooled to 50° C., and then transversely stretched 3 times at 110-120° C., and finally pulled and rolled.

[0048] Embodiment 4:

[0049] 1) Add 100 mol of terephthalic acid, 30 mol of calcium dihydroxybenzene sulfonate, 100 mol of butanediol and 300 mg / kg of antimony trioxide as a catalyst into a reactor, control the pressure in the reactor at 0.3 MPa, raise the temperature to 230-250° C. and react for 2-3 hours; reduce the pressure in the reactor to normal pressure, then evacuate and reduce the pressure to below 100 Pa, and raise the temperature to 280° C. and react for 3-5 hours. After the reaction, introduce nitrogen, cool the discharged material with cooling water, and cut into pellets;

[0050] 2) dispersing the pelletized product in acetone for 1 to 2 hours, taking it out and drying it, then placing it in a dichloromethane solution containing 3 times the mass of glycidyl methacrylate, introducing nitrogen to replace the air in the system, and then placing the mixed system in a radiation field for irradiation under a nitrogen atmosphere; after the irradiation is completed, filtering it with suction, and finally washing and drying it to obtain the modified grafted PBT;

[0051] 3) placing PEN resin and hexamethylenediamine in a mass ratio of 1:5 in a reaction kettle and heating to 200° C. for reaction for 24 hours to obtain a pretreated PEN resin;

[0052] 4) 80 parts of PET resin, 14 parts of modified grafted PBT, 5 parts of pretreated PEN resin, 0.3 parts of antioxidant 1010 and 0.7 parts of lubricant (pentaerythritol stearate) are sent into a mixing bin and mixed to form a mixture;

[0053] 5) The mixed material is fed into an extruder, and the extrusion temperature is set at 270-290° C., and the temperature of the cooling roller is set at 15° C. to extrude a cast sheet; the composite cast sheet is first longitudinally stretched 3.5 times at 90-120° C. and then cooled to 50° C., and then transversely stretched 3 times at 110-120° C., and finally pulled and rolled.

[0054] Embodiment 5:

[0055] 1) Add 100 mol of terephthalic acid, 30 mol of calcium dihydroxybenzene sulfonate, 100 mol of butanediol and 300 mg / kg of antimony trioxide as a catalyst into a reactor, control the pressure in the reactor at 0.3 MPa, raise the temperature to 230-250° C. and react for 2-3 hours; reduce the pressure in the reactor to normal pressure, then evacuate and reduce the pressure to below 100 Pa, and raise the temperature to 280° C. and react for 3-5 hours. After the reaction, introduce nitrogen, cool the discharged material with cooling water, and cut into pellets;

[0056] 2) dispersing the pelletized product in acetone for 1 to 2 hours, taking it out and drying it, then placing it in a dichloromethane solution containing 3 times the mass of glycidyl methacrylate, introducing nitrogen to replace the air in the system, and then placing the mixed system in a radiation field for irradiation under a nitrogen atmosphere; after the irradiation is completed, filtering it with suction, and finally washing and drying it to obtain the modified grafted PBT;

[0057] 3) placing PEN resin and hexamethylenediamine in a mass ratio of 1:5 in a reaction kettle and heating to 200° C. for reaction for 24 hours to obtain a pretreated PEN resin;

[0058] 4) 70 parts of PET resin, 19 parts of modified grafted PBT, 10 parts of pretreated PEN resin, 0.3 parts of antioxidant 1010 and 0.7 parts of lubricant (pentaerythritol stearate) are sent into a mixing bin and mixed to form a mixture;

[0059] 5) The mixed material is fed into an extruder, and the extrusion temperature is set at 270-290° C., and the temperature of the cooling roller is set at 15° C. to extrude a cast sheet; the composite cast sheet is first longitudinally stretched 3.5 times at 90-120° C. and then cooled to 50° C., and then transversely stretched 3 times at 110-120° C., and finally pulled and rolled.

[0060] The mechanical properties of the prepared base film were tested, and the tensile strength and mechanical properties at room temperature were tested. Then, the sample was aged at 85°C and 85% humidity for 48 hours, and the tensile strength after aging was tested. The tensile strength retention after aging was calculated, and the average values ​​of the longitudinal and transverse directions were taken. The thermal shrinkage of the base film was tested at 150°C for 30 minutes and 190°C for 10 minutes, and the results are recorded in Table 1.

[0061] Table 1

[0062]

[0063]

[0064] As can be seen from Table 1, the base film prepared in this application has excellent mechanical properties at room temperature and can meet the basic requirements for preparing composite current collectors. The heat shrinkage rate can also be kept at a low level at high temperature, controlled below 1.5%, and the tensile strength retention rate after aging reaches more than 98%, indicating that the base film prepared in this application also has heat resistance and aging resistance.

[0065] Application: Preparation of composite current collector

[0066] A copper metal conductive layer is formed on the upper and lower surfaces of the PET film prepared above by vacuum evaporation to prepare a composite current collector.

[0067] When the metal layer is plated, observe whether the base film has wrinkles, deformation, and other problems, and record the defective rate in Table 2.

[0068] Table 2

[0069] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Defective rate 0.98% 0.86% 0.78% 1.01% 0.72% 5.41%

[0070] It can be seen from Table 2 that when the composite current collector is prepared using the base film of the present application, the product defect rate is greatly reduced.

[0071] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. A method for preparing a base film for a high temperature resistant and aging resistant composite current collector, It is characterized in that The steps include: 1) Add terephthalic acid, calcium dihydroxybenzene sulfonate, butanediol and a catalyst into a reactor, control the pressure in the reactor at 0.3 MPa, raise the temperature to 230-250° C. and react for 2-3 hours; reduce the pressure in the reactor to normal pressure, then evacuate and reduce the pressure to below 100 Pa, and raise the temperature to 280° C. and react for 3-5 hours. After the reaction, introduce nitrogen, cool the discharged material with cooling water, and cut into pellets; 2) dispersing the pelletized product in acetone for 1 to 2 hours, taking it out and drying it, then placing it in a dichloromethane solution containing glycidyl methacrylate, introducing nitrogen to replace the air in the system, and then placing the mixed system in a radiation field for irradiation under a nitrogen atmosphere; after the irradiation is completed, filtering it with suction, and finally washing and drying it to obtain the modified grafted PBT; 3) placing the PEN resin and hexamethylenediamine in a reaction kettle and mixing them for a certain period of time to obtain a pretreated PEN resin; 4) sending PET resin, modified grafted PBT, pretreated PEN resin, antioxidant and lubricant into a mixing bin to mix and prepare a mixture; 5) The mixed material is fed into an extruder, extruded and formed, then biaxially stretched, and finally pulled and rolled; In the step 1), the molar ratio of terephthalic acid, calcium dihydroxybenzene sulfonate and butanediol is 100:20 to 40:100; In the step 2), the mass ratio of the pelletized product to glycidyl methacrylate is 1:0.2-0.5; the irradiation source is a cobalt source, and the irradiation dose is 25 kGy.

2. The method for preparing the base film for the high temperature resistant and aging resistant composite current collector according to claim 1, It is characterized in that The catalyst is an antimony-based catalyst with a mass fraction of 200 to 300 mg / kg.

3. The method for preparing the base film for the high temperature resistant and aging resistant composite current collector according to claim 1, It is characterized in that The mass ratio of the PEN resin to hexamethylenediamine is 1:3-5; the treatment temperature is 200° C., and the treatment time is 24 hours.

4. The method for preparing the base film for the high temperature resistant and aging resistant composite current collector according to claim 1, It is characterized in that The antioxidant is antioxidant 1010 or antioxidant 168; the lubricant is pentaerythritol stearate.

5. The method for preparing the base film for the high temperature resistant and aging resistant composite current collector according to claim 1, It is characterized in that The feeding proportions of the PET resin, modified grafted PBT, pretreated PEN resin, antioxidant and lubricant are 70-80 parts, 5-20 parts, 2-10 parts, 0.3-0.5 parts and 0.5-1 parts respectively.

6. A base film for a high temperature and aging resistant composite current collector prepared by the preparation method according to any one of claims 1 to 5.

Citation Information

Cited By

  • Ageing-resistant high-flame-retardant high-adhesive-force base film for composite current collector and preparation method thereof

    CN122278158A

  • Aging-resistant high-flame-retardant high-adhesion base film for composite current collectors and a preparation method thereof